A guar gum silane prepolymer modified solid acrylic resin and preparation method thereof

By introducing guar silane prepolymer and multifunctional silane coupling agent into solid acrylic resin, the problem of insufficient performance of polyurethane hot melt adhesive in high temperature and high humidity environments is solved, and its compatibility, initial viscosity and Heat resistance enhances the adhesive strength.

CN118652380BActive Publication Date: 2024-11-01RETACHEM ANQING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411133243.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-01
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The existing reactive polyurethane hot melt adhesives have problems such as high melting temperature, large viscosity, poor initial viscosity, insufficient flexibility and heat resistance in high temperature and high humidity environments, and the solid acrylic resin has poor compatibility with it, resulting in Applications are limited in high temperature environments.

Method used

By introducing guar silane prepolymer into solid acrylic resin, increasing hydroxyl and ether bonds, improving compatibility and initial viscosity, and enhancing the cementing strength and heat resistance of the final cured adhesive using a multifunctional silane coupling agent. .

Benefits of technology

The compatibility and initial adhesion of solid acrylic resin and polyurethane hot melt adhesive is significantly improved, the flexibility and heat resistance of the adhesive are enhanced, and the bonding strength and heat resistance of the adhesive are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of adhesive resin synthesis, and discloses a guar gum silane prepolymer modified solid acrylic resin and a preparation method thereof, wherein the guar gum silane prepolymer modified solid acrylic resin is composed of the following components: 100 parts by weight of acrylate monomer, 10-30 parts by weight of guar gum silane prepolymer, 1-5 parts by weight of catalyst, 1-5 parts by weight of suspending agent, and 300 parts by weight of deionized water. The invention introduces a large amount of hydroxyl groups of the guar gum silane prepolymer into the solid acrylic resin, thereby increasing the compatibility and initial viscosity with a polyurethane hot melt adhesive, the introduction of ether bonds improves the flexibility of the adhesive, and the multifunctional silane coupling agent improves the bonding strength and heat resistance of the final cured adhesive layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesive resin synthesis, and in particular to a guar gum silane prepolymer modified solid acrylate resin and a preparation method thereof. Background Art

[0002] Reactive polyurethane hot melt adhesive (PUR) uses the residual NCO group in the structure to react with moisture in the air or on the surface of the adherend to extend the chain, forming a high-molecular polymer with high cohesion between the two adherends, which significantly improves the adhesion and heat resistance. It has the characteristics of hot melt adhesives such as no solvent, high initial adhesion, and rapid positioning, as well as the properties of reactive adhesives such as temperature, humidity and medium resistance. This type of adhesive is currently widely used in furniture manufacturing, plastic decorative panels, metal hardware and other fields. Although the performance characteristics of reactive polyurethane hot melt adhesives are very outstanding, there are still some technical problems that need to be solved, such as reducing the melting temperature and melt viscosity, improving the initial adhesion, shortening the positioning time, and enhancing the flexibility, heat resistance and flame retardancy of the product.

[0003] The traditional modification method is to add 5-10% of thermoplastic resin to the polyurethane matrix resin, and then add a small amount of tackifying resin and antioxidants, catalysts, fillers and other additives for modification. Among them, the thermoplastic resin can shorten the positioning time of PUR, improve the cold setting time, initial adhesion, flexibility and film-forming properties of the adhesive, and is currently basically solid acrylic resin. However, the compatibility of solid acrylic resin and PUR resin is not good. When a large amount is added, coarse particles are likely to appear. While reducing the melting temperature and melt viscosity of the resin, it will greatly reduce the heat resistance of PUR and cannot meet the application in high temperature and high humidity environments. Summary of the invention

[0004] To this end, the technical problem to be solved by the present invention is to provide a guar gum silane prepolymer modified solid acrylic resin and a preparation method thereof. By introducing a large number of hydroxyl groups of the guar gum silane prepolymer into the solid acrylic resin, the compatibility and initial adhesion with the polyurethane hot melt adhesive can be increased, the introduction of ether bonds improves the flexibility of the adhesive, and the multifunctional silane coupling agent improves the bonding strength and heat resistance of the final cured adhesive layer.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A guar gum silane prepolymer modified solid acrylic resin is composed of the following components: 100 parts by weight of acrylate monomer, 10-30 parts by weight of guar gum silane prepolymer, 1-5 parts by weight of catalyst, 1-5 parts by weight of suspending agent and 300 parts by weight of deionized water; wherein the guar gum silane prepolymer is prepared from 100 parts by weight of guar gum, 20-60 parts by weight of silane coupling agent monomer, 1-3 parts by weight of potassium hydroxide and 200 parts by weight of deionized water by the following steps:

[0007] (1) Add guar gum and deionized water into a reactor, stir and heat to 80°C and keep warm for 30 minutes, then add potassium hydroxide;

[0008] (2) Slowly add the silane coupling agent dropwise into the reaction kettle for 1-2 hours. After the addition of the silane coupling agent, stir and heat to 90°C for 4 hours. After the reaction is completed, guar gum silane prepolymer is obtained.

[0009] The guar gum silane prepolymer modified solid acrylic resin, the acrylic acid ester monomer is one or more of methyl methacrylate, butyl acrylate, n-butyl methacrylate, isobutyl methacrylate.

[0010] The guar gum silane prepolymer modified solid acrylic resin, the catalyst is benzoyl peroxide or tert-butyl peroxide-2-ethylhexanoate.

[0011] The guar gum silane prepolymer modified solid acrylic resin, the suspending agent is one or more of polyvinyl alcohol, hydroxyethyl cellulose and sodium polyacrylate.

[0012] The guar gum silane prepolymer modified solid acrylic resin, the silane coupling agent is one of vinyl triethoxy silane, vinyl trimethoxy silane, vinyl tri (β-methoxyethoxy) silane and methacryloxypropyl trimethoxy silane.

[0013] The guar gum silane prepolymer modified solid acrylic resin is composed of the following components: 100 parts by weight of acrylate monomer, 10-30 parts by weight of guar gum silane prepolymer, 1-3 parts by weight of catalyst, 1-5 parts by weight of suspending agent and 300 parts by weight of deionized water.

[0014] The guar gum silane prepolymer modified solid acrylic resin is composed of the following components: 70 parts by weight of methyl methacrylate, 30 parts by weight of butyl acrylate, 30 parts by weight of guar gum silane prepolymer, 1 part by weight of catalyst benzoyl peroxide, 1 part by weight of suspending agent polyvinyl alcohol and 300 parts by weight of deionized water.

[0015] The guar gum silane prepolymer modified solid acrylic resin is prepared from 100 parts by weight of guar gum, 20 parts by weight of vinyl triethoxy silane, 1 part by weight of potassium hydroxide and 200 parts by weight of deionized water.

[0016] The guar gum silane prepolymer modified solid acrylic resin is prepared from 100 parts by weight of guar gum, 20-60 parts by weight of vinyltrimethoxysilane, 1-3 parts by weight of potassium hydroxide and 200 parts by weight of deionized water.

[0017] A method for preparing the above-mentioned guar gum silane prepolymer modified solid acrylic resin comprises the following steps:

[0018] (I) adding deionized water, a suspending agent and the first portion of acrylate monomer into a reaction kettle, passing nitrogen, starting stirring, and heating to 80° C., wherein the first portion of acrylate monomer accounts for 80% of the total weight of the acrylate monomer;

[0019] (II) adding guar gum silane prepolymer, stirring for 30 minutes, then adding the first catalyst, and keeping the temperature to react for 3 hours, wherein the first catalyst accounts for 80% of the total weight of the catalyst;

[0020] (III) adding a second portion of acrylate monomer and a second portion of catalyst to keep the temperature for reaction for 2 hours, wherein the second portion of acrylate monomer accounts for 20% of the total weight of acrylate monomer, the first portion of acrylate monomer and the second portion of acrylate monomer have the same composition, the second portion of catalyst accounts for 20% of the total weight of catalyst, and the first portion of catalyst and the second portion of catalyst have the same composition;

[0021] (IV) Cooling, filtering and drying the discharged material to obtain a solid acrylic resin powder.

[0022] The technical solution of the present invention achieves the following beneficial technical effects:

[0023] The guar gum silane prepolymer in the present invention is synthesized by guar gum and a silane coupling agent, and an unsaturated double bond is introduced to react with an acrylic resin for free radical polymerization, so that the prepolymer can be connected to the main structure of the resin at a low temperature of suspension polymerization. A large number of hydroxyl groups of the guar gum silane prepolymer are introduced into the solid acrylic resin, which can increase the compatibility and initial viscosity with the polyurethane hot melt adhesive, and the introduction of the ether bond improves the flexibility of the adhesive, while the multifunctional silane coupling agent improves the bonding strength and heat resistance of the final cured adhesive layer. DETAILED DESCRIPTION

[0024] Example 1

[0025] In this embodiment, the raw material composition is 70 parts by weight of methyl methacrylate and 30 parts by weight of butyl acrylate, 10 parts by weight of guar gum silane prepolymer, 1 part by weight of catalyst benzoyl peroxide, 1 part by weight of suspending agent polyvinyl alcohol, and 300 parts by weight of deionized water. The synthesis is carried out according to the following process:

[0026] (I) Deionized water, a suspending agent, and the first portion of the acrylate mixed monomer are added into a reaction kettle, nitrogen is introduced, stirring is started, and the temperature is raised to 80° C., wherein the first portion of the acrylate mixed monomer accounts for 80% of the total weight of the acrylate mixed monomer;

[0027] (II) adding guar gum silane prepolymer, stirring for 30 minutes, then adding the first catalyst, and keeping the temperature to react for 3 hours, wherein the first catalyst accounts for 80% of the total weight of the catalyst;

[0028] (III) adding a second portion of the acrylate mixed monomer and a second portion of the catalyst and keeping the mixture warm for 2 hours, wherein the second portion of the acrylate mixed monomer accounts for 20% of the total weight of the acrylate mixed monomer, and the first portion of the acrylate mixed monomer and the second portion of the acrylate mixed monomer have the same composition, and the second portion of the catalyst monomer accounts for 20% of the total weight of the catalyst, and the first portion of the catalyst and the second portion of the catalyst have the same composition;

[0029] (IV) cooling, filtering and drying the discharged material to obtain guar gum silane prepolymer modified solid acrylic resin powder.

[0030] The guar gum silane prepolymer is prepared from 100 parts by weight of guar gum, 20 parts by weight of vinyl triethoxy silane, a silane coupling agent monomer, 1 part by weight of potassium hydroxide, and 200 parts by weight of deionized water by the following steps:

[0031] Add guar gum and deionized water into a reactor, stir and heat to 80°C and keep warm for 30 minutes, then add potassium hydroxide; slowly add vinyl triethoxysilane dropwise into the reactor for 1 hour, after the addition of vinyl triethoxysilane, stir and heat to 90°C and keep warm for 4 hours, and the guar gum silane prepolymer is obtained after the reaction is completed.

[0032] Example 2

[0033] The guar gum silane prepolymer modified solid acrylic resin in this embodiment is different from that in Embodiment 1 in that the amount of guar gum silane prepolymer added in this embodiment is 20 parts by weight.

[0034] Example 3

[0035] The guar gum silane prepolymer modified solid acrylic resin in this embodiment is different from that in Embodiment 1 in that the amount of guar gum silane prepolymer added in this embodiment is 30 parts by weight.

[0036] Example 4

[0037] The guar gum silane prepolymer modified solid acrylic resin in this embodiment is different from that in Embodiment 1 in that the amount of catalyst added in this embodiment is 3 parts by weight.

[0038] Example 5

[0039] The guar gum silane prepolymer modified solid acrylic resin in this embodiment is different from that in Embodiment 1 in that the amount of catalyst added in this embodiment is 5 parts by weight.

[0040] Example 6

[0041] The guar gum silane prepolymer modified solid acrylic resin in this embodiment is different from that in Embodiment 1 in that the amount of the silane coupling agent monomer added in this embodiment is 40 parts by weight.

[0042] Example 7

[0043] The guar gum silane prepolymer modified solid acrylic resin in this embodiment is different from that in Embodiment 1 in that the amount of the silane coupling agent monomer added in this embodiment is 60 parts by weight.

[0044] Example 8

[0045] The guar gum silane prepolymer modified solid acrylic resin in this embodiment is different from that in Embodiment 1 in that the dropping time of the silane coupling agent monomer in this embodiment is 2 hours.

[0046] Example 9

[0047] The guar gum silane prepolymer modified solid acrylic resin in this embodiment is different from that in Embodiment 1 in that the silane coupling agent monomer vinyl triethoxy silane in this embodiment is replaced by vinyl trimethoxy silane.

[0048] Example 10

[0049] The guar gum silane prepolymer modified solid acrylic resin in this embodiment is different from that in Embodiment 1 in that the silane coupling agent monomer vinyl triethoxy silane in this embodiment is replaced by vinyl tri (β-methoxyethoxy) silane.

[0050] Embodiment 11

[0051] The guar gum silane prepolymer modified solid acrylic resin in this embodiment is different from that in Embodiment 1 in that the silane coupling agent monomer vinyl triethoxy silane in this embodiment is replaced by methacryloxypropyl trimethoxy silane.

[0052] Comparative Example 1

[0053] The solid acrylic resin in this comparative example is different from that in Example 1 in that no guar gum silane prepolymer is added during the synthesis of the solid acrylic resin.

[0054] Comparative Example 2

[0055] The solid acrylic resin in this comparative example is different from that in comparative example 1 in that guar gum is added during the synthesis of the solid acrylic resin, and the amount of guar gum used is the same as that of the guar gum silane prepolymer used in Example 1.

[0056] Comparative Example 3

[0057] The solid acrylic resin in this comparative example is different from that in comparative example 1 in that vinyl triethoxy silane is added during the synthesis of the solid acrylic resin, and the amount of vinyl triethoxy silane used is the same as that of the guar gum silane prepolymer in Example 1.

[0058] Comparative Example 4

[0059] The solid acrylic resin in this comparative example is different from that in comparative example 1 in that guar gum and vinyl triethoxysilane are added during the synthesis of the solid acrylic resin, the sum of the amounts of guar gum and vinyl triethoxysilane used is the same as the amount of guar gum silane prepolymer used in Example 1, and the weight ratio of guar gum to vinyl triethoxysilane in this example is the same as the weight ratio of guar gum to vinyl triethoxysilane in Example 1.

[0060] The guar gum silane prepolymer modified solid acrylic resin prepared in Examples 1 to 11 and the solid acrylic resin prepared in Comparative Examples 1 to 4 were tested for relevant properties in the following manner. The test results are shown in Table 1:

[0061] (1) The softening point is measured according to the ring and ball method in GB T 4507-2014 Determination of softening point of asphalt;

[0062] (2) The particle size was tested using Malvern's solid powder particle size analyzer;

[0063] (3) Polyurethane compatibility: melt and stir solid acrylic resin and polyurethane to check the transparency and the presence of particles after melting. Complete melting is grade 0, a small amount of particles is grade 1, and a large number of particles is grade 2.

[0064] (4) Bond strength: After the adhesive is melted, it is applied to the wood surface and bonded to the PVC edge banding strip before measurement.

[0065] Table 1 Comparison of resin properties

[0066]

[0067] From the data in Table 1, it can be seen that the use of guar gum silane prepolymer to modify solid acrylate can significantly improve the compatibility of solid acrylic resin and polyurethane, and at the same time improve the bonding strength of solid acrylic resin to a certain extent.

[0068] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the claims of this patent application.

Claims

1. A guar gum silane prepolymer modified solid acrylic resin, characterized in that: The invention comprises the following components: 100 parts by weight of acrylate monomer, 10-30 parts by weight of guar gum silane prepolymer, 1-5 parts by weight of catalyst, 1-5 parts by weight of suspending agent and 300 parts by weight of deionized water, wherein the acrylate monomer is methyl methacrylate and butyl acrylate; wherein the guar gum silane prepolymer is prepared from 100 parts by weight of guar gum, 20-60 parts by weight of silane coupling agent monomer, 1-3 parts by weight of potassium hydroxide and 200 parts by weight of deionized water by the following steps: (1) Add guar gum and deionized water into a reactor, stir and heat to 80°C and keep warm for 30 minutes, then add potassium hydroxide; (2) slowly adding the silane coupling agent dropwise into the reaction kettle for 1-2 hours. After the addition of the silane coupling agent, stirring and heating to 90° C. for 4 hours, the reaction is completed to obtain the guar gum silane prepolymer. The silane coupling agent is one of vinyl triethoxysilane, vinyl trimethoxysilane, vinyl tri(β-methoxyethoxy)silane and methacryloxypropyl trimethoxysilane.

2. The guar gum silane prepolymer modified solid acrylic resin according to claim 1, characterized in that: The catalyst is benzoyl peroxide or tert-butyl peroxide-2-ethylhexanoate.

3. The guar gum silane prepolymer modified solid acrylic resin according to claim 1, characterized in that: The suspending agent is one or more of polyvinyl alcohol, hydroxyethyl cellulose and sodium polyacrylate.

4. The guar gum silane prepolymer modified solid acrylic resin according to claim 1, characterized in that: The invention is composed of the following components: 100 parts by weight of acrylate monomer, 10-30 parts by weight of guar gum silane prepolymer, 1-3 parts by weight of catalyst, 1-5 parts by weight of suspending agent and 300 parts by weight of deionized water.

5. The guar gum silane prepolymer modified solid acrylic resin according to claim 1, characterized in that: The invention is composed of the following components: 70 parts by weight of methyl methacrylate, 30 parts by weight of butyl acrylate, 30 parts by weight of guar gum silane prepolymer, 1 part by weight of catalyst benzoyl peroxide, 1 part by weight of suspending agent polyvinyl alcohol and 300 parts by weight of deionized water.

6. The guar gum silane prepolymer modified solid acrylic resin according to claim 1, characterized in that: The guar gum silane prepolymer is prepared from 100 parts by weight of guar gum, 20 parts by weight of vinyltriethoxysilane, 1 part by weight of potassium hydroxide and 200 parts by weight of deionized water.

7. The guar gum silane prepolymer modified solid acrylic resin according to claim 1, characterized in that: The guar gum silane prepolymer is prepared from 100 parts by weight of guar gum, 20-60 parts by weight of vinyltrimethoxysilane, 1-3 parts by weight of potassium hydroxide and 200 parts by weight of deionized water.

8. A method for preparing a guar gum silane prepolymer modified solid acrylic resin according to claim 1, characterized in that: The steps include: (I) adding deionized water, a suspending agent and the first portion of acrylate monomer into a reaction kettle, passing nitrogen, starting stirring, and heating to 80° C., wherein the first portion of acrylate monomer accounts for 80% of the total weight of the acrylate monomer; (II) adding guar gum silane prepolymer, stirring for 30 minutes, then adding the first catalyst, and keeping the temperature to react for 3 hours, wherein the first catalyst accounts for 80% of the total weight of the catalyst; (III) adding a second portion of acrylate monomer and a second portion of catalyst to keep the temperature for reaction for 2 hours, wherein the second portion of acrylate monomer accounts for 20% of the total weight of acrylate monomer, the first portion of acrylate monomer and the second portion of acrylate monomer have the same composition, the second portion of catalyst accounts for 20% of the total weight of catalyst, and the first portion of catalyst and the second portion of catalyst have the same composition; (IV) Cooling, filtering and drying the discharged material to obtain a solid acrylic resin powder.