A powder metallurgy oil-containing bearing and a preparation method thereof
By increasing the copper content, reducing the graphite content and adding molybdenum disulfide, combined with the use of modified base oil to form a protective film, the problem of limited friction reduction performance of powder metallurgy Fe-Cu-based oil-containing bearings at high temperatures is solved, and excellent Anti-wear and corrosion resistance.
Patent Information
- Application Number
- CN202410903522.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-08
AI Technical Summary
Existing powder metallurgical Fe-Cu-based oil-containing bearings have limited friction reduction performance at high temperatures, and graphite-assisted lubrication has the risk of noise and excessive hardness.
By increasing the copper content, reducing the graphite content, and adding molybdenum disulfide, combining copper nanoparticle modified base oil and copper complex modified base oil as lubricant, an organic composite film and iron-copper alloy protective film are formed to enhance the bearings anti-wear properties.
Excellent anti-wear performance under the same oil content conditions is achieved, the friction coefficient is reduced, the corrosion resistance of the bearing and the reduction of operating noise are improved.
Smart Images

Figure BDA0004931266610000081 
Figure BDA0004931266610000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of powder metallurgy, in particular to a powder metallurgy oil-containing bearing and a preparation method thereof. Background Art
[0002] Powder metallurgy oil-containing bearings have been widely used in the machinery industry and have become an important mechanical structural part because of their ability to automatically supply lubricating oil, low friction coefficient, ideal running-in and wear resistance, and low manufacturing cost. At present, oil-containing bearings are mainly made of Fe-based, Cu-based and Fe-Cu-based materials.
[0003] Fe-based oil-containing bearing materials have high compressive strength and hardness, can withstand high loads, and have good wear resistance. In contrast, Cu-based oil-containing bearing materials have a small friction coefficient, low noise, good corrosion resistance, and stable operation, but their load-bearing capacity is relatively poor. Fe-Cu-based bearing materials have the advantages of both Fe-based and Cu-based materials, have good comprehensive performance, and are moderately priced. With the intensification of competition in the oil-containing bearing market, the market demand for Fe-Cu-based bearing materials continues to increase due to their excellent comprehensive performance.
[0004] Powder metallurgy Fe-Cu based oil-containing bearings not only have high physical and mechanical properties and good vibration load capacity, but also have good corrosion resistance. Their anti-friction performance is no less than that of bronze materials, and they are suitable for occasions that require both structural characteristics and bearing characteristics. A certain amount of graphite or MoS2 is usually added to Fe-based oil-containing bearing materials for auxiliary lubrication, so that the material has excellent damping characteristics and can produce bearings that run quietly. However, the content of combined carbon must be strictly controlled to prevent the formation of noise and bearings with excessive hardness. At the same time, MoS2 is easy to decompose at high temperatures, which limits its anti-friction performance to a certain extent.
[0005] Therefore, it is of great significance to invent an oil-containing bearing with excellent anti-friction and anti-wear properties. Summary of the invention
[0006] The object of the present invention is to provide a powder metallurgy oil-containing bearing and a preparation method thereof to solve the problems raised in the above background technology.
[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0008] A method for preparing a powder metallurgy oil-containing bearing comprises the following steps:
[0009] S1: Mixing: Mix iron powder, graphite powder, copper powder, molybdenum disulfide and zinc stearate according to the proportion and obtain a mixed powder;
[0010] S2: Pressing: putting the mixed powder into a mold and pressing it into a compact;
[0011] S3: Sintering: placing the compact in a hydrogen-nitrogen atmosphere and sintering at high temperature to obtain a semi-finished product;
[0012] S4: Post-processing: The semi-finished products sintered at high temperature are subjected to full finishing and vacuum oil immersion in turn to obtain oil-containing bearings.
[0013] Furthermore, in step S4, the lubricating oil used in the oil immersion process consists of copper nanoparticle-modified base oil, copper complex-modified base oil, and base oil.
[0014] Furthermore, the method for preparing the copper nanoparticle-modified base oil comprises the following steps:
[0015] Heat n-octanol to 60-70°C, add phosphorus pentasulfide in batches, wait until no gas is generated, heat to 90-100°C for reaction for 80-100 minutes, cool, filter, and obtain a thiophosphoric acid intermediate; use a saturated solution of sodium dodecylbenzenesulfonate base oil as a solvent, add cupric acetate, anhydrous sodium carbonate, hydrazine hydrate, thiophosphoric acid intermediate, and tetrabutylammonium bromide in sequence, heat to 85-90°C for reflux reaction for 4-5 hours, control the pH of the reflux process to 10-10.5, cool, add deionized water, shake, stand and separate, collect the oil phase, heat to 100°C and stir for 5-6 hours, and obtain a copper nanoparticle modified base oil.
[0016] Furthermore, in the thiophosphoric acid intermediate, phosphorus pentasulfide is added in 3-5 batches within 70-80 minutes; the molar ratio of n-octanol:phosphorus pentasulfide is 4:(1-1.3); and in the copper nanoparticle modified base oil, the mass ratio of copper acetate:hydrazine hydrate:thiophosphoric acid intermediate is 1:(5-8):(1-2).
[0017] Furthermore, the method for preparing the copper complex modified base oil comprises the following steps:
[0018] The saturated solution of sodium dodecylbenzene sulfonate base oil, ethanol and isooctyl alcohol are stirred evenly and heated to 78-80°C to obtain a reverse micelle solution; salicylaldehyde and ethylenediamine are added, and the mixture is kept warm and refluxed for 1-1.5 hours; copper acetate is added, and the mixture is kept warm and refluxed for 2-2.5 hours; the mixture is cooled, deionized water is added, and the mixture is shaken, and the mixture is allowed to stand and separate, and the oil phase is collected to obtain a copper complex modified base oil.
[0019] Furthermore, in the reverse micelle solution, the mass ratio of saturated solution of sodium dodecylbenzenesulfonate base oil: ethanol: isooctyl alcohol is (1.2-1.3):(0.2-0.3):(0.03-0.06); in the copper complex modified base oil, the mass ratio of salicylaldehyde: ethylenediamine: copper acetate is 2:1.5:2.
[0020] Furthermore, the proportions of the components in the lubricating oil, by mass percentage, are 40-50wt% of the base oil modified by copper nanoparticles, 40-50wt% of the base oil modified by copper complexes, and the rest is base oil.
[0021] Furthermore, the proportion of each component in the mixed powder, by mass percentage, is 1.0-1.5wt% of graphite powder, 18-20wt% of copper powder, 2-3wt% of molybdenum disulfide, and the rest is iron powder, and the amount of zinc stearate added is 0.4-0.5wt% of the total mass of the aforementioned raw materials.
[0022] Furthermore, the compact density is 6.2-6.3 g / cm 3 ; The gas atmosphere during the sintering process is 5% H2+95% N2 by volume; the sintering temperature is 1000-1050℃, and the time is 30-45min.
[0023] Furthermore, the mass of sodium dodecylbenzene sulfonate in the saturated solution of sodium dodecylbenzene sulfonate base oil is 0.26 g per 100 mL of base oil.
[0024] Furthermore, in the copper nanoparticle modified base oil, copper complex modified base oil, and base oil, the base oil is soybean oil.
[0025] Furthermore, in the copper nanoparticle-modified base oil, the content of copper nanoparticles is 1 wt %; in the copper complex-modified base oil, the content of copper complex is 1 wt % and the content of salicylic acid Schiff base is 1 wt %.
[0026] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0027] The present invention prepares an oil-containing bearing by increasing the copper content, reducing the graphite content, and adding a certain amount of molybdenum disulfide. The increase in copper content can enhance the corrosion resistance of the bearing material and reduce the noise during operation, but it will reduce the bearing capacity of the material. Therefore, the graphite content is reduced to avoid a large amount of graphite existing in a free form, weakening the overall strength of the bearing, and at the same time, reducing the impact on the copper-iron interface bonding, avoiding the impact of free graphite on the strengthening effect of copper, but the reduction in graphite content will reduce the oil content of the oil-containing bearing. Therefore, a certain amount of molybdenum disulfide is added. During the sintering process, molybdenum disulfide reacts with copper and part of the sulfur escapes in the form of gas, which increases the pores inside the bearing and improves the oil content of the oil-containing bearing.
[0028] Increasing the copper content, reducing the graphite content, and adding molybdenum disulfide can all reduce the friction coefficient of the oil-containing bearing and improve the anti-wear performance of the bearing. In order to further improve the anti-wear performance of the oil-containing bearing under the condition of the same oil content, the present invention prepares a lubricating oil composed of a copper nanoparticle modified base oil, a copper complex modified base oil, and a base oil, and uses the lubricating oil as the lubricating oil used in the vacuum oil impregnation step.
[0029] The invention uses a saturated solution of sodium dodecylbenzene sulfonate and soybean oil, ethanol, and isooctyl alcohol in a certain ratio to prepare a W / O (water / oil) type microemulsion reactor, and prepares a copper complex modified base oil containing nano-scale copper complex and Schiff base structure in a base oil matrix. The copper complex nanoparticles in the copper complex modified base oil are adsorbed on the friction surface of the bearing to form an organic composite film on the surface; at the same time, the salicylaldehyde Schiff base structure contains abundant -OH groups, which can easily improve the binding force between the organic composite film and the bearing surface through intermolecular hydrogen bonds, and ensure that the organic composite film plays a role in reducing friction and resisting wear during the friction process; as the load friction increases, the organic composite film formed by physical adsorption is destroyed, the copper complex nanoparticles begin to decompose under the action of friction heat, the copper ions decompose and precipitate in the form of copper element, enrich and adhere to the bearing surface, and further react chemically with the friction metal to generate a firm iron-copper alloy protective film, further ensuring the durability and stability of the friction and anti-wear effect.
[0030] The present invention adopts the same principle as above and uses soybean oil as solvent to prepare a copper nanoparticle modified base oil modified by phosphate sulfate. In the synthesis process, a tetrabutylammonium bromide phase transfer catalyst is added as a cosurfactant, and the tetrabutylammonium bromide molecules are inserted between the surfactant molecules of the oil-water interface film, thereby weakening the electrostatic repulsion between the ion heads of the ionic surfactant molecules and enhancing the stability of the interface film; by affecting the thermodynamic properties of the system, the instantaneous negative surface tension mechanism is exerted, and a strong interface film is used to protect the already generated ultrafine particles to prevent aggregation during the collision process, thereby achieving the effect of reducing the particle size of the copper nanoparticles, and the particle size is 5-6nm. The copper nanoparticles can smoothly enter the gap between the friction pairs under boundary lubrication by using the small particle size, increase the oil film thickness under boundary lubrication, and transform the relative motion between the friction pairs from the sliding friction state to the rolling friction state, thereby generating a "microball bearing effect", avoiding direct contact between the friction pairs, and further enhancing the friction reduction and anti-wear performance of the oil-containing bearing. DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] In the following examples, the base oil is soybean oil CAS: 8001-22-7; the iron powder has a particle size of 150 μm and a purity of 99.8 wt%; the graphite powder has a particle size of 50 μm and a purity of 99.5 wt%; the copper powder has a particle size of 65 μm and a purity of 99.9 wt%; and the remaining raw materials are commercially available.
[0033] Embodiment 1: A method for preparing a powder metallurgy oil-containing bearing: S1: Copper nanoparticle modified base oil: Heat 4 mol of n-octanol to 60°C, add 1 mol of phosphorus pentasulfide in batches, and when no gas is generated, heat to 90°C for reaction for 80 minutes, cool, and filter to obtain a thiophosphoric acid intermediate; use a saturated solution of sodium dodecylbenzenesulfonate base oil as a solvent, add 1g of copper acetate, 0.5g of anhydrous sodium carbonate, 5g of hydrazine hydrate, 1g of thiophosphoric acid intermediate, and 0.26g of tetrabutylammonium bromide in sequence, heat to 85°C and reflux for reaction for 4h, control the pH of the reflux process to 10, cool, add deionized water, shake, stand and separate, collect the oil phase, heat to 100°C and stir for 5-6h to obtain a copper nanoparticle modified base oil;
[0034] S2: Copper complex modified base oil: 120g of saturated solution of sodium dodecylbenzene sulfonate base oil, 20g of ethanol, and 3g of isooctyl alcohol were stirred evenly and heated to 78°C to obtain a reverse micelle solution; 2g of salicylaldehyde and 1.5g of ethylenediamine were added, and the mixture was refluxed for 1h, 2g of copper acetate was added, and the mixture was refluxed for 2h, cooled, deionized water was added, and the mixture was shaken and allowed to stand for separation.
[0035] collecting the oil phase to obtain the copper complex modified base oil;
[0036] S3: Mixing: 79wt% iron powder, 1wt% graphite powder, 18wt% copper powder, 2wt% molybdenum disulfide, and additional 0.5wt% zinc stearate are mixed uniformly to obtain a mixed powder;
[0037] S4: Pressing: The mixed powder is put into a mold and pressed to obtain a compact; the compact density is 6.2g / cm 3 ;
[0038] S5: Sintering: placing the compact in a 5% H2+95% N2 atmosphere and sintering at 1050°C for 30 minutes to obtain a semi-finished product;
[0039] S6: Post-processing: The semi-finished products sintered at high temperature are subjected to full finishing and vacuum oil immersion in turn to obtain oil-containing bearings.
[0040] In the above experiment, the lubricating oil used in the oil immersion process consists of 40 wt % copper nanoparticle modified base oil, 40 wt % copper complex modified base oil, and 20 wt % base oil.
[0041] Example 2: A method for preparing a powder metallurgy oil-containing bearing: S1: Copper nanoparticle modified base oil: Heat 4 mol of n-octanol to 60°C, add 1 mol of phosphorus pentasulfide in batches, and when no gas is generated, heat to 90°C for reaction for 80 minutes, cool, and filter to obtain a thiophosphoric acid intermediate; use a saturated solution of sodium dodecylbenzenesulfonate base oil as a solvent, add 1g of copper acetate, 0.5g of anhydrous sodium carbonate, 5g of hydrazine hydrate, 1g of thiophosphoric acid intermediate, and 0.26g of tetrabutylammonium bromide in sequence, heat to 85°C and reflux for reaction for 4h, control the pH of the reflux process to 10, cool, add deionized water, shake, stand and separate, collect the oil phase, heat to 100°C and stir for 5-6h to obtain a copper nanoparticle modified base oil;
[0042] S2: Copper complex modified base oil: 120g of saturated solution of sodium dodecylbenzene sulfonate base oil, 20g of ethanol and 3g of isooctyl alcohol were stirred evenly and heated to 78°C to obtain a reverse micelle solution; 2g of salicylaldehyde and 1.5g of ethylenediamine were added, and the mixture was kept warm and refluxed for 1h, 2g of copper acetate was added, and the mixture was kept warm and refluxed for 2h, cooled, deionized water was added, shaken, allowed to stand and separate, and the oil phase was collected to obtain a copper complex modified base oil;
[0043] S3: Mixing: 79wt% iron powder, 1wt% graphite powder, 18wt% copper powder, 2wt% molybdenum disulfide, and additional 0.5wt% zinc stearate are mixed uniformly to obtain a mixed powder;
[0044] S4: Pressing: The mixed powder is put into a mold and pressed to obtain a compact; the compact density is 6.2g / cm 3 ;
[0045] S5: Sintering: placing the compact in a 5% H2+95% N2 atmosphere and sintering at 1050°C for 30 minutes to obtain a semi-finished product;
[0046] S6: Post-processing: The semi-finished products sintered at high temperature are subjected to full finishing and vacuum oil immersion in turn to obtain oil-containing bearings.
[0047] In the above experiment, the lubricating oil used in the oil immersion process consists of 45 wt % copper nanoparticle modified base oil, 45 wt % copper complex modified base oil, and 10 wt % base oil.
[0048] Example 3: A method for preparing a powder metallurgy oil-containing bearing: S1: Copper nanoparticle modified base oil: Heat 4 mol of n-octanol to 60°C, add 1 mol of phosphorus pentasulfide in batches, and when no gas is generated, heat to 90°C for reaction for 80 minutes, cool, and filter to obtain a thiophosphoric acid intermediate; use a saturated solution of sodium dodecylbenzenesulfonate base oil as a solvent, add 1g of copper acetate, 0.5g of anhydrous sodium carbonate, 5g of hydrazine hydrate, 1g of thiophosphoric acid intermediate, and 0.26g of tetrabutylammonium bromide in sequence, heat to 85°C and reflux for reaction for 4h, control the pH of the reflux process to 10, cool, add deionized water, shake, stand and separate, collect the oil phase, heat to 100°C and stir for 5-6h to obtain a copper nanoparticle modified base oil;
[0049] S2: Copper complex modified base oil: 120g of saturated solution of sodium dodecylbenzene sulfonate base oil, 20g of ethanol and 3g of isooctyl alcohol were stirred evenly and heated to 78°C to obtain a reverse micelle solution; 2g of salicylaldehyde and 1.5g of ethylenediamine were added, and the mixture was kept warm and refluxed for 1h, 2g of copper acetate was added, and the mixture was kept warm and refluxed for 2h, cooled, deionized water was added, shaken, allowed to stand and separate, and the oil phase was collected to obtain a copper complex modified base oil;
[0050] S3: Mixing: 79wt% iron powder, 1wt% graphite powder, 18wt% copper powder, 2wt% molybdenum disulfide, and additional 0.5wt% zinc stearate are mixed uniformly to obtain a mixed powder;
[0051] S4: Pressing: The mixed powder is put into a mold and pressed to obtain a compact; the compact density is 6.2g / cm 3 ;
[0052] S5: Sintering: placing the compact in a 5% H2+95% N2 atmosphere and sintering at 1050°C for 30 minutes to obtain a semi-finished product;
[0053] S6: Post-processing: The semi-finished products sintered at high temperature are subjected to full finishing and vacuum oil immersion in turn to obtain oil-containing bearings.
[0054] In the above experiment, the lubricating oil used in the oil immersion process consists of 50 wt % copper nanoparticle modified base oil and 50 wt % copper complex modified base oil.
[0055] Comparative Example 1: A method for preparing a powder metallurgy oil-containing bearing: S1: Mixing: 79wt% iron powder, 1wt% graphite powder, 18wt% copper powder, 2wt% molybdenum disulfide, and additional 0.5wt% zinc stearate are mixed uniformly to obtain a mixed powder;
[0056] S2: Pressing: The mixed powder is put into a mold and pressed to obtain a compact; the compact density is 6.2g / cm 3 ;
[0057] S3: Sintering: placing the compact in a 5% H2+95% N2 atmosphere and sintering at 1050°C for 30 minutes to obtain a semi-finished product;
[0058] S4: Post-processing: The semi-finished products sintered at high temperature are subjected to full finishing and vacuum oil immersion in turn to obtain oil-containing bearings.
[0059] In the above experiments, the lubricating oil used in the oil immersion process consisted of 100 wt % base oil.
[0060] Comparative Example 2: A method for preparing a powder metallurgy oil-containing bearing: S1: Mixing: 79wt% iron powder, 1wt% graphite powder, 18wt% copper powder, 2wt% molybdenum disulfide, and additional 0.5wt% zinc stearate are mixed uniformly to obtain a mixed powder;
[0061] S2: Pressing: The mixed powder is put into a mold and pressed to obtain a compact; the compact density is 6.2g / cm 3 ;
[0062] S3: Sintering: placing the compact in a 5% H2+95% N2 atmosphere and sintering at 1050°C for 30 minutes to obtain a semi-finished product;
[0063] S4: Post-processing: The semi-finished products sintered at high temperature are subjected to full finishing and vacuum oil immersion in turn to obtain oil-containing bearings.
[0064] In the above experiment, the lubricating oil used in the oil immersion process consisted of 2 wt % copper powder and 98 wt % base oil.
[0065] In the above experiment, the lubricating oil used in the oil immersion process consists of 40 wt % copper nanoparticle modified base oil, 40 wt % copper complex modified base oil, and 20 wt % base oil.
[0066] Comparative Example 3: A method for preparing a powder metallurgy oil-containing bearing: S1: Copper nanoparticle modified base oil: 4 mol of n-octanol is heated to 60°C, 1 mol of phosphorus pentasulfide is added in batches, and when no gas is generated, it is heated to 90°C for reaction for 80 minutes, cooled, filtered, and a thiophosphoric acid intermediate is obtained; a saturated solution of sodium dodecylbenzenesulfonate base oil is used as a solvent, 1g of copper acetate, 0.5g of anhydrous sodium carbonate, 5g of hydrazine hydrate, 1g of thiophosphoric acid intermediate, and 0.26g of tetrabutylammonium bromide are added in sequence, heated to 85°C for reflux reaction for 4h, the pH of the reflux process is controlled to be 10, cooled, deionized water is added, shaken, the liquid is separated by standing, the oil phase is collected, heated to 100°C and stirred for 5-6h, petroleum ether is added for demulsification, and a precipitate is obtained; the precipitate is washed until the oil and fat are completely removed to obtain copper nanoparticles; 1wt% of copper nanoparticles are added to the base oil to obtain a copper nanoparticle modified base oil;
[0067] S2: Copper complex modified base oil: 120g of saturated solution of sodium dodecylbenzene sulfonate base oil, 20g of ethanol, and 3g of isooctyl alcohol were stirred evenly and heated to 78°C to obtain a reverse micelle solution; 2g of salicylaldehyde and 1.5g of ethylenediamine were added, and the mixture was refluxed for 1h, 2g of copper acetate was added, and the mixture was refluxed for 2h, cooled, deionized water was added, and the mixture was shaken and allowed to stand for separation.
[0068] collecting the oil phase to obtain the copper complex modified base oil;
[0069] S3: Mixing: 79wt% iron powder, 1wt% graphite powder, 18wt% copper powder, 2wt% molybdenum disulfide, and additional 0.5wt% zinc stearate are mixed uniformly to obtain a mixed powder;
[0070] S4: Pressing: The mixed powder is put into a mold and pressed to obtain a compact; the compact density is 6.2g / cm 3 ;
[0071] S5: Sintering: placing the compact in a 5% H2+95% N2 atmosphere and sintering at 1050°C for 30 minutes to obtain a semi-finished product;
[0072] S6: Post-processing: The semi-finished products sintered at high temperature are subjected to full finishing and vacuum oil immersion in turn to obtain oil-containing bearings.
[0073] In the above experiment, the lubricating oil used in the oil immersion process consists of 40 wt % copper nanoparticle modified base oil, 40 wt % copper complex modified base oil, and 20 wt % base oil.
[0074] Comparative Example 4: A method for preparing a powder metallurgy oil-containing bearing: S1: Copper nanoparticle modified base oil: Heat 4 mol of n-octanol to 60°C, add 1 mol of phosphorus pentasulfide in batches, and wait until no gas is generated, heat to 90°C for reaction for 80 minutes, cool, and filter to obtain a thiophosphoric acid intermediate; use a saturated solution of sodium dodecylbenzenesulfonate base oil as a solvent, add 1g of copper acetate, 0.5g of anhydrous sodium carbonate, 5g of hydrazine hydrate, 1g of thiophosphoric acid intermediate, and 0.26g of tetrabutylammonium bromide in sequence, heat to 85°C and reflux for reaction for 4h, control the pH of the reflux process to 10, cool, add deionized water, shake, stand and separate, collect the oil phase, heat to 100°C and stir for 5-6h to obtain a copper nanoparticle modified base oil;
[0075] S2: Copper complex modified base oil: 120g of saturated solution of sodium dodecylbenzene sulfonate base oil, 20g of ethanol and 3g of isooctyl alcohol were stirred evenly and heated to 78°C to obtain a reverse micelle solution; 2g of salicylaldehyde and 1.5g of ethylenediamine were added, and the mixture was kept warm and refluxed for 1h, 2g of copper acetate was added, and the mixture was kept warm and refluxed for 2h, cooled, deionized water was added, shaken, and the mixture was allowed to stand for separation, the oil phase was collected, and petroleum ether was added to break the emulsion to obtain a precipitate; the precipitate was washed until the oil and fat were completely removed to obtain a copper complex; 1wt% of the copper complex was added to the base oil to obtain a copper complex modified base oil;
[0076] S3: Mixing: 79wt% iron powder, 1wt% graphite powder, 18wt% copper powder, 2wt% molybdenum disulfide, and additional 0.5wt% zinc stearate are mixed uniformly to obtain a mixed powder;
[0077] S4: Pressing: The mixed powder is put into a mold and pressed to obtain a compact; the compact density is 6.2g / cm 3 ;
[0078] S5: Sintering: placing the compact in a 5% H2+95% N2 atmosphere and sintering at 1050°C for 30 minutes to obtain a semi-finished product;
[0079] S6: Post-processing: The semi-finished products sintered at high temperature are subjected to full finishing and vacuum oil immersion in turn to obtain oil-containing bearings.
[0080] In the above experiment, the lubricating oil used in the oil immersion process is composed of 40wt% copper nanoparticle modified base oil, 40wt% copper complex modified base oil, and 20wt% base oil.
[0081] Experiment: Crushing strength: Use a universal testing machine to test the radial crushing strength of the bearing.
[0082] Wear performance: At room temperature, the wear performance test was carried out using a wear testing machine. The pair was a φ70mm×8mm grinding disc made of 42CrMo with a hardness of 55-57HRC.
[0083] Oil content: Use an oil content density tester to test the oil content of the bearing.
[0084] Table 1 Oil-bearing performance test data
[0085]
[0086]
[0087] Conclusion: The oil-containing bearing prepared by the present invention has excellent wear resistance.
[0088] In Comparative Example 1, ordinary commercial soybean oil was used as the lubricating oil immersion oil, and in Comparative Example 2, ordinary commercial copper powder was directly blended with soybean oil as the lubricating oil immersion oil; both resulted in reduced wear performance of the oil-containing bearing.
[0089] In Comparative Examples 3 and 4, copper nanoparticles and copper complexes were separated from the reaction solvent, and then added to the base oil for blending to prepare copper nanoparticle-modified base oil and copper complex-modified base oil; due to the dispersion conditions in the separated lubricating oil, some copper nanoparticles and copper complexes will have agglomerated forms after separation, which reduces their dispersion performance in their respective original solvents. In addition, the copper complex-modified base oil also loses the salicylaldehyde Schiff base structure in the original system solvent due to separation, resulting in reduced wear performance.
[0090] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a powder metallurgy oil-containing bearing, characterized in that: The following steps are involved: S1: Mixing: Mix iron powder, graphite powder, copper powder, molybdenum disulfide and zinc stearate according to the proportion and obtain a mixed powder; S2: Pressing: putting the mixed powder into a mold and pressing it into a compact; S3: Sintering: placing the compact in a hydrogen-nitrogen atmosphere and sintering at a high temperature of 1000-1050°C to obtain a semi-finished product; S4: Post-processing: The semi-finished products sintered at high temperature are subjected to full finishing and vacuum oil immersion in turn to obtain oil-containing bearings; In the step S4, the lubricating oil used in the oil immersion process is composed of copper nanoparticle modified base oil, copper complex modified base oil, and base oil, and the base oil is soybean oil; The method for preparing the copper nanoparticle modified base oil comprises the following steps: The n-octanol is heated to 60-70°C, phosphorus pentasulfide is added in batches, and when no gas is generated, the reaction is heated to 90-100°C for 80-100 minutes, cooled, and filtered to obtain a thiophosphoric acid intermediate; a saturated solution of sodium dodecylbenzenesulfonate base oil is used as a solvent, copper acetate, anhydrous sodium carbonate, hydrazine hydrate, thiophosphoric acid intermediate, and tetrabutylammonium bromide are added in sequence, and the reaction is heated to 85-90°C for reflux reaction for 4-5 hours, and the pH value of the reflux process is controlled to be 10-10.5, cooled, deionized water is added, shaken, and the liquid is separated by standing, and the oil phase is collected, and the reaction is heated to 100°C and stirred for 5-6 hours to obtain a copper nanoparticle modified base oil; The method for preparing the copper complex modified base oil comprises the following steps: The saturated solution of sodium dodecylbenzene sulfonate base oil, ethanol and isooctyl alcohol are stirred evenly and heated to 78-80°C to obtain a reverse micelle solution; salicylaldehyde and ethylenediamine are added, and the mixture is kept warm and refluxed for 1-1.5 hours; copper acetate is added, and the mixture is kept warm and refluxed for 2-2.5 hours; the mixture is cooled, deionized water is added, and the mixture is shaken, and the mixture is allowed to stand and separate, and the oil phase is collected to obtain a copper complex modified base oil.
2. The method for preparing a powder metallurgy oil-containing bearing according to claim 1, characterized in that: The proportions of the components in the mixed powder are, by mass percentage, 1.0-1.5wt% of graphite powder, 18-20wt% of copper powder, 2-3wt% of molybdenum disulfide, and the rest is iron powder. The amount of zinc stearate added is 0.4-0.5wt% of the total mass of the above raw materials.
3. The method for preparing a powder metallurgy oil-containing bearing according to claim 1, characterized in that: The compact density is 6.2-6.3 g / cm 3 ; The gas atmosphere during sintering is 5% H 2 +95%N 2 ; The sintering temperature is 1000-1050°C and the sintering time is 30-45min.
4. The method for preparing a powder metallurgy oil-containing bearing according to claim 1, characterized in that: In the thiophosphoric acid intermediate, phosphorus pentasulfide is added in 3-5 batches within 70-80 minutes; the molar ratio of n-octanol:phosphorus pentasulfide is 4:(1-1.3); in the copper nanoparticle modified base oil, the mass ratio of copper acetate:hydrazine hydrate:thiophosphoric acid intermediate is 1:(5-8):(1-2).
5. The method for preparing a powder metallurgy oil-containing bearing according to claim 1, characterized in that: In the reverse micelle solution, the mass ratio of saturated solution of sodium dodecylbenzenesulfonate base oil: ethanol: isooctyl alcohol is (1.2-1.3): (0.2-0.3): (0.03-0.06); in the copper complex modified base oil, the mass ratio of salicylaldehyde: ethylenediamine: copper acetate is 2:1.5:
2.
6. The method for preparing a powder metallurgy oil-containing bearing according to claim 1, characterized in that: The proportions of the components in the lubricating oil, by weight percentage, are 40-50 wt % of the base oil modified by copper nanoparticles, 40-50 wt % of the base oil modified by copper complexes, and the rest is base oil.
7. A powder metallurgy oil-containing bearing prepared according to the method for preparing a powder metallurgy oil-containing bearing according to any one of claims 1 to 6.
Citation Information
Patent Citations
High-performance iron-based powder metallurgy oil-containing self-lubricating bearing and production process thereof
CN102062149A
Method for manufacturing sintered bearing, sintered bearing, and vibration motor equipped with same
CN105009425A