A high-performance waterproof and breathable polyurethane membrane material and preparation method thereof
By introducing modified porous biochar and diatomaceous earth, polyurethane membrane materials can maintain good moisture permeability and water pressure resistance while solving the problem of decreased waterproof and moisture permeability in existing technologies, thus realizing the application of high-performance polyurethane membrane materials.
Patent Information
- Application Number
- CN202411110081.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-14
AI Technical Summary
Existing polyurethane membrane materials have shortcomings in terms of waterproof and breathable properties and mechanical properties, especially after repeated washing, their performance deteriorates, and their microporous structure is unstable.
Modified porous biochar and modified diatomaceous earth are used as raw materials. A large number of through-pore structures and active groups are introduced into the polyurethane membrane material through specific chemical treatment methods to improve moisture permeability and water pressure resistance, and enhance mechanical properties through covalent bonding.
The prepared high-performance waterproof and breathable polyurethane membrane material retains good moisture permeability and water pressure resistance after multiple water washes, and has excellent mechanical properties, making it suitable for textiles.
Smart Images

Figure CN118652541B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane membrane materials, and in particular relates to a high-performance waterproof and moisture-permeable polyurethane membrane material and a preparation method thereof. Background Art
[0002] With the development of society and the continuous improvement of people's quality of life, there is an increasing demand for functional clothing, especially in sportswear fabrics, such as jackets, mountaineering suits, raincoats, etc., which need to have good waterproof and breathable properties. This not only requires preventing rain and snow from penetrating the fabric, but also allows the sweat discharged from the human body to be transferred to the outside of the body through the fabric in the form of water vapor to ensure wearing comfort. In recent years, waterproof and breathable fabrics have developed rapidly, and their application areas are not only limited to military supplies and medical protective supplies, but are also rapidly expanding to the field of outdoor leisure sportswear and equipment.
[0003] Waterproof and breathable fabrics are special functional fabrics that are both waterproof and breathable, and are vividly called "breathable fabrics". The main functions include waterproofing, windproofing, moisture permeability, and warmth retention. Specifically, it means that under a certain external pressure, raindrops cannot penetrate the fabric, and at the same time, it can effectively and quickly conduct the sweat vapor produced by the human body to the outside of the body, preventing sweat from condensing into sweat droplets in the clothing, providing a temperature and humidity balance in the micro-environment between the clothing and the human skin, and a good balance between waterproofing, breathability, windproofing and warmth retention, keeping the human body surface dry for a long time, and preventing mold, so as to achieve the purpose of wearing comfort.
[0004] There are two main types of polyurethane waterproof and breathable membranes: microporous waterproof and breathable membranes and dense waterproof and breathable membranes. The surface of the microporous waterproof and breathable membrane is distributed with a large number of micropores with a diameter of 2-20μm. Due to the effect of surface tension, such small micropores can prevent water droplets (water droplet diameter is 100-300μm) from passing through, but allow water molecules to pass through in the form of single molecules (water vapor diameter is about 0.4nm), thereby achieving waterproof (water droplets) and moisture permeability (water vapor) functions. The dense waterproof and breathable membrane is composed of hydrophilic polymers. Water vapor passes through the film through physical effects such as adsorption-diffusion-desorption with hydrophilic groups, making the membrane breathable.
[0005] Chinese patent CN108976766A discloses a waterproof and breathable polyurethane microporous film and a preparation method thereof, comprising the following components in parts by weight: 0.01-20.00 parts of aqueous ultrafine powder, 80.00-99.99 parts of polyurethane; the aqueous ultrafine powder is one or more of sodium chloride powder, glucose powder, aqueous titanium dioxide powder, aqueous titanium dioxide aerogel, aqueous graphene powder, aqueous silicon dioxide powder, aqueous silicon dioxide aerogel and aqueous ferric oxide powder in any combination; by controlling aqueous ultrafine powders of different proportions and different characteristics, waterproof and breathable microporous polyurethane films with different properties can be prepared. Among them, the micropores generated by the aqueous ultrafine powder can realize the waterproof and breathable function of the polyurethane film in the polyurethane film, and by controlling the size and distribution of the micropores, the prepared waterproof and breathable microporous polyurethane film can have different waterproof and breathable effects. However, the micropores in the patent are caused by the incompatibility between the ultrafine powder and the polyurethane matrix, which is bound to affect the mechanical properties and water pressure resistance of the polyurethane film, and the larger the micropores, the greater the impact on the mechanical properties and water pressure resistance of the polyurethane film. Chinese patent CN106867017A discloses a microporous membrane with controllable pore size and a preparation method thereof, wherein the microporous membrane is a polyurethane resin membrane, and its pore size is 0.5-20 μm, and the content of acid-soluble microparticles in the membrane is less than 5.0% by weight. By using acid-soluble microparticles in the coating resin and then dissolving them by acid treatment, a microporous membrane with controllable pore size can be obtained, the method is simple and easy, and the obtained microporous membrane has excellent water pressure resistance and moisture permeability, soft hand feel, and can be used in outdoor sportswear and other aspects, and has broad application prospects. The invention uses an acid-soluble method to dissolve acid-soluble microparticles to form micropores, realize controllable pore size, and have a good moisture permeability effect. However, the technology may have insufficient dissolution, thereby affecting the porosity, so that the waterproof and breathable membrane cannot achieve the expected optimal performance. Summary of the invention
[0006] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a high-performance waterproof and breathable polyurethane membrane material and a preparation method thereof. The polyurethane membrane material has good mechanical properties, good waterproofness, and strong moisture permeability. The prepared fabric has strong water wash resistance, high water pressure resistance, and good air permeability, and is very suitable for textiles.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] A high-performance waterproof and breathable polyurethane membrane material, comprising the following raw materials in parts by weight:
[0009] 60-80 parts of polyether diol, 35-50 parts of diisocyanate, 40-50 parts of organic solvent, 8-14 parts of modified porous biochar, 4-8 parts of modified diatomaceous earth, 5-10 parts of chain extender, 2-3 parts of thickener, 1-2 parts of defoamer, 0.1-0.2 parts of ultraviolet absorber, 0.05-0.1 parts of dibutyltin dilaurate;
[0010] The modified diatomaceous earth is obtained by treating with a silane coupling agent and then grafting with 2-acrylamide-2-methylpropanesulfonic acid.
[0011] In the present invention, the high-performance waterproof and breathable polyurethane membrane material uses polyether diol and diisocyanate as raw materials, and by adding modified porous biochar and modified diatomaceous earth, it contains a large number of through-hole structures inside, which can serve as a transmission channel for water vapor, thereby improving the moisture permeability of the polyurethane membrane material.
[0012] Preferably, the polyether diol is a polypropylene oxide ether diol with a molecular weight of 3000-4000; the diisocyanate is one or more of isophorone diisocyanate, dicyclohexylmethane diisocyanate, and hexamethylene diisocyanate; the chain extender is one or more of ethylene glycol, 1,3-propylene glycol, and ethylenediamine; the thickener is a polyurethane associative thickener; the ultraviolet absorber is one or more of UV-9, UV-531, and UVP-327; and the defoamer is a silicone defoamer.
[0013] Preferably, the specific preparation method of the modified diatomaceous earth is as follows:
[0014] The diatomaceous earth is added to a sodium hydroxide solution with a mass fraction of 10%, and stirred and impregnated. After the stirring and impregnation, the solution is filtered, dried, and calcined to obtain pretreated diatomaceous earth. The pretreated diatomaceous earth is added to an ethanol aqueous solution, and then vinyl triethoxysilane is added to react at a constant temperature. After the reaction is completed, the solution is filtered, washed, and dried to obtain vinyl diatomaceous earth. The vinyl diatomaceous earth is added to DMF, and then 2-acrylamido-2-methylpropanesulfonic acid and ammonium persulfate are added to react by heating. After the reaction is completed, the solution is filtered, washed, and dried to obtain the product.
[0015] Preferably, the stirring and impregnation temperature is 40-50°C, the time is 1-2h, the calcination temperature is 350-450°C, and the time is 1-2h; the mass ratio of the pretreated diatomaceous earth and vinyltriethoxysilane is 50:5-9, the constant temperature reaction temperature is 60-70°C, and the time is 2-3h; the ratio of the vinyl diatomaceous earth, 2-acrylamido-2-methylpropanesulfonic acid, and ammonium persulfate is 50:5-9:0.3-0.6, the heating reaction temperature is 80-90°C, and the time is 3-4h.
[0016] In the present invention, the addition of modified diatomite can effectively improve the moisture absorption and anti-humidity performance of the polyurethane film material. Diatomite has a unique orderly arranged microporous structure, high porosity, large pore volume, large specific surface area, and good humidity control effect. The diatomite is first treated with alkali to remove impurities in the micropores of the diatomite, so that more micropores inside the diatomite are exposed, the specific surface area of the diatomite is increased, and the moisture absorption performance of the diatomite is improved; then the diatomite is reacted with vinyl triethoxysilane to improve the dispersibility of the diatomite, and at the same time, active double bond groups are introduced into the diatomite, which is conducive to the subsequent reaction; then the vinyl diatomite is reacted with 2-acrylamide-2-methylpropane sulfonic acid to introduce strong hydrophilic groups such as amide groups and sulfonic acid groups into the diatomite, thereby improving the adsorption of diatomite to water vapor molecules, which is conducive to improving the moisture permeability of the polyurethane film material.
[0017] Preferably, the method for preparing the modified porous biochar comprises the following steps:
[0018] S1. Add corn stalk powder to deionized water, then add urea and cetyl ammonium bromide to carry out hydrothermal carbonization reaction. After the reaction is completed, filter, wash and dry. Then mix the solid product with potassium hydroxide and roast it in a nitrogen atmosphere. After the roasting is completed, soak it in a nitric acid solution, then wash and dry it to obtain porous biochar;
[0019] S2, adding the porous biochar prepared in step S1 to an ethanol aqueous solution, and then adding γ-mercaptopropyltrimethoxysilane, stirring to react, and filtering, washing, and drying after the reaction is completed to obtain a thiolated porous biochar;
[0020] S3. Add DMF to the thiol-modified porous biochar in step S2, and then add 2-(trifluoromethyl)acrylic acid and benzophenone to carry out a thiol-ene reaction under ultraviolet light. After the reaction is completed, filter, wash and dry to obtain the modified porous biochar.
[0021] Preferably, in step S1, the mass ratio of corn straw powder, deionized water, urea and hexadecyl ammonium bromide is 70-80:1000:40-50:5-10, the temperature of the hydrothermal carbonization reaction is 180-220°C, and the time is 4-7h; the mass ratio of the solid product and potassium hydroxide is 20-30:15-20, the roasting temperature is 650-750°C, and the time is 2-3h.
[0022] In the present invention, through a specific preparation method, the obtained porous biochar contains a large number of porous structures, which can be beneficial to the transmission of water vapor molecules. At the same time, since the diameter of the micropores in the prepared modified porous biochar is basically less than 10μm, it can effectively prevent water droplets from passing through and has good water pressure resistance.
[0023] Preferably, in step S2, the mass ratio of the porous biochar to γ-mercaptopropyltrimethoxysilane is 20-30:2-4, the temperature of the stirring reaction is 60-70° C., and the time is 1-2 h.
[0024] In the present invention, the porous biochar is reacted with γ-mercaptopropyltrimethoxysilane, thereby improving the dispersibility of the porous biochar and introducing mercapto groups into the porous biochar, which is beneficial to the subsequent reactions.
[0025] Preferably, in step S3, the mass ratio of the thiolated porous biochar, 2-(trifluoromethyl)acrylic acid, and benzophenone is 20-30:1.4-2.8:0.1-0.2, and the intensity of the ultraviolet light is 500-600 mW / cm 2 The temperature of the mercapto-ene reaction is 40-50°C and the time is 20-30 minutes.
[0026] In the present invention, 2-(trifluoromethyl)acrylic acid is introduced into the porous biochar through the thiol-ene reaction, and the short-chain fluorine-containing compound, 2-(trifluoromethyl)acrylic acid, is used as the hydrophobic surface of the porous biochar. Compared with long linear fluoroalkyl chain compounds, it will not release perfluoroalkyl sulfonates or perfluoroalkyl acids during the oxidative decomposition process, and has the characteristics of low toxicity and greater environmental protection. On the one hand, the introduced trifluoromethyl group can significantly improve the hydrophobic properties of the porous biochar, and on the other hand, the carboxyl group in 2-(trifluoromethyl)acrylic acid can react with isocyanate in the subsequent preparation of polyurethane membrane materials, and combine with polyurethane in the form of a covalent bond, thereby improving the binding performance of the two and improving the water washability of the polyurethane membrane material.
[0027] The present invention also protects a method for preparing the high-performance waterproof and breathable polyurethane film material as described above, comprising the following steps:
[0028] Add polyether diol and organic solvent into a reactor, add diisocyanate, ultraviolet absorber and dibutyltin dilaurate under nitrogen protection, and stir to react at 65-75°C. When the content of NCO group reaches 7%, add chain extender, modified porous biochar, modified diatomaceous earth, defoamer and thickener, and continue to react for 1-2 hours. After the reaction is completed, pour it onto release paper, use a scraper to scrape out a thin film on the surface of the release paper, and then dry it in a 90-100°C oven to form a film, so as to obtain the high-performance waterproof and moisture-permeable polyurethane membrane material.
[0029] The present invention also protects the use of the high-performance waterproof and breathable polyurethane membrane material in textiles.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) The high-performance waterproof and breathable polyurethane membrane material provided by the present invention is made of polyether diol and diisocyanate as raw materials. By adding modified porous biochar and modified diatomaceous earth, the polyurethane membrane material contains a large number of through-hole structures inside, which can serve as a transmission channel for water vapor, thereby improving the moisture permeability of the polyurethane membrane material; and the carboxyl groups contained in the modified porous biochar and modified diatomaceous earth can react with isocyanate when preparing the polyurethane membrane, so that the two are combined with the polyurethane in the form of covalent bonds, thereby improving the mechanical properties of the polyurethane membrane material, and also avoiding the problem that the micropores of the polyurethane membrane material become larger due to incompatibility between the porous biochar, modified diatomaceous earth and the polyurethane membrane after multiple water washings, thereby reducing the physical properties and water pressure resistance of the polyurethane membrane material.
[0032] (2) The high-performance waterproof and breathable polyurethane membrane material provided by the present invention contains modified diatomaceous earth. The diatomaceous earth is first treated with alkali to remove impurities in the micropores of the diatomaceous earth, so that more micropores inside the diatomaceous earth are exposed, thereby improving the hygroscopic performance of the diatomaceous earth. The diatomaceous earth is then reacted with vinyl triethoxysilane to improve the dispersibility of the diatomaceous earth and introduce active double bond groups into the diatomaceous earth, which is beneficial to the subsequent reaction. Finally, the vinyl diatomaceous earth is reacted with 2-acrylamide-2-methylpropane sulfonic acid to introduce strong hydrophilic groups such as amide groups and sulfonic acid groups into the diatomaceous earth, thereby improving the adsorption of diatomaceous earth to water vapor molecules, which is beneficial to improving the moisture permeability of the polyurethane membrane material. Through the good pore structure and rich pore coordination of the diatomaceous earth, water vapor is adsorbed by capillary action, and an entry and exit channel for water vapor molecules is provided for the polyurethane membrane material, thereby maintaining good moisture permeability.
[0033] (3) The high-performance waterproof and breathable polyurethane membrane material provided by the present invention contains a large number of porous structures in the modified porous biochar added by a specific preparation method. The porous structure can facilitate the transmission of water vapor molecules. At the same time, since the diameter of the micropores in the prepared modified porous biochar is basically less than 10 μm, it can effectively prevent water droplets from passing through and has good water pressure resistance. The porous biochar is then thiol-modified, and finally a short-chain fluorine-containing compound, 2-(trifluoromethyl)acrylic acid, is introduced into the porous biochar through a thiol-ene reaction. On the one hand, the introduced trifluoromethyl group can significantly improve the hydrophobicity of the porous biochar. On the other hand, the carboxyl group in 2-(trifluoromethyl)acrylic acid can react with isocyanate in the subsequent preparation of the polyurethane membrane material and combine with the polyurethane in the form of a covalent bond, thereby improving the binding performance of the two. The polyurethane membrane material has good physical properties and water pressure resistance after multiple water washings, thereby extending the service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1This is a SEM image of the modified porous biochar prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] In the present invention, the polypropylene oxide ether diol is purchased from Green Union (Jining) Chemical Technology Co., Ltd.; the particle size of the diatomaceous earth is 45-50 μm; the model of the polyurethane associative thickener is Dow RM-8W; and the silicone defoamer is a silicone polyether defoamer. Example 1
[0037] A high-performance waterproof and breathable polyurethane membrane material, comprising the following raw materials:
[0038] 70g of polyoxypropylene ether diol with a molecular weight of 3000, 45g of isophorone diisocyanate, 45g of ethyl acetate, 12g of modified porous biochar, 6g of modified diatomaceous earth, 8g of ethylene glycol, 2.5g of polyurethane associative thickener, 1.5g of silicone polyether defoamer, 0.15g of UV-9, and 0.08g of dibutyltin dilaurate.
[0039] Wherein, the specific preparation method of the modified diatomite is as follows:
[0040] 50 g of diatomaceous earth was added to 800 g of 10% sodium hydroxide solution by mass, and the mixture was stirred and impregnated at 45° C. for 1.5 h. After the stirring and impregnation, the mixture was filtered and dried, and calcined at 400° C. for 1.5 h to obtain pretreated diatomaceous earth. 50 g of pretreated diatomaceous earth was added to 800 mL of ethanol aqueous solution (the volume ratio of ethanol to water was 8:2), and then 7 g of vinyltriethoxysilane was added, and the mixture was reacted at a constant temperature of 65° C. for 2.5 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain vinyl diatomaceous earth. 50 g of vinyl diatomaceous earth was added to 800 mL of DMF, and then 7 g of 2-acrylamido-2-methylpropanesulfonic acid and 0.5 g of ammonium persulfate were added, and the mixture was reacted at 85° C. for 3.5 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain the product.
[0041] The method for preparing the modified porous biochar comprises the following steps:
[0042] S1. Add 75 g corn stalk powder (100 mesh) to 1000 g deionized water, then add 45 g urea and 8 g hexadecyl ammonium bromide, and perform hydrothermal carbonization reaction at 200 ° C for 6 h. After the reaction is completed, filter, wash and dry. Then, mix 25 g of the solid product with 18 g of potassium hydroxide, and roast it at 700 ° C in a nitrogen atmosphere for 2.5 h. After the roasting is completed, add it to a 10 wt% nitric acid solution and soak it for 1.5 h, then wash and dry it to obtain porous biochar;
[0043] S2, adding 25g of the porous biochar in step S1 to 500mL of ethanol aqueous solution (the volume ratio of ethanol to water is 8:2), then adding 3g of γ-mercaptopropyltrimethoxysilane, stirring and reacting at 65°C for 1.5h, filtering, washing and drying after the reaction is completed to obtain thiolated porous biochar;
[0044] S3, add 25g of thiolated porous biochar in step S2 to 600mL of DMF, then add 2.2g of 2-(trifluoromethyl)acrylic acid and 0.15g of benzophenone, and 2 , react at 45°C for 25 minutes. After the reaction is completed, filter, wash and dry to obtain modified porous biochar.
[0045] like Figure 1 As shown, the modified porous biochar prepared in this embodiment contains a large number of micropores, which are conducive to the transmission of water vapor molecules, and the diameter of the micropores is basically less than 10 μm, which can effectively prevent water droplets from passing through, so that the polyurethane membrane material has good water pressure resistance.
[0046] A method for preparing a high-performance waterproof and breathable polyurethane membrane material comprises the following steps:
[0047] The raw materials were weighed according to the above formula, and polyoxypropylene ether diol with a molecular weight of 3000 and ethyl acetate were added into the reactor. Under nitrogen protection, isophorone diisocyanate, UV-9 and dibutyltin dilaurate were added, and the reaction was stirred at 70°C. When the content of the NCO group reached 7%, ethylene glycol, modified porous biochar, modified diatomaceous earth, silicone polyether defoamer and polyurethane associative thickener were added, and the reaction was continued for 1.5 hours. After the reaction was completed, it was poured onto release paper, and a thin film was scraped out on the surface of the release paper with a scraper, and then dried in a 95°C oven to form a film, so as to obtain the high-performance waterproof and moisture-permeable polyurethane membrane material. Example 2
[0048] A high-performance waterproof and breathable polyurethane membrane material, comprising the following raw materials:
[0049] 70g of polyoxypropylene ether diol with a molecular weight of 4000, 40g of dicyclohexylmethane diisocyanate, 45g of ethyl acetate, 11g of modified porous biochar, 6g of modified diatomaceous earth, 7g of 1,3-propylene glycol, 2.5g of polyurethane associative thickener, 1.5g of silicone polyether defoamer, 0.15g of UV-531, and 0.07g of dibutyltin dilaurate.
[0050] Wherein, the specific preparation method of the modified diatomite is as follows:
[0051] 50 g of diatomaceous earth was added to 800 g of 10% sodium hydroxide solution by mass, and the mixture was stirred and impregnated at 45° C. for 1.5 h. After the stirring and impregnation, the mixture was filtered and dried, and calcined at 400° C. for 1.5 h to obtain pretreated diatomaceous earth. 50 g of pretreated diatomaceous earth was added to 800 mL of ethanol aqueous solution (the volume ratio of ethanol to water was 8:2), and then 7 g of vinyltriethoxysilane was added, and the mixture was reacted at a constant temperature of 65° C. for 2.5 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain vinyl diatomaceous earth. 50 g of vinyl diatomaceous earth was added to 800 mL of DMF, and then 7 g of 2-acrylamido-2-methylpropanesulfonic acid and 0.4 g of ammonium persulfate were added, and the mixture was reacted at 85° C. for 3.5 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain the obtained product.
[0052] The method for preparing the modified porous biochar comprises the following steps:
[0053] S1. Add 75 g corn stalk powder (100 mesh) to 1000 g deionized water, then add 45 g urea and 7 g hexadecyl ammonium bromide, and perform hydrothermal carbonization reaction at 210 ° C for 5 h. After the reaction is completed, filter, wash and dry. Then, mix 25 g of the solid product with 17 g of potassium hydroxide, and roast it at 700 ° C in a nitrogen atmosphere for 2.5 h. After the roasting is completed, add it to a 10 wt% nitric acid solution and soak it for 1.5 h, then wash and dry it to obtain porous biochar;
[0054] S2, adding 25g of the porous biochar in step S1 to 500mL of ethanol aqueous solution (the volume ratio of ethanol to water is 8:2), then adding 3g of γ-mercaptopropyltrimethoxysilane, stirring and reacting at 65°C for 1.5h, filtering, washing and drying after the reaction is completed to obtain thiolated porous biochar;
[0055] S3, add 25g of thiolated porous biochar in step S2 to 600mL of DMF, then add 2g of 2-(trifluoromethyl)acrylic acid and 0.15g of benzophenone, and 2 , react at 45°C for 25 minutes. After the reaction is completed, filter, wash and dry to obtain modified porous biochar.
[0056] A method for preparing a high-performance waterproof and breathable polyurethane membrane material comprises the following steps:
[0057] The raw materials were weighed according to the above formula, and polyoxypropylene ether diol with a molecular weight of 4000 and ethyl acetate were added into the reactor. Under nitrogen protection, dicyclohexylmethane diisocyanate, UV-531 and dibutyltin dilaurate were added, and the mixture was stirred and reacted at 70°C. When the content of the NCO group reached 7%, 1,3-propylene glycol, modified porous biochar, modified diatomaceous earth, silicone polyether defoamer and polyurethane associative thickener were added, and the reaction was continued for 1.5 hours. After the reaction was completed, the mixture was poured onto release paper, and a thin film was scraped out on the surface of the release paper with a scraper, and then dried in a 95°C oven to form a film, thereby obtaining the high-performance waterproof and moisture-permeable polyurethane membrane material. Example 3
[0058] A high-performance waterproof and breathable polyurethane membrane material, comprising the following raw materials:
[0059] 60g of polyoxypropylene ether diol with a molecular weight of 3000, 35g of hexamethylene diisocyanate, 40g of ethyl acetate, 8g of modified porous biochar, 4g of modified diatomaceous earth, 5g of ethylenediamine, 2g of polyurethane associative thickener, 1g of silicone polyether defoamer, 0.1g of UVP-327, and 0.05g of dibutyltin dilaurate.
[0060] Wherein, the specific preparation method of the modified diatomite is as follows:
[0061] 50 g of diatomaceous earth was added to 800 g of 10% sodium hydroxide solution by mass, and stirred and impregnated at 40°C for 2 h. After the stirring and impregnation was completed, the mixture was filtered and dried, and calcined at 350°C for 2 h to obtain pretreated diatomaceous earth; 50 g of pretreated diatomaceous earth was added to 800 mL of ethanol aqueous solution (the volume ratio of ethanol to water was 8:2), and then 5 g of vinyltriethoxysilane was added, and the mixture was reacted at a constant temperature of 60°C for 3 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain vinyl diatomaceous earth; 50 g of vinyl diatomaceous earth was added to 800 mL of DMF, and then 5 g of 2-acrylamido-2-methylpropanesulfonic acid and 0.3 g of ammonium persulfate were added, and the mixture was reacted at 80°C for 4 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain the obtained product.
[0062] The method for preparing the modified porous biochar comprises the following steps:
[0063] S1. Add 70 g corn stalk powder (100 mesh) to 1000 g deionized water, then add 40 g urea and 5 g hexadecyl ammonium bromide, and perform hydrothermal carbonization reaction at 180 ° C for 7 h. After the reaction is completed, filter, wash and dry. Then, mix 20 g of the solid product with 15 g potassium hydroxide, and roast it at 650 ° C for 3 h in a nitrogen atmosphere. After the roasting is completed, add it to a 10 wt% nitric acid solution and soak it for 1 h, then wash and dry it to obtain porous biochar;
[0064] S2, adding 20g of the porous biochar in step S1 to 500mL of ethanol aqueous solution (the volume ratio of ethanol to water is 8:2), then adding 2g of γ-mercaptopropyltrimethoxysilane, stirring and reacting at 60°C for 2h, filtering, washing and drying after the reaction is completed to obtain thiolated porous biochar;
[0065] S3, add 20g of thiolated porous biochar in step S2 to 600mL of DMF, then add 1.4g of 2-(trifluoromethyl)acrylic acid and 0.1g of benzophenone, and then add 100mL of thiolated porous biochar to the mixture under ultraviolet light intensity of 500mW / cm 2 , react at 40°C for 30 minutes. After the reaction is completed, filter, wash and dry to obtain modified porous biochar.
[0066] A method for preparing a high-performance waterproof and breathable polyurethane membrane material comprises the following steps:
[0067] The raw materials were weighed according to the above formula, and polypropylene oxide ether diol with a molecular weight of 3000 and ethyl acetate were added into the reactor. Under nitrogen protection, hexamethylene diisocyanate, UVP-327 and dibutyltin dilaurate were added, and the mixture was stirred and reacted at 65°C. When the content of the NCO group reached 7%, ethylenediamine, modified porous biochar, modified diatomaceous earth, silicone polyether defoamer and polyurethane associative thickener were added, and the reaction was continued for 2 hours. After the reaction was completed, the mixture was poured onto release paper, and a thin film was scraped out on the surface of the release paper with a scraper, and then dried in an oven at 90°C to form a film, thereby obtaining the high-performance waterproof and moisture-permeable polyurethane membrane material. Example 4
[0068] A high-performance waterproof and breathable polyurethane membrane material, comprising the following raw materials:
[0069] 80g of polyoxypropylene ether diol with a molecular weight of 4000, 50g of isophorone diisocyanate, 50g of ethyl acetate, 14g of modified porous biochar, 8g of modified diatomaceous earth, 10g of ethylene glycol, 3g of polyurethane associative thickener, 2g of silicone polyether defoamer, 0.2g of UV-9, and 0.1g of dibutyltin dilaurate.
[0070] Wherein, the specific preparation method of the modified diatomite is as follows:
[0071] 50 g of diatomaceous earth was added to 800 g of 10% sodium hydroxide solution by mass, and stirred and impregnated at 50° C. for 1 h. After the stirring and impregnation was completed, the mixture was filtered and dried, and calcined at 450° C. for 1 h to obtain pretreated diatomaceous earth; 50 g of pretreated diatomaceous earth was added to 800 mL of ethanol aqueous solution (the volume ratio of ethanol to water was 8:2), and then 9 g of vinyltriethoxysilane was added, and the mixture was reacted at a constant temperature of 70° C. for 2 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain vinyl diatomaceous earth; 50 g of vinyl diatomaceous earth was added to 800 mL of DMF, and then 9 g of 2-acrylamido-2-methylpropanesulfonic acid and 0.6 g of ammonium persulfate were added, and the mixture was reacted at 90° C. for 3 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain the product.
[0072] The method for preparing the modified porous biochar comprises the following steps:
[0073] S1. Add 80g corn stalk powder (100 mesh) to 1000g deionized water, then add 50g urea and 10g hexadecyl ammonium bromide, and perform hydrothermal carbonization reaction at 220°C for 4h. After the reaction is completed, filter, wash and dry. Then, mix 30g of the solid product with 20g potassium hydroxide, and roast it at 750°C in a nitrogen atmosphere for 2h. After the roasting is completed, add it to a 10wt% nitric acid solution and soak it for 2h, then wash and dry it to obtain porous biochar;
[0074] S2, adding 30g of the porous biochar in step S1 to 500mL of ethanol aqueous solution (the volume ratio of ethanol to water is 8:2), then adding 4g of γ-mercaptopropyltrimethoxysilane, stirring and reacting at 70°C for 1h, filtering, washing and drying after the reaction is completed to obtain thiolated porous biochar;
[0075] S3, add 30g of thiolated porous biochar in step S2 to 600mL of DMF, then add 2.8g of 2-(trifluoromethyl)acrylic acid and 0.2g of benzophenone, and 2 , react at 50°C for 20 minutes. After the reaction is completed, filter, wash and dry to obtain modified porous biochar.
[0076] A method for preparing a high-performance waterproof and breathable polyurethane membrane material comprises the following steps:
[0077] The raw materials were weighed according to the above formula, and polyoxypropylene ether diol with a molecular weight of 4000 and ethyl acetate were added into the reactor. Under nitrogen protection, isophorone diisocyanate, UV-9 and dibutyltin dilaurate were added, and the reaction was stirred at 75°C. When the content of the NCO group reached 7%, ethylene glycol, modified porous biochar, modified diatomaceous earth, silicone polyether defoamer and polyurethane associative thickener were added, and the reaction was continued for 1 hour. After the reaction was completed, it was poured onto release paper, and a thin film was scraped out on the surface of the release paper with a scraper, and then dried in an oven at 100°C to form a film, so as to obtain the high-performance waterproof and moisture-permeable polyurethane membrane material. Comparative Example 1
[0078] A high-performance waterproof and breathable polyurethane membrane material, comprising the following raw materials:
[0079] 70g of polyoxypropylene ether diol with a molecular weight of 3000, 45g of isophorone diisocyanate, 45g of ethyl acetate, 12g of porous biochar, 6g of modified diatomaceous earth, 8g of ethylene glycol, 2.5g of polyurethane associative thickener, 1.5g of silicone polyether defoamer, 0.15g of UV-9, and 0.08g of dibutyltin dilaurate.
[0080] Wherein, the specific preparation method of the modified diatomite is as follows:
[0081] 50 g of diatomaceous earth was added to 800 g of 10% sodium hydroxide solution by mass, and the mixture was stirred and impregnated at 45° C. for 1.5 h. After the stirring and impregnation, the mixture was filtered and dried, and calcined at 400° C. for 1.5 h to obtain pretreated diatomaceous earth. 50 g of pretreated diatomaceous earth was added to 800 mL of ethanol aqueous solution (the volume ratio of ethanol to water was 8:2), and then 7 g of vinyltriethoxysilane was added, and the mixture was reacted at a constant temperature of 65° C. for 2.5 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain vinyl diatomaceous earth. 50 g of vinyl diatomaceous earth was added to 800 mL of DMF, and then 7 g of 2-acrylamido-2-methylpropanesulfonic acid and 0.5 g of ammonium persulfate were added, and the mixture was reacted at 85° C. for 3.5 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain the product.
[0082] The method for preparing the porous biochar comprises the following steps:
[0083] S1. Add 75g corn straw powder (100 mesh) into 1000g deionized water, then add 45g urea and 8g hexadecyl ammonium bromide, and perform hydrothermal carbonization reaction at 200°C for 6h. After the reaction is completed, filter, wash and dry. Then, mix 25g of the solid product with 18g potassium hydroxide, and roast it at 700°C in a nitrogen atmosphere for 2.5h. After roasting, add it to a 10wt% nitric acid solution and soak it for 1.5h, then wash and dry it to obtain porous biochar.
[0084] A method for preparing a high-performance waterproof and breathable polyurethane membrane material comprises the following steps:
[0085] The raw materials were weighed according to the above formula, and polyoxypropylene ether diol with a molecular weight of 3000 and ethyl acetate were added into the reactor. Under nitrogen protection, isophorone diisocyanate, UV-9 and dibutyltin dilaurate were added, and the reaction was stirred at 70°C. When the content of NCO groups reached 7%, ethylene glycol, porous biochar, modified diatomaceous earth, silicone polyether defoamer and polyurethane associative thickener were added, and the reaction was continued for 1.5 hours. After the reaction was completed, it was poured onto release paper, and a thin film was scraped out on the surface of the release paper with a scraper, and then dried in a 95°C oven to form a film, so as to obtain the high-performance waterproof and moisture-permeable polyurethane membrane material. Comparative Example 2
[0086] A high-performance waterproof and breathable polyurethane membrane material, comprising the following raw materials:
[0087] 70g of polyoxypropylene ether diol with a molecular weight of 3000, 45g of isophorone diisocyanate, 45g of ethyl acetate, 12g of modified porous biochar, 6g of diatomaceous earth, 8g of ethylene glycol, 2.5g of polyurethane associative thickener, 1.5g of silicone polyether defoamer, 0.15g of UV-9, and 0.08g of dibutyltin dilaurate.
[0088] The method for preparing the modified porous biochar comprises the following steps:
[0089] S1. Add 75 g corn stalk powder (100 mesh) to 1000 g deionized water, then add 45 g urea and 8 g hexadecyl ammonium bromide, and perform hydrothermal carbonization reaction at 200 ° C for 6 h. After the reaction is completed, filter, wash and dry. Then, mix 25 g of the solid product with 18 g of potassium hydroxide, and roast it at 700 ° C in a nitrogen atmosphere for 2.5 h. After the roasting is completed, add it to a 10 wt% nitric acid solution and soak it for 1.5 h, then wash and dry it to obtain porous biochar;
[0090] S2, adding 25g of the porous biochar in step S1 to 500mL of ethanol aqueous solution (the volume ratio of ethanol to water is 8:2), then adding 3g of γ-mercaptopropyltrimethoxysilane, stirring and reacting at 65°C for 1.5h, filtering, washing and drying after the reaction is completed to obtain thiolated porous biochar;
[0091] S3, add 25g of thiolated porous biochar in step S2 to 600mL of DMF, then add 2.2g of 2-(trifluoromethyl)acrylic acid and 0.15g of benzophenone, and 2 , react at 45°C for 25 minutes. After the reaction is completed, filter, wash and dry to obtain modified porous biochar.
[0092] A method for preparing a high-performance waterproof and breathable polyurethane membrane material comprises the following steps:
[0093] The raw materials were weighed according to the above formula, and polyoxypropylene ether diol with a molecular weight of 3000 and ethyl acetate were added into the reactor. Under nitrogen protection, isophorone diisocyanate, UV-9 and dibutyltin dilaurate were added, and the reaction was stirred at 70°C. When the content of NCO groups reached 7%, ethylene glycol, modified porous biochar, diatomaceous earth, silicone polyether defoamer and polyurethane associative thickener were added, and the reaction was continued for 1.5 hours. After the reaction was completed, it was poured onto release paper, and a thin film was scraped out on the surface of the release paper with a scraper, and then dried in a 95°C oven to form a film, so as to obtain the high-performance waterproof and moisture-permeable polyurethane membrane material.
[0094] The high-performance waterproof and breathable polyurethane membrane materials prepared in Examples 1-4 and Comparative Examples 1-2 were subjected to performance tests, wherein the breaking strength and breaking elongation were tested with reference to GB / T 3923.1-2013 "Tensile properties of textile fabrics Part 1: Determination of breaking strength and breaking elongation (strip method)"; the moisture permeability was tested with reference to GB / T 12704.2-2009 "Test method for moisture permeability of textile fabrics Part 2: Evaporation method"; the hydrostatic pressure resistance was tested with reference to GB / T 4744-2013 "Testing and evaluating the waterproof performance of textiles - Hydrostatic pressure method"; the test results are shown in the following Table 1:
[0095] Table 1 Performance test results of different groups of high-performance waterproof and breathable polyurethane membrane materials
[0096]
[0097] It can be seen from Table 1 above that the high-performance waterproof and breathable polyurethane membrane material prepared by the present invention has high mechanical properties, as well as excellent moisture permeability and resistance to hydrostatic pressure, and has good application prospects; in Comparative Example 1, since the porous biochar is not modified, the mechanical properties and waterproofness of the polyurethane membrane material are significantly reduced; in Comparative Example 2, since the diatomaceous earth is not modified, the polyurethane membrane material and moisture permeability are significantly reduced.
[0098] The high-performance waterproof and breathable polyurethane membrane materials prepared in Example 1 and Comparative Examples 1-2 were washed with water at 40° C. for 15 min. After washing 10 times, the hydrostatic pressure resistance thereof was tested again. The test results are shown in Table 2:
[0099] Table 2 Performance of high-performance waterproof and breathable polyurethane membrane material after 10 washes
[0100]
[0101] It can be seen from Table 2 above that the high-performance waterproof and breathable polyurethane membrane material prepared in the present invention has good water washing resistance, and after being washed with water for 10 times, it still has a high resistance to hydrostatic pressure.
[0102] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high-performance waterproof and breathable polyurethane membrane material, characterized in that: By weight, it includes the following raw materials: 60-80 parts of polyether diol, 35-50 parts of diisocyanate, 40-50 parts of organic solvent, 8-14 parts of modified porous biochar, 4-8 parts of modified diatomaceous earth, 5-10 parts of chain extender, 2-3 parts of thickener, 1-2 parts of defoamer, 0.1-0.2 parts of ultraviolet absorber, 0.05-0.1 parts of dibutyltin dilaurate; Wherein, the modified diatomaceous earth is obtained by treating with a silane coupling agent and then grafting with 2-acrylamide-2-methylpropanesulfonic acid; The method for preparing the modified porous biochar comprises the following steps: S1. Add corn stalk powder to deionized water, then add urea and cetyl ammonium bromide to carry out hydrothermal carbonization reaction. After the reaction is completed, filter, wash and dry. Then mix the solid product with potassium hydroxide and roast it in a nitrogen atmosphere. After the roasting is completed, soak it in a nitric acid solution, then wash and dry it to obtain porous biochar; S2, adding the porous biochar prepared in step S1 to an ethanol aqueous solution, and then adding γ-mercaptopropyltrimethoxysilane, stirring to react, and filtering, washing, and drying after the reaction is completed to obtain a thiolated porous biochar; S3, adding DMF to the thiol-modified porous biochar in step S2, and then adding 2-(trifluoromethyl)acrylic acid and benzophenone, and carrying out a thiol-ene reaction under ultraviolet light. After the reaction is completed, filtering, washing, and drying to obtain modified porous biochar; In step S3, the mass ratio of the thiolated porous biochar, 2-(trifluoromethyl)acrylic acid, and benzophenone is 20-30:1.4-2.8:0.1-0.2, and the intensity of the ultraviolet light is 500-600 mW / cm 2 The temperature of the mercapto-ene reaction is 40-50°C and the time is 20-30 minutes.
2. The high-performance waterproof and breathable polyurethane membrane material according to claim 1, characterized in that: The polyether diol is a polypropylene oxide ether diol with a molecular weight of 3000-4000; the diisocyanate is one or more of isophorone diisocyanate, dicyclohexylmethane diisocyanate, and hexamethylene diisocyanate; the chain extender is one or more of ethylene glycol, 1,3-propylene glycol, and ethylenediamine; the thickener is a polyurethane associative thickener; the ultraviolet absorber is one or more of UV-9, UV-531, and UVP-327; and the defoamer is a silicone defoamer.
3. The high-performance waterproof and breathable polyurethane membrane material according to claim 1, characterized in that: The specific preparation method of the modified diatomite is as follows: The diatomaceous earth is added to a sodium hydroxide solution with a mass fraction of 10%, and stirred and impregnated. After the stirring and impregnation, the solution is filtered, dried, and calcined to obtain pretreated diatomaceous earth. The pretreated diatomaceous earth is added to an ethanol aqueous solution, and then vinyl triethoxysilane is added to react at a constant temperature. After the reaction is completed, the solution is filtered, washed, and dried to obtain vinyl diatomaceous earth. The vinyl diatomaceous earth is added to DMF, and then 2-acrylamido-2-methylpropanesulfonic acid and ammonium persulfate are added to react by heating. After the reaction is completed, the solution is filtered, washed, and dried to obtain the product.
4. The high-performance waterproof and breathable polyurethane membrane material according to claim 3, characterized in that: The stirring and impregnation temperature is 40-50°C and the time is 1-2h, the calcination temperature is 350-450°C and the time is 1-2h; the mass ratio of the pretreated diatomaceous earth and vinyl triethoxysilane is 50:5-9, the constant temperature reaction temperature is 60-70°C and the time is 2-3h; the ratio of the vinyl diatomaceous earth, 2-acrylamido-2-methylpropane sulfonic acid and ammonium persulfate is 50:5-9:0.3-0.6, the heating reaction temperature is 80-90°C and the time is 3-4h.
5. The high-performance waterproof and breathable polyurethane membrane material according to claim 1, characterized in that: In step S1, the mass ratio of corn stalk powder, deionized water, urea and hexadecyl ammonium bromide is 70-80:1000:40-50:5-10, the temperature of the hydrothermal carbonization reaction is 180-220°C, and the time is 4-7h; the mass ratio of the solid product and potassium hydroxide is 20-30:15-20, the roasting temperature is 650-750°C, and the time is 2-3h.
6. The high-performance waterproof and breathable polyurethane membrane material according to claim 1, characterized in that: In step S2, the mass ratio of the porous biochar to γ-mercaptopropyltrimethoxysilane is 20-30:2-4, the stirring reaction temperature is 60-70° C., and the time is 1-2 h.
7. A method for preparing a high-performance waterproof and breathable polyurethane membrane material according to any one of claims 1 to 6, characterized in that: The following steps are involved: Add polyether diol and organic solvent into a reactor, add diisocyanate, ultraviolet absorber and dibutyltin dilaurate under nitrogen protection, and stir to react at 65-75°C. When the content of NCO group reaches 7%, add chain extender, modified porous biochar, modified diatomaceous earth, defoamer and thickener, and continue to react for 1-2 hours. After the reaction is completed, pour it onto release paper, use a scraper to scrape out a thin film on the surface of the release paper, and then dry it in a 90-100°C oven to form a film, so as to obtain the high-performance waterproof and moisture-permeable polyurethane membrane material.
8. Use of the high-performance waterproof and breathable polyurethane membrane material according to any one of claims 1 to 6 in textiles.