A simulation method for particle movement and interaction behavior in a continuous casting mold
Through multi-physics-multi-phase flow simulation and UDF program calculation, the problem of simulating the motion behavior of argon bubbles and inclusions in the continuous casting mold was solved, achieving more accurate simulation of the distribution of argon bubbles and inclusions, and guiding the continuous casting process. optimization and equipment design.
Patent Information
- Application Number
- CN202411126533.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-16
AI Technical Summary
Existing technology cannot effectively simulate the motion behavior and interaction of argon bubbles and inclusions in the continuous casting mold, especially during the capture process of the solidification front. The calculation is difficult and the removal rate has errors.
A three-dimensional model is established using software such as Spaceclaim and ANSYS Fluent. Through multi-physics-multiphase flow simulation, the motion of argon bubbles and inclusions under the action of electromagnetic braking is considered, and the UDF program is used to compile and calculate the collision behavior of argon bubbles and inclusions. Improve calculation accuracy and efficiency.
The simulation results are more consistent with the actual process, can accurately describe the distribution of argon bubbles and inclusions, provide precise control of key process parameters and equipment optimization guidance, and improve the production efficiency of continuous casting equipment.
Smart Images

Figure CN118657039B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of iron and steel metallurgical process simulation, and in particular relates to a simulation method for particle movement and interaction behavior in a continuous casting crystallizer. Background Art
[0002] The crystallizer is the core equipment of the continuous casting process of steel, and it undertakes the important function of solidifying the molten steel into a billet shell. There are complex physical and chemical phenomena such as turbulent flow, heat transfer, solute diffusion and discrete phase particle movement inside the continuous casting crystallizer. It is a complex system in a multi-physical field-multiphase flow coupling state. In order to avoid nodule blockage at the nozzle and improve the cleanliness of the molten steel, argon is usually blown at the submerged nozzle of the crystallizer to prevent inclusions from accumulating on the nozzle wall and promote the floating and removal of inclusion particles in the crystallizer. Therefore, it is crucial to analyze the instantaneous motion, interaction and capture behavior of discrete phase particles such as argon bubbles and inclusions in the crystallizer steel liquid at the solidification front to improve the cleanliness of the molten steel and enhance production stability.
[0003] Due to the limitation of high temperature conditions in the crystallizer, it is very difficult to directly observe the movement behavior of argon bubbles and inclusions at the industrial site. Therefore, numerical simulation research has become an effective method to study the movement behavior and interaction between the two. Based on numerical simulation technology, researchers proposed a method to calculate the collision behavior of argon bubbles and inclusions, and analyzed the removal effect in specific metallurgical reactors. For example, the article Numerical investigation on particles removal by bubble flotation in swirling flow (Cui H, Li T, Zhu Y, et al. Numerical investigation on particles removal by bubble flotation in swirling flow [J]. Journal of Iron and Steel Research International, 2022, 29 (6): 961-972.) proposed a method to calculate the collision behavior of argon bubbles and inclusions based on their position, movement speed and time step. By analyzing the position of each argon bubble and inclusion after the end of the time step in the simulation calculation, it is determined whether the two collide. The articles Numerical Simulation of Inclusion Removal by Bubble Injection inthe Submerged Nozzle With Swirling Flow (Xin Z, Cui H, Li T, et al. Metallurgical and Materials Transactions B, 2022, 53(4): 2570-2586.) and Simulation of Inclusion Removal in Bottom-blowing Ladle with Tracking the Collision of Inclusions and Bubbles in Transient Time Steps (Liu K, Zhang L, Cui H, et al. ISIJ International, 2023, 63(10): 1677-1686.) respectively studied the effects of argon blowing processes in continuous casting tundish and ladle on inclusion removal based on this method.
[0004] However, the above method is not suitable for studying the movement behavior and interaction between argon bubbles and inclusions in the continuous casting crystallizer. First, the existing method only considers the interaction between argon bubbles and inclusions and their removal at the slag interface, without considering their capture process at the solidification front of the crystallizer; second, the existing method needs to traverse and solve the positions and velocities of a large number of argon bubbles and inclusions when determining the collision between argon bubbles and inclusions, which is difficult to calculate and time-consuming to solve; finally, the existing method makes collision judgments based on the positions of argon bubbles and inclusions at the end of each time step, ignoring the possible collision behavior between the two in a single time step, resulting in errors in the final removal rate. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the present invention provides a simulation method for the movement and interaction behavior of particles in a continuous casting crystallizer, aiming to solve the technical problems that the prior method cannot solve the capture behavior of discrete phase particles such as argon bubbles and inclusions in the molten steel in the crystallizer at the solidification front, and the calculation of the collision between argon bubbles and inclusions takes a long time and has low accuracy.
[0006] In order to achieve the above technical objectives, the present invention provides the following technical solutions:
[0007] A method for simulating particle movement and interaction behavior in a continuous casting crystallizer comprises the following steps:
[0008] S1: Obtain the geometric structure parameters of the continuous casting mold in actual production, and use Spaceclaim 3D modeling software to establish a 3D geometric model of the continuous casting mold;
[0009] S2: The three-dimensional geometric model of the continuous casting crystallizer is extracted by using Spaceclaim three-dimensional modeling software, and structured meshing is performed by using ICEM software to obtain a mesh model of the fluid domain of the molten steel in the crystallizer;
[0010] S3: importing the mesh model of the molten steel flow domain in the crystallizer into ANSYS Fluent simulation software, selecting a calculation model and a solution algorithm, defining physical parameters and boundary conditions, performing an initialization operation and then performing an iterative solution to obtain the molten steel flow field, temperature field and solidified shell distribution in the crystallizer under electromagnetic braking;
[0011] S4: Establish the injection points of argon bubbles and inclusions in the crystallizer, call the UDF program to compile and calculate the floating removal behavior of argon bubbles and inclusions at the slag interface, the capture behavior of argon bubbles and inclusions at the solidification front, and the collision and aggregation behavior of argon bubbles and inclusions, and obtain the movement behavior of argon bubbles and inclusions in the crystallizer;
[0012] S5: coupling calculation is performed on the flow field, temperature field and solidified shell distribution of the molten steel in the crystallizer under the electromagnetic braking effect obtained in step S3 and the movement behavior of the argon bubbles and inclusions in the crystallizer obtained in step S4, and solving the crystallizer multi-physics field-multiphase flow simulation result considering the electromagnetic braking effect and the collision and aggregation behavior of the argon bubbles and inclusions;
[0013] S6: Post-processing the crystallizer multi-physics field-multiphase flow simulation results considering the electromagnetic braking effect and the argon bubble-inclusion collision aggregation behavior to obtain the simulation results of the flow field, temperature field, solidified shell distribution and discrete phase movement behavior in the crystallizer at different times.
[0014] Furthermore, in step S1, the geometrical parameters of the continuous casting crystallizer include the width, height and thickness of the crystallizer, as well as the diameter of the submerged nozzle, the outlet height, the outlet width and the outlet position.
[0015] Furthermore, in step S2, during the process of extracting the fluid domain volume and performing structured meshing on the three-dimensional geometric model of the continuous casting crystallizer, a local boundary layer mesh encryption operation is performed on the area near the fluid domain wall to accurately calculate the growth of the solidified shell.
[0016] The encryption operation is specifically as follows: using a hexahedral structured grid to divide the area near the wall of the fluid domain, adding grid nodes to the range of 10-15 mm from the wall of the calculation domain, the thickness of the encrypted grid is in the range of 0.5-1.5 mm, the overall grid quality is in the range of 0.6-1.0, the maximum aspect ratio of a single grid is less than 10, and the total number of grids is greater than 1 million.
[0017] Furthermore, step S3 specifically includes:
[0018] S31: Select calculation model and solution algorithm:
[0019] In ANSYS Fluent software, the large eddy simulation model (LES) is selected to solve the turbulent motion of the molten steel in the crystallizer, the volume of fluid (VOF) model is selected to solve the wave behavior of the molten steel-molding slag interface, the energy conservation equation is enabled to solve the heat transfer behavior of the molten steel in the crystallizer, the solidification and melting model (Solidification and MeltingModel) is selected to solve the solidification and melting behavior of the molten steel and define the movement speed of the billet shell according to the pulling speed, and the magnetohydrodynamics (MHD) model is selected to solve the influence of the electromagnetic field on the flow behavior of the molten steel;
[0020] The coupled algorithm is used for pressure-velocity coupling, the PRESTO algorithm is used for spatial discretization of pressure, the bounded central difference algorithm is used for spatial discretization of momentum, the energy equation and the magnetohydrodynamic equation are discretized by the second-order upwind and first-order upwind schemes respectively; the bounded second-order implicit transient formula is used for solution to ensure the stability of calculation;
[0021] Among them, the PRESTO! algorithm (PREssure STaggering Option, PRESTO!) is a staggered pressure algorithm used to discretize the pressure term so that the pressure can better satisfy the momentum equation and the continuity equation at the same time; the PRESTO! algorithm is a regular option in the Fluent software and is a conventional technology.
[0022] S32: Define physical properties and boundary conditions: Set the density, viscosity, thermal conductivity, specific heat, latent heat, liquidus temperature, solidus temperature, electrical conductivity and magnetic permeability parameters of molten steel and mold slag in ANSYS Fluent software, and set the density of argon bubbles and inclusions;
[0023] The inlet of the submerged nozzle is set as the velocity inlet boundary condition. The specific inlet velocity value is calculated in combination with the drawing speed and the cross-sectional size. The inlet temperature value is set as the pouring temperature of the molten steel, and the discrete phase boundary condition type at the inlet is set as rebound; the top surface of the crystallizer is set as the adiabatic slip wall boundary condition, and the discrete phase boundary condition type of the top surface of the crystallizer is set as escape; the bottom surface of the crystallizer is set as the fluid outflow boundary condition, and the discrete phase boundary condition type of the bottom surface of the crystallizer is set as escape; the side wall of the crystallizer is set as the no-slip wall boundary condition, and the heat transfer type is convection heat transfer. The convection heat transfer coefficient is determined according to the empirical formula of the heat flux density of the continuous casting crystallizer, and the formula is as follows:
[0024] ;
[0025] Where h is the convection heat transfer coefficient of the side wall of the crystallizer, A and B are both empirical constants calculated based on the water volume of the crystallizer. A can take the empirical value of 2680000, and B can take the empirical value of 355000. y is the coordinate of the billet drawing direction, v is the billet drawing speed, T and T ref They are wall temperature and reference temperature respectively. The reference temperature is the ambient temperature of the crystallizer. The discrete phase boundary condition type of the crystallizer side wall is set to escape.
[0026] S33: After initializing the flow field and temperature field in the calculation domain, set the solution parameters and perform iterative solution.
[0027] Further, in step S32, the inlet velocity value is calculated in combination with the pulling speed and the cross-sectional dimensions, specifically:
[0028] Inlet velocity = (pulling speed × cross-sectional area of crystallizer) / water inlet area.
[0029] Furthermore, step S4 specifically includes the following steps:
[0030] S41: Get the inclusion radius R p , the injection points of argon bubbles and inclusions are established through the surface injection function in ANSYS Fluent, the submerged nozzle inlet is selected as the injection point, and the size of the argon bubbles and inclusions is set; the radius R of the argon bubble b 1~5×10 -3 m;
[0031] S42: calling the DEFINE_DPM_SCALAR_UPDATE macro through the UDF program to calculate the floating removal behavior of argon bubbles and inclusions at the steel-slag interface and the capture behavior of argon bubbles and inclusions at the solidification front. When the argon bubbles or inclusions move to the point where the volume fraction of the protective slag phase or the solid phase ratio reaches the separation condition, the corresponding argon bubbles or inclusion particles are removed from the calculation domain, thus obtaining the first remaining argon bubbles and the first remaining inclusions.
[0032] S43: Calculate the collision aggregation behavior of the first remaining argon bubble and the first remaining inclusion obtained in step S42 by calling the EXECUTE_AT_END macro, and obtain the position coordinate x of the first remaining argon bubble in the calculation domain at the current moment. b ,y b 、z b And the velocity components v in each direction b,x 、v b,y 、v b,z , the position coordinate x of the first remaining inclusion p ,y p 、z p and the velocity components v in each direction p,x 、v p,y 、v p,z , and set the calculation time step t, and calculate the potential collision zone radius R based on the speed of the first remaining argon bubble in each direction and the time step c , as shown below:
[0033] ;
[0034] The inclusion particles whose distance from the argon bubble is less than Rc are defined as the first potential collision inclusions;
[0035] S44: calculating the velocity angle θ between all the first remaining argon bubbles and the first potential collision inclusions according to the vector synthesis method, screening out the first potential collision inclusions whose angles with the first remaining argon bubbles are within the collisionable angle range, and defining them as second potential collision inclusions;
[0036] S45: Divide the time step t into n equal parts, and calculate the position coordinates of the first remaining argon bubble and the second potential collision inclusion in the i-th state (1≤i≤n) within t seconds according to the position coordinates and velocities in each direction of the first remaining argon bubble and the second potential collision inclusion. The calculation formula is as follows:
[0037] ;
[0038] ;
[0039] ;
[0040] ;
[0041] ;
[0042] ;
[0043] Among them, x b,(i / n)t ,y b,(i / n)t and z b,(i / n)t are the position coordinates of the first remaining argon bubble in the i-th state within t seconds, x p,(i / n)t ,y p,(i / n)t and z p,(i / n)t are the position coordinates of the second potential collision inclusion in the i-th state within t seconds respectively;
[0044] S46: Calculate the spherical center distance D between the first remaining argon bubble and the second potential collision inclusion at the i-th state, i.e., at the time i / n, according to the position coordinates of each argon bubble and the inclusion obtained in step S46. i As shown below:
[0045]
[0046] Define the distance D between the sphere center of the inclusion and the argon bubble i Less than the sum of the two radii (R b +R p ), the corresponding inclusions collide with the bubbles, which are the inclusions to be removed. The inclusions to be removed are removed from the first remaining inclusions to obtain second remaining inclusions. The second remaining inclusions and the first remaining argon bubbles have motion behavior, that is, the motion behavior of argon bubbles and inclusions in the crystallizer is obtained.
[0047] Furthermore, the specific method for obtaining the inclusion radius Rp in step 41 is: sampling the ingot and measuring the inclusion size by electron microscope observation; the radius Rp of the argon bubble b 1~5×10 -3 m. R b The size range of bubbles can be obtained through water model physical experimental tests and reference literature data, which is a conventional technique.
[0048] Furthermore, the separation condition in step S42 is specifically: the volume fraction of the mold slag phase f slag ≥0.5 or solid phase ratio f solid ≥ 0.7.
[0049] Further, in step S44, the collisionable angle range is -90 to 90 degrees.
[0050] The beneficial effects of the present invention are:
[0051] The present invention provides a simulation method for particle movement and interaction behavior in a continuous casting crystallizer. By considering the capture behavior of argon bubbles and inclusions in the crystallizer at the slag interface and the solidification front and the argon bubble-inclusion collision behavior, the movement behavior of argon bubbles and inclusions in molten steel during the continuous casting process is simulated. The obtained distribution of argon bubbles and inclusions is more consistent with the actual continuous casting process, and the influence of key process parameters such as submerged nozzle structure, casting speed, and electromagnetic braking parameters on the movement and distribution of discrete phase particles in the crystallizer can be obtained. The obtained results have important guiding significance for the precise regulation of actual continuous casting parameters, the design optimization of continuous casting equipment, and the quality and efficiency improvement of continuous casting production lines. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1a Schematic diagram of the crystallizer geometry model established in the embodiment of the present invention.
[0053] Figure 1b Schematic diagram of a structured grid divided in an embodiment of the present invention.
[0054] Figure 1c It is a local schematic diagram of a structured grid divided in an embodiment of the present invention.
[0055] Figure 2 Schematic diagram of the position and collision state of argon bubbles and inclusions at each intermediate time after the time step is divided into four equal parts in an embodiment of the present invention.
[0056] Figure 3 The figure is a schematic diagram of the number of inclusions and the sampling positions of the ingot involved in verifying the simulation calculation results based on the electrolysis experiment in the embodiment of the present invention.
[0057] Figure 4This is a comparison diagram of inclusion contents at different positions along the width direction of the ingot obtained through simulation calculation and electrolysis experiment under the working conditions described in the embodiment of the present invention;
[0058] Figure 5 Schematic diagram of the angle between the first remaining argon bubble and the first potential collision inclusion. DETAILED DESCRIPTION
[0059] The technical solution of the present invention is further described below in conjunction with specific embodiments and drawings.
[0060] This embodiment provides a method for simulating particle movement and interaction behavior in a continuous casting crystallizer, which specifically includes the following steps:
[0061] S1: Based on the thin slab continuous casting crystallizer and its matching porous immersion nozzle provided by a steel plant, the geometric model of the crystallizer and the nozzle was constructed using ANSYS Spaceclaim 3D modeling software, such as Figure 1a As shown, the width of the crystallizer is 1250 mm, the thickness is 110 mm, and the height is 1200 mm. The upper part of the submerged nozzle is cylindrical, the inlet diameter is 125 mm, and the bottom is flat. It is divided into a wide nozzle surface and a narrow nozzle surface. There are four outlets in total, of which two lateral outlets are located on the narrow surfaces on both sides of the nozzle, 20 mm away from the bottom surface of the nozzle, and 30 mm away from the wide surfaces on both sides of the nozzle. The outlet surface is rectangular, 80 mm long, and 50 mm wide. The two main outlets are located on the bottom surface of the nozzle, 55 mm away from the narrow surfaces on both sides of the nozzle, and 30 mm away from the wide surfaces on both sides of the nozzle. The outlet surface is rectangular, 120 mm long, and 50 mm wide. It is saved as a .scdoc format file;
[0062] S2: Use Spaceclaim software to extract the computational domain for solving the flow of molten steel in the crystallizer and nozzle based on Boolean operations, and import the extracted computational domain into the ICEM meshing software. First, define and name each boundary surface, then associate Vertex, Edge and Face and divide Block. When dividing the mesh, add mesh nodes within 15 mm of the computational domain from the wall, and perform local boundary layer mesh encryption to accurately calculate the growth of the solidified shell. The mesh thickness of the encrypted area is 0.5 mm, the overall mesh quality is higher than 0.6, the maximum aspect ratio of a single mesh is less than 10, the total number of meshes is 1.3 million, and it is exported as an .msh format file, such as Figure 1b and Figure 1c As shown;
[0063] S3: Import the exported .msh format crystallizer mesh file into ANSYS Fluent and perform solution settings;
[0064] According to the specific flow of molten steel in the crystallizer, the LES turbulence model is selected in ANSYS Fluent software to solve the turbulent motion of molten steel in the crystallizer, the VOF model is selected to solve the wave behavior of the molten steel-molding slag interface, the energy conservation equation is enabled to solve the heat transfer behavior of molten steel in the crystallizer, the Solidification and Melting model is selected to solve the solidification and melting behavior of molten steel and the shell movement speed is set to 0.1 m / s according to the pulling speed, and the MHD model is selected to solve the influence of electromagnetic field on the flow behavior of molten steel. The Coupled algorithm is used for pressure-velocity coupling, the PRESTO! algorithm is used to spatially discretize the pressure, the Bounded Central Differencing algorithm is used to spatially discretize the momentum, and the energy equation and MHD equation are discretized using the second-order upwind and first-order upwind schemes respectively. In addition, the Bounded Second Order Implicit transient formula is used to solve to ensure the stability of the calculation.
[0065] The physical properties of the continuous phase molten steel, protective slag, discrete phase argon bubbles, and inclusions are set in ANSYS Fluent software. The molten steel is the main phase of the continuous phase, and its density is 7020 kg / m 3 , viscosity is 0.0053 Pa·s, thermal conductivity is 27 W / (m·K), specific heat capacity is 720 J / (kg·K), latent heat of solidification is 275000 J / kg, liquidus temperature is 1794 K, solidus temperature is 1749 K, electrical conductivity is 714000 S / m, magnetic permeability is 1.257×10 -6 H / m; the mold slag is a continuous phase and a secondary phase, with a density of 3000kg / m 3 , viscosity is 0.259 Pa·s, thermal conductivity is 2W / (m·K), specific heat capacity is 830 J / (kg·K), liquidus temperature is 1573K, solidus temperature is 1352 K, electrical conductivity is 714000 S / m, magnetic permeability is 1.257×10 -6 H / m; Argon bubbles are discrete phases with a density of 1.6228 kg / m 3 ; The inclusions are discrete phases with a density of 2700 kg / m 3 .
[0066] The boundary conditions were set in ANSYS Fluent software. The inlet of the submerged nozzle was set as the velocity inlet boundary condition. The inlet velocity was calculated to be 1.0852 m / s based on the actual velocity value of 6 m / min. The inlet molten steel temperature was 1826 K based on the actual pouring temperature. The discrete phase boundary condition type at the inlet was set to Reflect. The top surface of the crystallizer was set to the adiabatic slip wall boundary condition, and the discrete phase boundary condition type of the top surface of the crystallizer was set to Escape. The bottom surface of the crystallizer was set to the Outflow boundary condition, and the discrete phase boundary condition type of the bottom surface of the crystallizer was set to Escape. The side wall of the crystallizer was set to the no-slip wall boundary condition, and the heat transfer type was convection heat transfer. The convection heat transfer coefficient was determined according to the empirical formula of the heat flux density of the continuous casting crystallizer, as follows:
[0067]
[0068] Where h is the side wall convection heat transfer coefficient, A and B are both empirical constants calculated based on the amount of water in the crystallizer, A is 2680000, B is 355000, y is the coordinate in the direction of billet drawing, v is the billet drawing speed, which is 6 m / min, T and T ref are the wall temperature and reference temperature respectively. The reference temperature is the ambient temperature of the crystallizer, which is set to 300 K.
[0069] After initializing the flow field and temperature field of the computational domain, the solution parameters are set. The initial velocity of the computational domain is set to 0 m / s, the initial temperature is set to 1826 K, and the solution time step t is set to 1×10 -3 s, iterate 200 steps in each time step for iterative calculation;
[0070] S4: The radius R of the inclusion is obtained by sampling during the actual pouring process through electron microscope experimental measurement p 2.5×10 -5 m, and the immersion nozzle inlet is used as the injection point of argon bubbles and inclusions through the surface injection function in the DPM model of ANSYS Fluent software. The radius of the argon bubble is obtained as R based on the actual casting process. b 1×10 -3 m;
[0071] The DEFINE_DPM_SCALAR_UPDATE macro is called through the UDF program to calculate the floating removal behavior of argon bubbles and inclusions at the slag interface and the capture behavior at the solidification front. It is set that when the argon bubbles or inclusions move to the volume fraction f of the protective slag phase slag Greater than 0.5 or solid fraction f solidWhen the area is greater than 0.7, the corresponding argon bubbles or inclusion particles are removed from the calculation domain to obtain the first remaining argon bubbles and the first remaining inclusions;
[0072] By calling the EXECUTE_AT_END macro, the collision aggregation behavior of the argon bubble and the inclusion is calculated, and the position coordinate x of the first remaining argon bubble in the calculation domain is obtained. b ,y b 、z b , velocity components v in each direction b,x 、v b,y 、v b,z , the position coordinate x of the first remaining inclusion p ,y p 、z p and the velocity components v in each direction p,x 、v p,y 、v p,z , and set the calculation time step t=1×10 -3 s, the radius Rc of the potential collision zone is calculated based on the velocities of the first remaining argon bubble in each direction and the time step, as shown in the following formula:
[0073] ;
[0074] The inclusion particles whose distance from the argon bubble is less than Rc are defined as the first potential collision inclusions;
[0075] According to the vector synthesis method, such as Figure 5 As shown, the velocity v of the first remaining argon bubble b Taking the direction of as a reference, calculate the velocity angle θ between all the first remaining argon bubbles and the first potential collision inclusions, screen out the first potential collision inclusions whose angles with the first remaining argon bubbles are within the collisionable angle range, and define them as the second potential collision inclusions;
[0076] Specifically, in the present invention, the velocity V of the first remaining argon bubbles is defined as b The direction is 0°, the angle is positive when rotating in the clockwise direction, and negative when rotating in the counterclockwise direction;
[0077] In this embodiment, the first potential collision inclusion ( Figure 5 In, V p is the velocity of the first potential collision inclusion), defined as the second potential collision inclusion.
[0078] Set the time step t = 1 × 10 -3s is divided into 4 parts, and according to the position coordinates of the first remaining argon bubble and the second potential collision inclusion and the velocity in each direction, the position coordinates of the argon bubble and the inclusion in the i-th (1≤i≤4) state within the time step are calculated, as follows: Figure 2 The calculation formula is shown below:
[0079] (1)
[0080] (2)
[0081] (3)
[0082] (4)
[0083] (5)
[0084] (6)
[0085] According to the above calculation, the 0.25×10 -3 s, 0.5×10 -3 s, 0.75×10 -3 s and 1×10 -3 The position coordinates of each argon bubble and inclusion at time s are calculated in sequence according to equations (7) to (10) at the 0.25×10 -3 s, 0.5×10 -3 s, 0.75×10 -3 s and 1×10 -3 The distances between the sphere centers of each inclusion and the argon bubble at time s are D1, D2, D3 and D4. After the calculation is completed, the distances between the sphere centers D1, D2, D3 and D4 are compared with the sum of the radii of the two. If any one of D1, D2, D3 and D4 is less than 2.05×10 -3 m, it is considered that the inclusion collides with the bubble, so it is removed from the calculation domain, and the inclusion to be removed is removed from the first remaining inclusion to obtain the second remaining inclusion, and the second remaining inclusion and the first remaining argon bubble have motion behavior.
[0086] (7)
[0087] (8)
[0088] (9)
[0089] (10)
[0090] S5: coupling calculation is performed on the flow field, temperature field and solidified shell distribution of the molten steel in the crystallizer under the electromagnetic braking obtained in step S3 and the motion behavior of the argon bubbles and inclusions with motion behavior in the crystallizer obtained in step S4, and the calculation results are saved at every 0.1 s time interval and exported to .cas and .dat format files;
[0091] S6: Import the .cas and .dat format files exported from S5 into the post-processing software Tecplot for post-processing operations, extract the central section of the wide surface of the crystallizer, and extract the positions of the discrete phase argon bubbles and inclusions under collision conditions, obtain the flow field, temperature field and distribution of discrete phase argon bubbles and inclusions in the crystallizer under electromagnetic braking and argon blowing conditions at 10 s, 20 s, 30 s, 40 s, and 50 s, and export the post-processing results in .tif format.
[0092] After the calculation is completed, the calculation results of 50 s are taken, and the outlet surface of the crystallizer is used as the bottom surface. 50 mm × 50 mm × 50 mm cubic areas are delineated at the center position, 1 / 4 position and edge position of the outlet surface respectively. The UDF program is called to count the number of inclusions falling within the above three statistical areas according to the coordinate data of the second residual inclusions, and the proportion of inclusions at each position is calculated. The statistical results are as follows: Figure 4 Dashed line - calculated value.
[0093] Verification experiment
[0094] Under the same working conditions as those in the specific embodiment of the present invention, molten steel is poured to obtain a cast billet. Samples of 50 mm×50 mm×50 mm are taken at the center, 1 / 4 and narrow surface of the billet according to the above statistical range for large sample electrolysis experiments. The electrolyzed inclusions are cleaned and weighed, and the weight proportion of the inclusions at each position is calculated, such as Figure 3 Solid line part - experimental value.
[0095] according to Figure 3 Comparison of the calculated values with the experimental values shows that the statistical deviation between the calculated values and the experimental values is within 5%, which indicates that the technical solution of the present invention can well simulate the collision behavior of bubbles and inclusions in the crystallizer.
[0096] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. For ordinary technicians in this field, they can still modify or transform the technical solutions described above, which all fall within the scope of protection of the present invention.
Claims
1. A simulation method for particle movement and interaction behavior in a continuous casting mold. It is characterized in that The following steps are involved: S1: Obtain the geometric structure parameters of the continuous casting mold in actual production and establish a three-dimensional geometric model of the continuous casting mold; S2: extracting the fluid domain volume and performing structured meshing on the three-dimensional geometric model of the continuous casting mold to obtain a mesh model of the fluid domain of the molten steel in the mold; S3: importing the grid model of the molten steel flow domain in the crystallizer into the simulation software, selecting the calculation model and the solution algorithm, defining the physical parameters and boundary conditions, performing an initialization operation and then performing an iterative solution to obtain the molten steel flow field, temperature field and solidified shell distribution in the crystallizer under the action of electromagnetic braking; S4: Establish the injection points of argon bubbles and inclusions in the crystallizer, compile and calculate the floating removal behavior of argon bubbles and inclusions at the slag interface, the capture behavior of argon bubbles and inclusions at the solidification front, and the collision and aggregation behavior of argon bubbles and inclusions, and obtain the movement behavior of argon bubbles and inclusions in the crystallizer; S5: coupling calculation is performed on the flow field, temperature field and solidified shell distribution of the molten steel in the crystallizer under the electromagnetic braking effect obtained in step S3 and the movement behavior of the argon bubbles and inclusions in the crystallizer obtained in step S4, and solving the crystallizer multi-physics field-multiphase flow simulation result considering the electromagnetic braking effect and the collision and aggregation behavior of the argon bubbles and inclusions; S6: Post-processing the crystallizer multi-physics field-multiphase flow simulation results considering the electromagnetic braking effect and the argon bubble-inclusion collision aggregation behavior to obtain the simulation results of the flow field, temperature field, solidified shell distribution and discrete phase movement behavior in the crystallizer at different times.
2. A method for simulating particle movement and interaction behavior in a continuous casting crystallizer as claimed in claim 1, It is characterized in that In step S1, the geometrical parameters of the continuous casting crystallizer include the width, height and thickness of the crystallizer, as well as the diameter of the submerged nozzle, the outlet height, the outlet width and the outlet position.
3. A method for simulating particle movement and interaction behavior in a continuous casting mold as claimed in claim 1, It is characterized in that In step S2, during the process of extracting the fluid domain volume and performing structured meshing on the three-dimensional geometric model of the continuous casting crystallizer, a local boundary layer mesh encryption operation is performed on the area near the fluid domain wall to accurately calculate the growth of the solidified shell.
4. A method for simulating particle movement and interaction behavior in a continuous casting crystallizer as claimed in claim 1, It is characterized in that Step S3 specifically includes: S31: Select the calculation model and solution algorithm: Select the large eddy simulation model to solve the turbulent motion of the molten steel in the crystallizer, select the fluid volume method model to solve the wave behavior of the molten steel-molten slag interface, enable the energy conservation equation to solve the heat transfer behavior of the molten steel in the crystallizer, select the solidification and melting model to solve the solidification and melting behavior of the molten steel and define the movement speed of the billet shell according to the pulling speed, and select the magnetohydrodynamic model to solve the influence of the electromagnetic field on the flow behavior of the molten steel; A coupling algorithm is used for pressure-velocity coupling, an interleaved pressure algorithm is used for spatial discretization of pressure, a bounded central difference format algorithm is used for spatial discretization of momentum, and the energy equation and magnetohydrodynamic equation are discretized using second-order upwind and first-order upwind formats respectively; a bounded second-order implicit transient formula is used for solution to ensure the stability of the calculation; S32: Define physical property parameters and boundary conditions: set the density, viscosity, thermal conductivity, specific heat, latent heat, liquidus temperature, solidus temperature, electrical conductivity and magnetic permeability parameters of molten steel and mold slag, and set the density of argon bubbles and inclusions; The inlet of the submerged nozzle is set as the velocity inlet boundary condition. The specific inlet velocity value is calculated in combination with the drawing speed and the cross-sectional size. The inlet temperature value is set as the pouring temperature of the molten steel, and the discrete phase boundary condition type at the inlet is set as rebound; the top surface of the crystallizer is set as the adiabatic slip wall boundary condition, and the discrete phase boundary condition type of the top surface of the crystallizer is set as escape; the bottom surface of the crystallizer is set as the fluid outflow boundary condition, and the discrete phase boundary condition type of the bottom surface of the crystallizer is set as escape; the side wall of the crystallizer is set as the no-slip wall boundary condition, and the heat transfer type is convection heat transfer. The convection heat transfer coefficient is determined according to the empirical formula of the heat flux density of the continuous casting crystallizer, and the formula is as follows: ; Where h is the convection heat transfer coefficient of the side wall of the crystallizer, A and B are empirical constants calculated based on the water volume in the crystallizer, y is the coordinate of the casting direction, v is the casting speed, T and T ref They are wall temperature and reference temperature respectively. The reference temperature is the ambient temperature of the crystallizer. The discrete phase boundary condition type of the crystallizer side wall is set to escape. S33: After initializing the flow field and temperature field in the calculation domain, set the solution parameters and perform iterative solution.
5. A method for simulating particle movement and interaction behavior in a continuous casting mold as claimed in claim 4, It is characterized in that In step S32, the inlet velocity value is calculated by combining the pulling speed and the cross-sectional dimensions, specifically: Inlet velocity = (pulling speed × cross-sectional area of crystallizer) / water inlet area.
6. A method for simulating particle movement and interaction behavior in a continuous casting mold as claimed in claim 1, It is characterized in that Step S4 specifically includes the following steps: S41: Get the inclusion radius R p , establish the injection point of argon bubbles and inclusions, select the submerged nozzle inlet as the injection point, and set the size of argon bubbles and inclusions; S42: Calculate the floating removal behavior of argon bubbles and inclusions at the slag interface and the capture behavior of argon bubbles and inclusions at the solidification front. When the argon bubbles or inclusions move to the point where the volume fraction of the protective slag phase or the solid phase ratio reaches the separation condition, remove the corresponding argon bubbles or inclusion particles from the calculation domain, and obtain the first residual argon bubbles and the first residual inclusions. S43: Calculate the collision and aggregation behaviors of the first remaining argon bubble and the first remaining inclusion obtained in step S42, and obtain the position coordinate x of the first remaining argon bubble in the calculation domain at the current moment. b ,y b 、z b And the velocity components v in each direction b,x 、v b,y 、v b,z , the position coordinate x of the first remaining inclusion p ,y p 、z p and the velocity components v in each direction p,x 、v p,y 、v p,z , and set the calculation time step t, and calculate the potential collision zone radius R based on the speed of the first remaining argon bubble in each direction and the time step c , as shown below: ; The inclusion particles whose distance from the argon bubble is less than Rc are defined as the first potential collision inclusions; S44: calculating the velocity angle θ between all the first remaining argon bubbles and the first potential collision inclusions according to the vector synthesis method, screening out the first potential collision inclusions whose angles with the first remaining argon bubbles are within the collisionable angle range, and defining them as second potential collision inclusions; S45: Divide the time step t into n equal parts, and calculate the position coordinates of the first remaining argon bubble and the second potential collision inclusion in the i-th state within t seconds according to the position coordinates and velocities in each direction of the first remaining argon bubble and the second potential collision inclusion, 1≤i≤n; the calculation formula is as follows: ; ; ; ; ; ; Among them, x b,(i / n)t ,y b,(i / n)t and z b,(i / n)t are the position coordinates of the first remaining argon bubble in the i-th state within t seconds, x p,(i / n)t ,y p,(i / n)t and z p,(i / n)t are the position coordinates of the second potential collision inclusion in the i-th state within t seconds respectively; S46: Calculate the spherical center distance D between the first remaining argon bubble and the second potential collision inclusion at the i-th state, i.e., at time i / n, according to the position coordinates of each argon bubble and inclusion obtained in step S46. i As shown below: ; Define the distance D between the sphere center of the inclusion and the argon bubble i When it is smaller than the sum of the two radii, the corresponding inclusion collides with the bubble, which is the inclusion to be removed. The inclusion to be removed is removed from the first remaining inclusions to obtain the second remaining inclusions. The second remaining inclusions and the first remaining argon bubbles have motion behavior, that is, the motion behavior of the argon bubbles and inclusions in the crystallizer is obtained.
7. A method for simulating particle movement and interaction behavior in a continuous casting mold as claimed in claim 6, It is characterized in that The specific method for obtaining the inclusion radius Rp in step 41 is: sampling the ingot and measuring the inclusion size by electron microscope observation; the radius Rp of the argon bubble b 1~5×10 -3 m.
8. A method for simulating particle movement and interaction behavior in a continuous casting mold as claimed in claim 6, It is characterized in that The separation condition in step S42 is specifically: the volume fraction of the mold slag phase f slag ≥0.5 or solid phase ratio f solid ≥ 0.
7.
9. A method for simulating particle movement and interaction behavior in a continuous casting mold as claimed in claim 6, It is characterized in that In step S44, the collisionable angle range is -90 to 90 degrees.
Citation Information
Patent Citations
Method for researching motion law of nonmetallic inclusion in continuous casting crystallizer under effect of stirring magnetic field
CN105108092A
Method for calculating motion of inclusion crossing slag / metal interface in VIDP smelting process
CN115841060A