Ether synthesis catalyst and its preparation method and application

By loading phosphotungstic acid on the modified fiber support to build a porous structure, the existing catalysts are solved, and the high-priced, toxic, unstable and difficult to recover are achieved, and the efficient catalysis of ethylene glycol dimethyl ether and the recyclability of catalysts are achieved. It is suitable for industrial applications.

CN118649694BActive Publication Date: 2024-11-08SHANDONG DONGYUE FLUO SILICON MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411106219.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-08
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The existing catalysts of ethylene glycol dimethyl ether have high prices, toxicity, unstable and difficult to recover, which limits their industrial application. Moreover, the operation of traditional phase transfer catalysts is complicated and difficult to achieve separation and recycling.

Method used

Phosphuttungstic acid is used as a catalyst and supported on a modified fiber support. By building a porous structure, catalytic activity and stability are improved, and the catalyst is efficiently recovered and used repeatedly.

Benefits of technology

It realizes efficient catalysis of ethylene glycol dimethyl ether, has mild reaction conditions, simple synthesis steps, easy catalyst separation and recycling, has excellent recycling performance, reduces production costs, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118649694B_ABST
    Figure CN118649694B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of organic compound synthesis, in particular to an ether synthesis catalyst and a preparation method and application thereof. The catalyst comprises a modified fiber carrier and phosphotungstic acid loaded on the modified fiber carrier, the mass ratio of the phosphotungstic acid to the modified fiber carrier is (1-3):1, and the modified fiber carrier is selected from one of modified cotton fiber, modified polyester fiber or modified polyacrylonitrile fiber. The ether synthesis catalyst provided by the invention uses phosphotungstic acid as a catalyst active component and modified porous fiber as a carrier, and realizes the construction of a fiber surface microenvironment through fiber modification, and the good loading of the phosphotungstic acid effectively regulates the catalytic activity and catalytic stability, thereby realizing efficient catalysis in the synthesis process of ethylene glycol dimethyl ether.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of organic compound synthesis, in particular to an ether synthesis catalyst and a preparation method and application thereof. Background Art

[0002] Ethylene glycol dimethyl ether (also known as butoxyethyl ether) is a commonly used solvent and chemical intermediate. It has good solubility and can dissolve many organic and inorganic substances, so it is widely concerned in the fields of synthesis, extraction, electrolyte solvent and catalytic reaction. In addition, it is a good surface coating solvent and antifreeze additive for military jet fuel. It can also be used as a cleaning agent for metals and glass. It can also be used in the cosmetics industry, fragrance industry, pharmaceutical industry, oil field industry and many other fields.

[0003] At present, the Williamson synthesis method is used for industrial-scale production of ethylene glycol dimethyl ether. Under the condition of phase transfer catalyst, halogenated hydrocarbons react with sodium alcohol or sodium phenol to obtain it. As introduced in the master's thesis "Preparation of Organic Catalytic Fibers and Their Application in Phase Transfer Catalytic Nucleophilic Substitution Reactions" (Peng Hui, Zhejiang University of Technology, 2020), the commonly used phase transfer catalysts include the following three categories: onium salts, such as tetrabutylammonium bromide, trioctylmethylammonium chloride, etc.; inclusion complexes, formed by the reaction of cations with negatively charged oxygen atoms on the crown ether ring; open-chain polyethers, such as polyethylene glycol, etc. Japanese Patent Tokkai 55-104221 reported that the yield of ethylene glycol dimethyl ether obtained by reacting sodium alcohol with methyl chloride in the presence of phase transfer catalysts such as crown ethers and quaternary ammonium salts was 90%. Zhu Xinbao used homemade polyethylene glycol ether as a catalyst, and used ethylene glycol or ethylene glycol monomethyl ether as a raw material to react with chloromethane. The yield of ethylene glycol dimethyl ether prepared under mild reaction conditions reached 90%, and the product purity was high, but there was still a great loss in the recovery of the catalyst. Using the same method, Chinese patent document CN 112246279 A (application number 202010659801.4) used polyethylene oxide-polypropylene oxide-polyethylene oxide triblock polymer as a catalyst to prepare ethylene glycol dimethyl ether. The catalyst can only be separated by extraction with an organic solvent, which is complicated to operate and not convenient for widespread industrial application.

[0004] Traditional phase transfer catalysts generally have disadvantages such as high price, toxicity, instability, and difficulty in recycling. With people's increasing concern about the environment and health, according to the principles of "green chemistry", it is urgent to develop new phase transfer catalysts to replace traditional catalysts. Supported phase transfer catalysts provide a practical solution for separation, recovery and recycling. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies of the above-mentioned prior art and provide an ether synthesis catalyst and its preparation method and application. The present invention innovatively uses phosphotungstic acid as a catalyst for the reaction of ethylene glycol dimethyl ether, and uses modified fiber as a carrier. By constructing a porous structure in the fiber, the fiber surface groups are more easily modified and are conducive to subsequent adsorption, so that the catalyst can be highly efficient in catalysis and can also be easily recovered and reused multiple times.

[0006] In order to achieve the above technical effects, the present invention adopts the following technical solutions:

[0007] An ether synthesis catalyst comprises a modified fiber carrier and phosphotungstic acid supported on the modified fiber carrier, wherein the mass ratio of the phosphotungstic acid to the modified fiber carrier is (1-3):1;

[0008] The preparation method of the modified fiber carrier comprises the following steps:

[0009] a. After drying the fiber, place it in a reaction container, add polyvinyl pyrrolidone (PVP), diethylenetriamine (DETA) and water, stir thoroughly for 4 hours, take out the fiber, soak the fiber in water for 24 hours to remove PVP, rinse it with deionized water several times, and dry it in a vacuum drying oven for 12 hours to obtain aminated porous fiber;

[0010] b. The aminated porous fiber was stirred under reflux with ethyl bromide and ethanol for 5 hours, the fiber was taken out and washed, and dried in a vacuum drying oven at 60°C for 12 hours to obtain a modified fiber carrier;

[0011] In step a, the fiber is selected from one of cotton fiber, polyester fiber or polyacrylonitrile fiber.

[0012] Preferably, in the method for preparing the modified fiber carrier, in step a, the fiber is polyacrylonitrile fiber. The modified fiber should be cheap, easily available and corrosion-resistant.

[0013] Preferably, in the preparation method of the modified fiber carrier, in step a, the ratio of fiber, PVP, DETA and water is 1g:1g:(20-100)mL:(20-100)mL; further preferably, the ratio of fiber, PVP, EDTA and water is 1g:1g:(20-50)mL:(20-50)mL; more preferably, the ratio of fiber, PVP, EDTA and water is 1g:1g:35mL:35mL.

[0014] Preferably, in the preparation method of the modified fiber carrier, in step b, the ratio of the aminated porous fiber, ethyl bromide and ethanol is 1g:(1-5)g:(10-50)mL; further preferably, the ratio of the aminated porous fiber, ethyl bromide and ethanol is 1g:(1-3)g:(30-50)mL; more preferably, the ratio of the aminated porous fiber, ethyl bromide and ethanol is 1g:1.3g:40mL.

[0015] The present invention also provides a method for preparing the ether synthesis catalyst. The modified fiber carrier and phosphotungstic acid are ultrasonically mixed in deionized water, stirred at room temperature, and then vacuum freeze-dried to obtain the ether synthesis catalyst.

[0016] Preferably, in the preparation method, the feed ratio of the modified fiber carrier, phosphotungstic acid and deionized water is 1g:(1-3)g:(10-50)mL; further preferably, the feed ratio of the modified fiber carrier, phosphotungstic acid and deionized water is 1g:(1-1.5)g:(30-50)mL; more preferably, the feed ratio of the modified fiber carrier, phosphotungstic acid and deionized water is 1g:1.5g:30mL.

[0017] Preferably, the stirring time at room temperature is 6 h to 24 h; more preferably, the stirring time at room temperature is 12 h.

[0018] Preferably, the vacuum freeze drying time is 5h-15h, the vacuum pressure is 300Pa, and the temperature is -30°C; further preferably, the vacuum freeze drying is performed at -30°C for 3h.

[0019] The present invention also provides the use of the ether synthesis catalyst or the ether synthesis catalyst prepared by the preparation method in catalytic synthesis of ethylene glycol dimethyl ether.

[0020] Preferably, the specific application method is as follows:

[0021] 1wt%-10wt% of the total amount of raw materials of the ether synthesis catalyst are added to ethylene glycol monomethyl ether, sodium hydroxide is added in batches, after the sodium hydroxide is completely dissolved, the reaction is carried out under the condition of passing chloromethane, the ether synthesis catalyst is taken out, and the product is filtered and distilled to obtain ethylene glycol dimethyl ether; the molar ratio of sodium hydroxide to ethylene glycol monomethyl ether is (0.1-0.7):1.

[0022] Further preferably, the temperature is maintained at 30°C-40°C when adding sodium hydroxide; the amount added each time is 1 / 4 of the total amount of sodium hydroxide; the reaction pressure is below 0.2MPa, the reaction temperature is 60°C-70°C, and the reaction time is 1h.

[0023] More preferably, the ether synthesis catalyst taken out after the reaction can be used again in the catalytic synthesis process of ethylene glycol dimethyl ether after being washed and dried.

[0024] Polyacrylonitrile fiber (PANF) is considered to be a good raw material for supported catalysts due to its excellent flexibility and good application performance. The PANF chain structure has a large number of cyano groups. The fiber is modified through covalent bond interactions to make the catalytic sites on the fiber more stable to improve reusability. The construction of a porous structure in the fiber exposes more accessible groups (cyano groups) for functional group grafting. These pores also reduce mass transfer resistance and accelerate adsorption kinetics. The increase in specific surface area is conducive to the exposure of active sites and improves the loading and utilization of the catalyst. Phosphotungstic acid is a multifunctional new catalyst with high catalytic activity and good stability. It can be used for homogeneous and heterogeneous reactions and can even be used as a phase transfer catalyst. It is environmentally friendly and is a green catalyst.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. The ether synthesis catalyst provided by the present invention uses phosphotungstic acid as the catalyst active component and modified porous fibers as carriers. By modifying the fibers, the construction of the fiber surface microenvironment is achieved, and the good loading of phosphotungstic acid effectively regulates the catalytic activity and catalytic stability.

[0027] 2. When the ether synthesis catalyst provided by the present invention is used to catalyze the synthesis of ethylene glycol dimethyl ether, the reaction conditions are mild, the synthesis steps are simple, and while efficient catalysis is achieved, the separation and recovery of the catalyst is relatively convenient, and the catalyst has excellent recyclability. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the verification spectrum of ethylene glycol dimethyl ether synthesized by the ether synthesis catalyst provided in Example 1 in Experimental Example 1. DETAILED DESCRIPTION

[0029] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.

[0030] The raw materials used in each embodiment and comparative example are all commonly used commercially available raw materials in the art. The specific sources are not described here in detail, and those skilled in the art can select them according to implementation requirements.

[0031] Example 1

[0032] An ether synthesis catalyst comprises a modified fiber carrier and phosphotungstic acid loaded on the modified fiber carrier, wherein the mass ratio of the phosphotungstic acid to the modified fiber carrier is 1:1. In this embodiment, the modified fiber carrier is modified cotton fiber. The preparation method of the modified cotton fiber is as follows:

[0033] a. 1g of cotton fiber was dried and placed in a three-necked flask, and 1g of polyvinyl pyrrolidone (PVP), 20mL of diethylenetriamine (DETA) and 20mL of water were added. After fully stirring for 4 hours, the fiber was taken out and soaked in water for 24 hours to remove PVP. After rinsing with deionized water for 3 times, it was placed in a vacuum drying oven and dried for 12 hours to obtain aminated porous fiber;

[0034] b. 1 g of aminated porous fiber was stirred with 1 g of ethyl bromide and 10 mL of ethanol under reflux for 5 hours, the fiber was taken out and washed, and dried in a vacuum drying oven at 60°C for 12 hours to obtain quaternary ammonium salt functionalized porous fiber, i.e. modified cotton fiber.

[0035] The preparation method of the ether synthesis catalyst is as follows: take 1g of the modified fiber carrier and 1g of phosphotungstic acid and mix them evenly with ultrasonic in 10mL of deionized water, stir at room temperature for 6h, pre-freeze at -30°C for 3h, and then vacuum freeze-dry at a vacuum pressure of 300Pa and a temperature of -30°C for 5h to obtain the ether synthesis catalyst.

[0036] Example 2

[0037] An ether synthesis catalyst includes a modified fiber carrier and phosphotungstic acid loaded on the modified fiber carrier, wherein the mass ratio of phosphotungstic acid to the modified fiber carrier is 3:1. In this embodiment, the modified fiber carrier is modified polyester fiber. The preparation method of the modified polyester fiber is as follows:

[0038] a. 1g of polyester fiber was dried and placed in a three-necked flask, and 1g of polyvinyl pyrrolidone (PVP), 100mL of diethylenetriamine (DETA) and 100mL of water were added. After fully stirring for 4 hours, the fiber was taken out and soaked in water for 24 hours to remove PVP. After rinsing with deionized water for 3 times, it was placed in a vacuum drying oven and dried for 12 hours to obtain aminated porous fiber;

[0039] b. 1 g of aminated porous fiber was stirred with 5 g of ethyl bromide and 50 mL of ethanol under reflux for 5 hours, the fiber was taken out and washed, and dried in a vacuum drying oven at 60°C for 12 hours to obtain quaternary ammonium salt functionalized porous fiber, i.e., modified polyester fiber.

[0040] The preparation method of the ether synthesis catalyst is as follows: take 1g of the modified fiber carrier and 3g of phosphotungstic acid and mix them evenly with ultrasonic in 50mL of deionized water, stir at room temperature for 6h, pre-freeze at -30℃ for 3h, and then vacuum freeze-dry at a vacuum pressure of 300Pa and a temperature of -30℃ for 5h to obtain the ether synthesis catalyst.

[0041] Example 3

[0042] An ether synthesis catalyst includes a modified fiber carrier and phosphotungstic acid supported on the modified fiber carrier, wherein the mass ratio of phosphotungstic acid to the modified fiber carrier is 1.5:1. In this embodiment, the modified fiber carrier is modified polypropylene fiber. The preparation method of the modified polypropylene fiber is as follows:

[0043] a. 1g of polypropylene fiber was dried and placed in a three-necked flask, and 1g of polyvinyl pyrrolidone (PVP), 35mL of diethylenetriamine (DETA) and 35mL of water were added. After fully stirring for 4 hours, the fiber was taken out and soaked in water for 24 hours to remove PVP. After rinsing with deionized water for 3 times, it was placed in a vacuum drying oven and dried for 12 hours to obtain aminated porous fiber;

[0044] b. 1 g of aminated porous fiber was stirred with 1.3 g of ethyl bromide and 40 mL of ethanol under reflux for 5 hours, the fiber was taken out and washed, and dried in a vacuum drying oven at 60°C for 12 hours to obtain quaternary ammonium salt functionalized porous fiber, i.e. modified polypropylene fiber.

[0045] The preparation method of the ether synthesis catalyst is as follows: take 1g of the modified fiber carrier and 1.5g of phosphotungstic acid and mix them evenly with ultrasonic in 30mL of deionized water, stir at room temperature for 6h, pre-freeze at -30℃ for 3h, and then vacuum freeze-dry at a vacuum pressure of 300Pa and a temperature of -30℃ for 5h to obtain the ether synthesis catalyst.

[0046] Comparative Example 1

[0047] The catalyst provided in this comparative example is the catalyst P4 provided in the specific embodiment of Chinese patent document CN 112246279 A.

[0048] Comparative Example 2

[0049] An ether synthesis catalyst, which is different from Example 3 in that the mass ratio of phosphotungstic acid to the modified fiber carrier is 4:1. Other process parameters and preparation methods are the same as those of Example 3.

[0050] Comparative Example 3

[0051] An ether synthesis catalyst is different from Example 3 in that in the preparation method of the modified fiber carrier, in step a, the fiber feed mass is adjusted to 2 g, and other process parameters and preparation methods are the same as those in Example 3.

[0052] Comparative Example 4

[0053] An ether synthesis catalyst is different from Example 3 in that, in the preparation method of the modified fiber carrier, in step a, the PVP feed mass is adjusted to 2 g, and other process parameters and preparation methods are the same as those in Example 3.

[0054] Experimental Example 1

[0055] The use of the catalysts provided in Examples 1-3 and Comparative Examples 1-4 in the catalytic synthesis of ethylene glycol diethyl ether is specifically described as follows:

[0056] Add 3 mol of ethylene glycol monomethyl ether to the reactor, keep the temperature in the reactor at 30-40℃, add the catalyst, slowly add 1.5 mol of sodium hydroxide in batches while stirring, and the amount added in each batch is 1 / 4 of the total amount of sodium hydroxide. Stir until the added sodium hydroxide is completely dissolved, evacuate the reaction system, pass methyl chloride into the reactor, keep the pressure at 0.15MPa and the temperature at 65℃, and continue to react for 1 hour after the pressure stabilizes. Filter out the catalyst, wash it with water 3 times, take it out after drying and set it aside, filter and distill the product, collect the fraction with a boiling point below 90℃, obtain the product ethylene glycol dimethyl ether and the by-product sodium chloride, and determine the conversion rate and yield of ethylene glycol diethyl ether. The dried catalyst is reacted under the same conditions, and the conversion rate and yield of ethylene glycol diethyl ether are determined again after being reused 6 times. At the same time, a blank group without adding catalyst is set up.

[0057] The statistics are shown in the table below.

[0058] Table 1 Measured data

[0059]

[0060] like Figure 1 As shown, it is the verification spectrum of ethylene glycol diethyl ether obtained in the first reaction of Group 1. It can be seen from the retention time of the peak position that the product obtained by Group 1 using the catalyst provided in Example 1 is ethylene glycol dimethyl ether.

[0061] Combining the data measured in each embodiment and comparative example, a horizontal comparison between Group 1 to Group 3 shows that when the catalyst feed accounts for 5wt% of the total raw material, the catalyst provided in Example 3 has the best catalytic effect, which indicates that the amount of solvent and the loading amount have a significant effect on the catalytic effect of the catalyst.

[0062] From the horizontal comparison of Group 3-Group 5, it can be seen that when the catalysts are all the catalysts of Example 3, the catalytic effect is best when the catalyst accounts for 5wt% of the total amount of raw materials. This is because when the amount of catalyst is too small, there are fewer active centers. Although the catalytic activity can be effectively improved, the effect is not significant. The catalytic effect reaches the highest value when the total amount of catalyst accounts for 5%. As the total amount of catalyst continues to increase to 10%, the catalyst is prone to aggregation, the effective contact area is reduced, and the catalytic effect is affected. Therefore, 5% is preferred as the best catalytic effect.

[0063] It can be seen from the comparison of group 3 and group 6-9 that although the catalyst provided by comparative example 1 can also achieve a certain catalytic effect, the catalyst synthesis step prepared by this scheme is simple, and the catalyst separation and recovery is more convenient, which is convenient for industrialization and wide application; the catalyst of comparative example 2 may cause the internal structure of the fiber to be destroyed when the phosphotungstic acid load is too much, and the activity and stability are all reduced, and the effect is not good; in comparative example 3, when the fiber dosage increases, the fiber surface does not obtain the construction of a good surface ion microenvironment, resulting in a reduction in the quaternary ammonium salt functional group, thereby affecting the subsequent catalyst loading and reducing the catalytic effect; in comparative example 4, the excessive addition of pore-forming agent increases the internal pore structure of the fiber, although it has no obvious effect on the catalytic activity, the increase in the pore structure reduces the mechanical strength of the modified fiber, and the catalyst stability is sharply reduced. For the blank control without adding a catalyst, embodiment 3 effectively shortens the reaction time, from 16h to 6h, reduces the production cost, has certain economic benefits, and is conducive to subsequent industrial applications.

Claims

1. An application of an ether synthesis catalyst in catalytic synthesis of ethylene glycol dimethyl ether, characterized in that: The ether synthesis catalyst comprises a modified fiber support and phosphotungstic acid supported on the modified fiber support, wherein the mass ratio of the phosphotungstic acid to the modified fiber support is (1-3):1; The preparation method of the modified fiber carrier comprises the following steps: a. After the fiber is dried, it is placed in a reaction vessel, PVP, DETA and water are added, and the fiber is taken out after being fully stirred for 4 hours, and the fiber is soaked in water for 24 hours to remove PVP, rinsed with deionized water, and placed in a vacuum drying oven to dry for 12 hours to obtain an aminated porous fiber; b. The aminated porous fiber was refluxed with ethyl bromide and ethanol for 5 hours, the fiber was taken out and washed, and dried in a vacuum drying oven at 60°C for 12 hours to obtain a quaternary ammonium salt functionalized porous fiber, which is a modified fiber carrier; In step a, the fiber is selected from one of cotton fiber, polyester fiber or polyacrylonitrile fiber; In step a, the ratio of fiber, PVP, DETA and water is 1 g: 1 g: (20-100) mL: (20-100) mL; The preparation method of the ether synthesis catalyst is as follows: taking the modified fiber carrier and phosphotungstic acid and mixing them uniformly in deionized water by ultrasonication, stirring the loaded material at room temperature and then performing vacuum freeze drying to obtain the ether synthesis catalyst.

2. The use according to claim 1, characterized in that In the preparation method of the modified fiber carrier, in step a, the fiber is polyacrylonitrile fiber.

3. The use according to claim 1, characterized in that In the preparation method of the modified fiber carrier, in step b, the ratio of the aminated porous fiber, ethyl bromide and ethanol is 1 g:(1-5) g:(10-50) mL.

4. The use according to claim 1, characterized in that In the preparation method of the ether synthesis catalyst, the feed ratio of the modified fiber carrier, phosphotungstic acid and deionized water is 1g:(1-3)g:(10-50)mL.

5. The use according to claim 1, characterized in that In the preparation method of the ether synthesis catalyst, the stirring time at room temperature is 6h-24h.

6. The use according to claim 1, characterized in that In the preparation method of the ether synthesis catalyst, the vacuum freeze drying time is 5h-15h, the vacuum pressure is 300Pa, and the temperature is -30°C.

7. The use according to claim 1, characterized in that The specific method of catalytic synthesis is as follows: 1wt%-10wt% of the total amount of raw materials of the ether synthesis catalyst is added to ethylene glycol monomethyl ether, sodium hydroxide is added in batches, after the sodium hydroxide is completely dissolved, reacted under the condition of passing chloromethane, the ether synthesis catalyst is taken out, and the product is filtered and distilled to obtain ethylene glycol dimethyl ether; the molar ratio of sodium hydroxide to ethylene glycol monomethyl ether is (0.1-0.7):1; When adding sodium hydroxide, the temperature is maintained at 30°C-40°C; the amount added each time is 1 / 4 of the total amount of sodium hydroxide; the reaction pressure is below 0.2MPa, the reaction temperature is 60°C-70°C, and the reaction time is 1h.

Citation Information

Patent Citations

  • Catalyst and preparation method of ethylene glycol dimethyl ether

    CN112246279A

  • Method for preparing diethylene glycol dimethyl ether through ethylene glycol monomethyl ether

    CN107141201A

  • Application of supported heteropoly acid catalyst in preparation of 9,9-bi(4-amido aryl) fluorene type compound

    CN108863807A

  • Method for producing (POLY)alkylene glycol dialkyl ether

    JP2016014001A