A MOFs-derived porous carbon-coated bifunctional metal nanocatalyst and its preparation method and application

Through the porous carbon-derived coated bifunctional metal nanocatalysts, the problems of non-precious metal catalysts are solved, and the activity instability and low selectivity of non-precious metal catalysts are achieved under high temperature and high pressure, and the long-term stability and high selectivity of the catalyst are achieved, reducing production costs. And it exhibits excellent catalytic properties in furfural preparation.

CN118649686BActive Publication Date: 2024-11-26GUANGDONG UNIV OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411132566.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The problems of non-precious metal catalysts' activity instability and low selectivity under long-term operation of high temperature and high pressure lead to high production costs and difficult to control product distribution.

Method used

Using porous carbon-derived bifunctional metal nanocatalysts, non-precious metal nanoparticles are prepared through hydrothermal synthesis and high-temperature pyrolysis, and the rare earth oxides are loaded on the non-precious metal surface through vacuum-assisted impregnation and calcination reduction technology to form a core shell The catalyst of structure.

Benefits of technology

The long-term stable activity and high selectivity of the catalyst are achieved, the production cost is reduced, and excellent catalytic properties are shown in the preparation of 1,5-pentanediol or tetrahydrofurfuryl alcohol.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118649686B_ABST
    Figure CN118649686B_ABST
Patent Text Reader

Abstract

The present invention discloses a MOFs-derived porous carbon-coated bifunctional metal nanocatalyst and a preparation method and application thereof, and belongs to the technical field of compound synthesis and catalyst materials. The present invention uses non-precious metals as active metals and rare earth oxides as alkaline sites. The two metals are coated with porous carbon in the form of nanoparticles to obtain a MOFs-derived porous carbon-coated bifunctional metal nanocatalyst with a core-shell structure. The obtained catalyst can maintain stable catalytic activity and high selectivity for a long time. The present invention also provides a method for preparing a MOFs-derived porous carbon-coated bifunctional metal nanocatalyst, which uses an organic ligand as a pore-forming template and is in-situ mixed with a non-precious metal, and is mixed with a rare earth oxide precursor solution after hydrothermal synthesis and high-temperature pyrolysis, and then reduced by vacuum-assisted impregnation and calcination to obtain a MOFs-derived porous carbon-coated bifunctional metal nanocatalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of compound synthesis and catalyst materials, and in particular relates to a MOFs-derived porous carbon-coated bifunctional metal nanocatalyst and a preparation method and application thereof. Background Art

[0002] The reaction of furfural to prepare 1,5-pentanediol requires the use of a catalyst, and the selection and design of the catalyst have a great influence on the reaction efficiency and product purity. At present, although precious metal catalysts such as palladium, platinum, and rhodium have shown excellent performance in many fields, their high cost has become a key factor restricting the economic efficiency of production. With the advancement of science and technology, the research and application of non-precious metal catalysts have become increasingly in-depth, providing a new way to reduce costs. However, non-precious metal catalysts also face many challenges in practical applications: they often require more stringent reaction conditions, such as high temperature and high pressure environments, which leads to the loss or sintering of the active metal components of the catalyst during long-term (more than 12 hours) continuous reactions, which in turn causes a significant decline in catalytic activity. This technical bottleneck, that is, the problem of instability of the activity of non-precious metal catalysts under long-term operation at high temperature and high pressure, is a problem that is difficult to completely avoid at present. Secondly, the low selectivity of non-precious metal catalysts is also a problem that needs to be solved urgently. Non-precious metal catalysts often find it difficult to achieve high selectivity comparable to precious metal catalysts, which makes it difficult to accurately control the distribution of products in practical applications, thereby affecting the quality and output of the products.

[0003] At present, there have been many explorations of optimization strategies for this problem. Among them, the structural optimization of the catalyst is one of the important ways, which involves strategies such as adjusting the coordination environment of the catalyst, optimizing the crystal structure, and regulating the pore size, aiming to enhance the stability and selectivity of the catalyst and delay its deactivation process. However, this method requires in-depth scientific research and design, so the implementation cost is relatively high. Another strategy is catalyst surface modification. By carefully selecting and introducing suitable functional groups on the catalyst surface, its stability and selectivity can be effectively improved, thereby slowing down the deactivation rate. However, this method also faces challenges, including the selection of functional groups and modification methods, as well as the cost considerations that come with it. In addition, the introduction of additives into the reaction system has also been proven to be an effective means of regulation, which can regulate the reaction microenvironment and help slow down the deactivation of the catalyst. However, the selection of suitable additives and their addition amounts is crucial, and it is necessary to be vigilant about the potential effects of additives on product purity and reaction efficiency. Finally, the improvement of catalyst carriers is also a key link in improving catalyst performance. By selecting and optimizing carrier materials and their preparation methods, the stability and selectivity of the catalyst can be significantly improved and the deactivation rate can be reduced. However, this process also requires sophisticated material selection and process design, which increases the implementation cost.

[0004] Therefore, there is an urgent need for a non-precious metal catalyst that is economical, efficient, and can maintain stable catalytic activity and high selectivity for a long time to solve the above problems. Summary of the invention

[0005] In order to solve the above technical problems, the present invention proposes a MOFs-derived porous carbon-coated bifunctional metal nanocatalyst and a preparation method and application thereof.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides a MOFs-derived porous carbon-coated bifunctional metal nanocatalyst, wherein the catalyst has a structure with porous carbon as a shell layer and non-precious metal and rare earth oxide as a core layer; the rare earth oxide is loaded on the surface of the non-precious metal.

[0008] Preferably, the non-precious metal includes one or more of nickel and cobalt; the loading amount of the non-precious metal is 60-80% of the total mass of the catalyst.

[0009] Preferably, the rare earth oxide includes one or more of lanthanum oxide, cerium oxide, and yttrium oxide; the loading amount of the rare earth oxide is 0.1-2% of the total mass of the catalyst.

[0010] The present invention provides a method for preparing the MOFs-derived porous carbon-coated bifunctional metal nanocatalyst described in the above technical solution, comprising the following steps:

[0011] (1) The organic ligand, non-precious metal precursor solution and polymer material are mixed, and then subjected to hydrothermal synthesis and high-temperature pyrolysis to obtain a MOFs-derived porous carbon-coated non-precious metal nanocatalyst;

[0012] (2) The MOFs-derived porous carbon-coated non-precious metal nanocatalyst obtained in step (1) is mixed with a rare earth oxide precursor solution and subjected to vacuum-assisted impregnation, followed by drying and calcination reduction to obtain the MOFs-derived porous carbon-coated bifunctional metal nanocatalyst.

[0013] Preferably, in step (1), the mass ratio of the organic ligand, the non-precious metal precursor in the non-precious metal precursor solution and the polymer material is 0.17:0.2:(0-0.1875).

[0014] Preferably, in step (1), the temperature of the hydrothermal synthesis is 100-200° C., and the time of the hydrothermal synthesis is 10-24 h.

[0015] Preferably, in step (1), the temperature of the high-temperature pyrolysis is 450-550°C, the holding time of the high-temperature pyrolysis is 2h, the rate of heating to the high-temperature pyrolysis temperature is 5°C / min, and the atmosphere of the high-temperature pyrolysis is argon.

[0016] Preferably, in step (2), the vacuum-assisted impregnation time is 30 to 120 minutes.

[0017] Preferably, in step (2), the calcination reduction temperature is 400°C, the calcination reduction holding time is 2h, the temperature is increased to the calcination reduction temperature at a rate of 5°C / min, and the calcination reduction atmosphere is a hydrogen-argon mixture.

[0018] The present invention also provides the use of the MOFs-derived porous carbon-coated bifunctional metal nanocatalyst described in the above technical solution in the preparation of 1,5-pentanediol or tetrahydrofurfuryl alcohol from furfural.

[0019] Compared with the prior art, the present invention has the following advantages and technical effects:

[0020] The present invention uses non-precious metals as active metals and rare earth oxides as alkaline sites. The two metals are coated with porous carbon in the form of nanoparticles to obtain a MOFs-derived porous carbon-coated bifunctional metal nanocatalyst with a core-shell structure. The obtained catalyst can maintain stable catalytic activity and high selectivity for a long time.

[0021] The present invention adopts an organic ligand which also serves as a pore-forming template and is mixed in situ with a non-precious metal, prepares a non-precious metal complex by hydrothermal synthesis, and then in situ pyrolyzes the non-precious metal complex by high-temperature pyrolysis to reduce it to a uniformly dispersed porous carbon-coated core-shell non-precious metal nanocatalyst, which is then mixed with a rare earth oxide precursor solution and allowed to enter the interior of the core-shell by vacuum-assisted impregnation to interact with the non-precious metal, which can effectively resist sintering and loss, and finally is calcined and reduced to obtain a MOFs-derived porous carbon-coated bifunctional metal nanocatalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0023] Figure 1 The La prepared in Example 1 x TEM image of Ni@C-PVP catalyst;

[0024] Figure 2 The La prepared in Example 1 x HRTEM image of Ni@C-PVP catalyst;

[0025] Figure 3 The La prepared in Example 1 x Mapping diagram of Ni@C-PVP catalyst;

[0026] Figure 4 The La prepared in Example 1 x BET plot of Ni@C-PVP catalyst;

[0027] Figure 5 The La prepared in Example 1 x XPS spectrum of La in Ni@C-PVP catalyst;

[0028] Figure 6 The La prepared in Example 1 x Schematic diagram of the structure of Ni@C-PVP catalyst;

[0029] Figure 7 A physical picture of the equipment used for vacuum-assisted impregnation in Examples 1-6;

[0030] Figure 8 The La prepared in Example 1 x Catalytic performance diagram of Ni@C-PVP for furfural to 1,5-pentanediol;

[0031] Fig. 9 The La prepared in Example 1 x Catalytic performance diagram of Ni@C-PVP for furfural to tetrahydrofurfuryl alcohol;

[0032] Fig.10 This is a diagram showing the catalytic performance of the catalyst prepared in Comparative Examples 1-2 for use in preparing 1,5-pentanediol from furfural. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0035] An embodiment of the present invention provides a MOFs-derived porous carbon-coated bifunctional metal nanocatalyst, wherein the catalyst has a structure with porous carbon as a shell layer and non-precious metals and rare earth oxides as a core layer; the rare earth oxides are loaded on the surface of the non-precious metal.

[0036] The present invention uses non-precious metals as active metals and rare earth oxides as alkaline sites. The two metals are coated with porous carbon in the form of nanoparticles to obtain a MOFs-derived porous carbon-coated bifunctional metal nanocatalyst with a core-shell structure. The obtained catalyst can maintain stable catalytic activity and high selectivity for a long time.

[0037] In a preferred embodiment, the non-precious metal includes one or more of nickel and cobalt, and nickel is more preferred. The present invention uses non-precious metals nickel and cobalt as active metals to replace the use of precious metals such as palladium, platinum, and rhodium, effectively reducing production costs.

[0038] In a preferred embodiment, the loading amount of the non-precious metal is 60-80% of the total mass of the catalyst. The present invention controls the loading amount of the non-precious metal within the above range, which not only ensures the catalytic activity and selectivity of the catalyst, but also avoids sintering due to excessive non-precious metal.

[0039] In a preferred embodiment, the rare earth oxide includes one or more of lanthanum oxide, cerium oxide, and yttrium oxide, and lanthanum oxide is more preferred. The present invention uses rare earth oxide as a basic site, which has the advantage of adsorbing and activating CO.

[0040] In a preferred embodiment, the loading amount of the rare earth oxide is 0.1-2% of the total mass of the catalyst. The present invention controls the loading amount of the rare earth oxide within the above range, which not only ensures the catalytic activity and selectivity of the catalyst, but also avoids the loss caused by excessive rare earth oxide.

[0041] The present invention provides a method for preparing the MOFs-derived porous carbon-coated bifunctional metal nanocatalyst described in the above technical solution, comprising the following steps:

[0042] (1) The organic ligand, non-precious metal precursor solution and polymer material are mixed, and then subjected to hydrothermal synthesis and high-temperature pyrolysis to obtain a MOFs-derived porous carbon-coated non-precious metal nanocatalyst;

[0043] (2) The MOFs-derived porous carbon-coated non-precious metal nanocatalyst obtained in step (1) is mixed with a rare earth oxide precursor solution and subjected to vacuum-assisted impregnation, followed by drying and calcination reduction to obtain the MOFs-derived porous carbon-coated bifunctional metal nanocatalyst.

[0044] The present invention adopts an organic ligand which also serves as a pore-forming template and is mixed in situ with a non-precious metal, and a uniformly dispersed porous carbon-coated core-shell type non-precious metal nanocatalyst is prepared through hydrothermal synthesis and high-temperature pyrolysis. The catalyst is then mixed with a rare earth oxide precursor solution, and vacuum-assisted impregnation is performed to enable the rare earth oxide precursor to better enter the interior of the core-shell. Finally, the MOFs-derived porous carbon-coated bifunctional metal nanocatalyst is obtained through calcination and reduction.

[0045] In a preferred embodiment, in step (1), the mass ratio of the organic ligand, the non-precious metal precursor in the non-precious metal precursor solution and the polymer material is 0.17:0.2:(0~0.1875).

[0046] In a preferred embodiment, the solvent of the non-noble metal precursor solution is deionized water.

[0047] In a preferred embodiment, the organic ligand is added in the form of an organic ligand solution; the solvent of the organic ligand solution includes N,N-dimethylformamide and ethanol.

[0048] In a preferred embodiment, in step (1), the organic ligand comprises terephthalic acid; and the polymer material comprises polyvinyl pyrrolidone. The polymer material in the present invention can improve the stability and dispersion of the catalyst.

[0049] In a preferred embodiment, in step (1), the temperature of the hydrothermal synthesis is 100-200°C, and the time of the hydrothermal synthesis is 10-24 hours. The present invention uses organic ligands, non-precious metal precursor solutions and polymer materials as raw materials, and obtains non-precious metal complexes through hydrothermal synthesis.

[0050] In a preferred embodiment, in step (1), the temperature of the high temperature pyrolysis is 450-550°C, the holding time of the high temperature pyrolysis is 2h, the rate of heating to the high temperature pyrolysis temperature is 5°C / min, and the atmosphere of the high temperature pyrolysis is argon. The present invention performs high temperature pyrolysis in an inert atmosphere to in-situ pyrolyze the non-precious metal complex and reduce it to a carbon-coated active component of zero-valent non-precious metal.

[0051] In a preferred embodiment, in step (2), the ratio of the rare earth oxide precursor solution to the non-precious metal precursor in the non-precious metal precursor solution is 10 mL:0.2 g; the concentration of the rare earth oxide precursor solution is 0.001 mol / L; and the solvent of the rare earth oxide precursor solution is ethanol.

[0052] In a preferred embodiment, in step (2), the vacuum-assisted impregnation time is 30 to 120 minutes. The present invention extracts gas from the sample hole through vacuum-assisted impregnation to form a negative pressure in the sample hole, thereby promoting the rare earth oxide precursor to better enter the porous carbon channel and interact with the non-precious metal, which can effectively resist sintering and loss.

[0053] In a preferred embodiment, in step (2), the calcination reduction temperature is 400°C, the calcination reduction holding time is 2h, the rate of heating to the calcination reduction temperature is 5°C / min, and the calcination reduction atmosphere is a hydrogen-argon mixed gas; the hydrogen volume content in the hydrogen-argon mixed gas is 5%. During the calcination reduction process, the rare earth oxide precursor will decompose to form rare earth oxides, and at the same time, the interaction between the non-precious metal and the rare earth oxide will be enhanced, and the bonding mode between the two will change from physical bonding to chemical bonding.

[0054] The present invention also provides the use of the MOFs-derived porous carbon-coated bifunctional metal nanocatalyst described in the above technical solution in the preparation of 1,5-pentanediol or tetrahydrofurfuryl alcohol from furfural.

[0055] In a preferred embodiment, when the catalyst is used to prepare 1,5-pentanediol from furfural, the reaction temperature is 60-300°C, the reaction time is 0.5-5h, and the space velocity is 500-9000h -1 , the yield of 1,5-pentanediol is ≥99%.

[0056] The room temperature in the embodiments of the present invention refers to "25±2°C".

[0057] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources.

[0058] Example 1

[0059] A method for preparing a MOFs-derived porous carbon-coated bifunctional metal nanocatalyst, the specific steps are as follows:

[0060] (1) Take 0.20g of nickel acetate tetrahydrate and dissolve it in 7mL of deionized water, stir for 10min, and obtain solution A; take 0.17g of terephthalic acid and dissolve it in 7mL of N,N-dimethylformamide and stir for 10min, then add 7mL of ethanol and stir for 10min, and obtain solution B; mix solution A and solution B and stir for 5min, slowly add 0.1875g of polyvinyl pyrrolidone (K88-96), and stir vigorously for 30min, and obtain solution C; place solution C in a hydrothermal autoclave, perform hydrothermal synthesis at 120℃ for 12h, collect light green powder, and then centrifuge and wash it with ethanol for 3 times, and then dry it at 80℃ for 12h, and then grind it to 80~200 mesh to obtain MOFs precursor;

[0061] (2) subjecting the MOFs precursor obtained in step (1) to high-temperature pyrolysis in an Ar gas flow tubular furnace, heating the temperature to 450°C at a heating rate of 5°C / min for 90 min, then keeping the temperature for 2 h, and naturally cooling to room temperature to obtain a Ni@C-PVP catalyst;

[0062] (3) The Ni@C-PVP catalyst obtained in step (2) was placed in a round-bottom flask, 10 mL of lanthanum nitrate hexahydrate ethanol solution with a concentration of 0.001 mol / L was added to the round-bottom flask, and the round-bottom flask was connected to a circulating vacuum pump for vacuum-assisted impregnation for 60 min. After the solution evaporated, it was calcined and reduced in a 5% H2 / Ar gas flow tubular furnace, and the temperature was increased to 400°C at a heating rate of 5°C / min, kept at this temperature for 2 h, and naturally cooled to obtain a LaxNi@C-PVP catalyst, in which the loading amount of lanthanum oxide in the catalyst was 1% of the total mass of the catalyst, and the loading amount of Ni was 62% of the total mass of the catalyst.

[0063] Figure 1 The La prepared in Example 1 x TEM image of Ni@C-PVP catalyst. Figure 1 It can be seen that the catalyst particles are uniformly dispersed spherical structures.

[0064] Figure 2 The La prepared in Example 1 x HRTEM image of Ni@C-PVP catalyst. Figure 2 It can be seen that the catalyst is a core-shell structure of carbon-coated Ni.

[0065] Figure 3 The La prepared in Example 1 x Mapping diagram of Ni@C-PVP catalyst. Figure 3 It can be seen that nickel and lanthanum are in La x The Ni@C-PVP catalyst is evenly distributed.

[0066] Figure 4 The La prepared in Example 1 x BET diagram of Ni@C-PVP catalyst. Figure 4 It can be seen that the La prepared in Example 1 of the present invention x The Ni@C-PVP catalyst has a porous structure.

[0067] Figure 5 The La prepared in Example 1 x XPS spectrum of La in Ni@C-PVP catalyst. Figure 5 It can be seen that lanthanum exists in the catalyst in the form of +3 valence.

[0068] Figure 6 The La prepared in Example 1 x Schematic diagram of the structure of Ni@C-PVP catalyst. Figure 6 It can be seen that La xThe Ni@C-PVP catalyst has a core-shell structure, in which porous carbon acts as a shell layer to wrap non-precious metal nickel and rare earth oxide lanthanum oxide, and the rare earth oxide lanthanum oxide is loaded on the surface of the non-precious metal nickel.

[0069] Example 2

[0070] The difference from Example 1 is that the lanthanum nitrate hexahydrate ethanol solution in step (3) is replaced with an yttrium nitrate hexahydrate ethanol solution of the same volume and concentration to obtain a Y x Ni@C-PVP catalyst.

[0071] Example 3

[0072] The difference from Example 1 is that the lanthanum nitrate hexahydrate ethanol solution in step (3) is replaced with an cerium nitrate hexahydrate ethanol solution of the same volume and concentration to obtain Ce with the same loading amount. x Ni@C-PVP catalyst.

[0073] Example 4

[0074] A method for preparing a MOFs-derived porous carbon-coated bifunctional metal nanocatalyst, the specific steps are as follows:

[0075] (1) Take 0.20g of cobalt acetate tetrahydrate and dissolve it in 7mL of deionized water, stir for 10min, and obtain solution A; take 0.17g of terephthalic acid and dissolve it in 7mL of N,N-dimethylformamide and stir for 10min, then add 7mL of ethanol and stir for 10min, and obtain solution B; mix solution A and solution B and stir slowly for 10min, and obtain solution C; place solution C in a hydrothermal reactor, perform hydrothermal synthesis at 120℃ for 12h, collect light green powder, and then wash it with ethanol by centrifugation for 3 times, and then dry it at 80℃ for 12h, and then grind it to 80~200 mesh to obtain MOFs precursor;

[0076] (2) subjecting the MOFs precursor obtained in step (1) to high-temperature pyrolysis in an Ar gas flow tubular furnace, heating the temperature to 550°C at a heating rate of 5°C / min for 110 min, then keeping the temperature for 2 h, and naturally cooling to room temperature to obtain a Co@C catalyst;

[0077] (3) The Co@C catalyst obtained in step (2) was placed in a round-bottom flask, 10 mL of lanthanum nitrate hexahydrate ethanol solution with a concentration of 0.001 mol / L was added to the round-bottom flask, and the round-bottom flask was connected to a circulating vacuum pump for vacuum-assisted impregnation for 60 min. After the solution evaporated, it was calcined and reduced in a 5% H2 / Ar gas flow tubular furnace, and the temperature was increased to 400°C at a heating rate of 5°C / min, kept at this temperature for 2 h, and cooled naturally to obtain La xCo@C catalyst, the loading amount of lanthanum oxide in the catalyst is 1% of the total mass of the catalyst, and the loading amount of Co is 80% of the total mass of the catalyst.

[0078] Example 5

[0079] The difference from Example 4 is that the lanthanum nitrate hexahydrate ethanol solution in step (3) is replaced with an yttrium nitrate hexahydrate ethanol solution of the same volume and concentration to obtain a Y x Co@C catalyst.

[0080] Example 6

[0081] The difference from Example 4 is that the lanthanum nitrate hexahydrate ethanol solution in step (3) is replaced with an cerium nitrate hexahydrate ethanol solution of the same volume and concentration to obtain Ce with the same loading amount. x Co@C catalyst.

[0082] Comparative Example 1

[0083] The difference from Example 1 is that the vacuum-assisted impregnation in step (3) is omitted to obtain La x Ni@C-PVP catalyst.

[0084] Comparative Example 2

[0085] The difference from Example 1 is that in step (3), calcination is carried out in an Ar gas flow tubular furnace to obtain the La-Ni@C-PVP catalyst.

[0086] Figure 7 This is a physical picture of the equipment used for vacuum assisted impregnation in Examples 1-6. Figure 7 It can be seen that the present invention extracts gas from the sample hole through vacuum-assisted impregnation, so that negative pressure is formed in the sample hole, thereby promoting the rare earth oxide precursor to better enter the porous carbon channel.

[0087] Application Example 1

[0088] The La prepared in Example 1 x Ni@C-PVP is used in the preparation of 1,5-pentanediol from furfural. The specific process is as follows:

[0089] 50 mg of catalyst LaxNi@C-PVP and 0.204 g of furfural were placed in a reactor, and then 10 mL of isopropanol was added as a solvent, and 0.1 g of dodecane was added as an internal standard. 3 MPa of hydrogen was filled into the reactor to replace the residual air in the reactor, and repeated 5 times, and then 3 MPa of hydrogen was filled. Then the reactor was heated to 180 ° C using a heating jacket, and stirred at 800 rpm for 0.5 to 5 hours. After the reaction was completed, the reactor was taken out of the heating jacket, and the pressure was vented after it was cooled to room temperature. The liquid in the reactor was separated into solid and liquid using a filter membrane to obtain liquid 1,5-pentanediol.

[0090] The liquid 1,5-pentanediol obtained in Application Example 1 was analyzed by gas chromatography to calculate the conversion rate and selectivity. The results are shown in Figure 8 .

[0091] Figure 8 The La prepared in Example 1 x Catalytic performance diagram of Ni@C-PVP for furfural to 1,5-pentanediol. Figure 8 It can be seen that when the reaction condition is 180°C, during the 5 cycles of the catalyst, the reaction activity is maintained at about 80% (bar graph), and the selectivity of 1,5-pentanediol is always maintained above 95% (line graph), indicating that the catalyst prepared in Example 1 has excellent catalytic hydrogenolysis activity, excellent selectivity and stability under relatively mild conditions.

[0092] Application Example 2

[0093] The La prepared in Example 1 x Ni@C-PVP is used in the hydrogenation of furfural to prepare tetrahydrofurfuryl alcohol. The specific process is as follows:

[0094] 30 mg of catalyst LaxNi@C-PVP and 0.192 g of furfural were placed in a reactor, and 0.1 g of dodecane was added as an internal standard. Then 10 mL of isopropanol was added as a solvent. 3 MPa of hydrogen was filled into the reactor to replace the residual air in the reactor. This was repeated 5 times. 3 MPa of hydrogen was then filled into the reactor. The reactor was heated to 110 ° C using a heating jacket and stirred at 800 rpm for 2 hours. After the reaction was completed, the reactor was removed from the heating jacket, the pressure was vented after cooling to room temperature, and the liquid in the reactor was separated into solid and liquid using a filter membrane to obtain liquid tetrahydrofurfuryl alcohol.

[0095] The liquid tetrahydrofurfuryl alcohol obtained in Application Example 2 was analyzed by gas chromatography to calculate the conversion rate and selectivity. The results are shown in Fig. 9 .

[0096] Fig. 9 The La prepared in Example 1 x Catalytic performance diagram of Ni@C-PVP for furfural to tetrahydrofurfuryl alcohol. Fig. 9 It can be seen that under the reaction conditions of 110°C and the reaction time of 2h, the conversion rate of furfural is 100%, and the selectivity is also greater than 99%, which remains stable, indicating that the catalyst prepared in Example 1 has excellent catalytic activity under mild conditions. The reaction mechanism of furfural hydrogenation to tetrahydrofurfuryl alcohol is: furfural is first dissolved in a solvent with hydrogen, and then dissociated to obtain tetrahydrofurfuryl alcohol after a catalyst adsorption reaction.

[0097] Comparative Application Examples 1~2

[0098] The catalyst prepared in Comparative Examples 1-2 was used to prepare 1,5-pentanediol from furfural, and the specific process was as follows:

[0099] 50 mg of catalyst and 0.204 g of furfural were placed in a reactor, and then 10 mL of isopropanol was added as a solvent, and 0.1 g of dodecane was added as an internal standard. 3 MPa of hydrogen was filled into the reactor to replace the residual air in the reactor, and repeated 5 times, and then 3 MPa of hydrogen was filled. Then the reactor was heated to 180 ° C using a heating jacket, and stirred at 800 rpm for 0.5 to 2 hours. After the reaction was completed, the reactor was taken out of the heating jacket, and the pressure was vented after it was cooled to room temperature. The liquid in the reactor was then separated into solid and liquid using a filter membrane to obtain liquid 1,5-pentanediol.

[0100] The liquid 1,5-pentanediol obtained in Comparative Application Examples 1 and 2 was analyzed by gas chromatography and the yield was calculated. The results are shown in Fig.10 .

[0101] Fig.10 The catalytic performance diagram of the catalyst prepared in Comparative Examples 1 and 2 for furfural to 1,5-pentanediol. Fig.10 It can be seen that when the catalyst prepared in Comparative Example 1 is used to prepare 1,5-pentanediol from furfural, the yield of 1,5-pentanediol is only 10% after 1 hour of reaction, and the product contains a large amount of intermediate products furfuryl alcohol and tetrahydrofurfuryl alcohol. After 2 hours of reaction, the yield of 1,5-pentanediol rises to 30%, while the yield of intermediate tetrahydrofurfuryl alcohol is as high as 70%, indicating that the selectivity of the catalyst prepared in Comparative Example 1 is poor. When the catalyst prepared in Comparative Example 2 is used to prepare 1,5-pentanediol from furfural, the yield of 1,5-pentanediol is only 28% after 1 hour of reaction, and the product contains a large amount of intermediate products furfuryl alcohol and tetrahydrofurfuryl alcohol. After 2 hours of reaction, the yield of 1,5-pentanediol rises to 45%, while the yield of intermediate tetrahydrofurfuryl alcohol is as high as 55%, indicating that the selectivity of the catalyst prepared in Comparative Example 2 is poor.

[0102] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. Application of a MOFs-derived porous carbon-coated bifunctional metal nanocatalyst in the preparation of 1,5-pentanediol from furfural, characterized in that: The MOFs-derived porous carbon-coated bifunctional metal nanocatalyst has a structure with porous carbon as a shell layer and non-precious metal and rare earth oxide as a core layer; the rare earth oxide is loaded on the surface of the non-precious metal; the non-precious metal includes one or more of nickel and cobalt, and the rare earth oxide includes one or more of lanthanum oxide, cerium oxide, and yttrium oxide; The method for preparing the MOFs-derived porous carbon-coated bifunctional metal nanocatalyst comprises the following steps: (1) An organic ligand, a non-precious metal precursor solution and a polymer material are mixed, and subjected to hydrothermal synthesis and high-temperature pyrolysis to obtain a MOFs-derived porous carbon-coated non-precious metal nanocatalyst; the polymer material comprises polyvinyl pyrrolidone; and the high-temperature pyrolysis temperature is 450-550°C; (2) The MOFs-derived porous carbon-coated non-precious metal nanocatalyst obtained in step (1) is mixed with a rare earth oxide precursor solution and subjected to vacuum-assisted impregnation. After drying and calcination reduction, the MOFs-derived porous carbon-coated bifunctional metal nanocatalyst is obtained; the calcination reduction temperature is 400°C, the calcination reduction holding time is 2h, the heating rate to the calcination reduction temperature is 5°C / min, and the calcination reduction atmosphere is a hydrogen-argon mixed gas.

2. The use of the MOFs-derived porous carbon-coated bifunctional metal nanocatalyst in the preparation of 1,5-pentanediol from furfural according to claim 1, characterized in that: In step (1), the mass ratio of the organic ligand, the non-precious metal precursor and the polymer material in the non-precious metal precursor solution is 0.17:0.2:(0-0.1875), and the mass of the polymer material is not 0.

3. The use of the MOFs-derived porous carbon-coated bifunctional metal nanocatalyst in the preparation of 1,5-pentanediol from furfural according to claim 1, characterized in that: In step (1), the temperature of the hydrothermal synthesis is 100-200° C., and the time of the hydrothermal synthesis is 10-24 hours.

4. The use of the MOFs-derived porous carbon-coated bifunctional metal nanocatalyst in the preparation of 1,5-pentanediol from furfural according to claim 1, characterized in that: In step (1), the holding time of the high-temperature pyrolysis is 2 hours, the rate of heating to the high-temperature pyrolysis temperature is 5°C / min, and the atmosphere of the high-temperature pyrolysis is argon.

5. The use of the MOFs-derived porous carbon-coated bifunctional metal nanocatalyst in the preparation of 1,5-pentanediol from furfural according to claim 1, characterized in that: In step (2), the vacuum-assisted impregnation time is 30 to 120 minutes.

6. Use of the MOFs-derived porous carbon-coated bifunctional metal nanocatalyst in the preparation of 1,5-pentanediol from furfural according to claim 1, characterized in that: The loading amount of the non-precious metal is 60-80% of the total mass of the catalyst.

7. Use of the MOFs-derived porous carbon-coated bifunctional metal nanocatalyst in the preparation of 1,5-pentanediol from furfural according to claim 1, characterized in that: The loading amount of the rare earth oxide is 0.1-2% of the total mass of the catalyst.

Citation Information

Cited By

  • Preparation of phenolic resin-based porous carbon and application of phenolic resin-based porous carbon in field of gas separation

    CN122276708A