A thermal insulation and warm-keeping composite fabric, preparation method and application in clothing
Through the combination of modified fiber and cellulose aerogel, the deficiencies in energy storage and antibacterial performance of existing insulation fabrics are solved, and the long-lasting antibacterial and insulation effects of the composite fabric are achieved, making it suitable for winter clothing.
Patent Information
- Application Number
- CN202411147762.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-08-21
AI Technical Summary
Existing thermal insulation composite fabrics have deficiencies in energy storage, heat storage and temperature regulation capabilities and antibacterial properties, which affects their application effects.
Modified cotton fiber and modified hollow polyester fiber are used to treat antibacterial finishing agents, and combined with an intermediate layer material of modified cellulose aerogel and phase change material eicosane to form a composite fabric with antibacterial and heat insulation properties.
It achieves the long-lasting antibacterial properties and excellent thermal insulation performance of the composite fabric, has heat storage and warmth preservation effect, and is suitable for winter clothing.
Smart Images

Figure CN118668484B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of multi-layer composite fabrics, and in particular to a heat-insulating and warm-keeping composite fabric, a preparation method and application in clothing. Background Art
[0002] The regulation of body temperature plays a key role in maintaining the normal functions of the human body. The principle of traditional thermal clothing is to prevent the heat emitted by the body from escaping. However, ordinary natural fibers or synthetic fibers have high thermal conductivity and average thermal insulation performance. Usually, the thickness and weight are increased to achieve better thermal insulation, which affects the lightweight development of clothing.
[0003] Aerogel, as a type of solid material with nanoporous structure, has the advantages of low thermal conductivity, high specific surface area, low density, etc. It has unique advantages in the field of lightweight thermal insulation applications. In the prior art, aerogel nanoparticles are added to the fabric by blending or spraying, or aerogel block materials are sandwiched between two layers of fabric as a core layer to play a role in heat insulation and warmth preservation. Prior art, such as Chinese patent application CN109130405A, discloses a thermal insulation cover and its preparation method, which uses a composite material made of aerogel and foaming material as an intermediate layer, selects suitable inner and outer fabrics for multi-layer lamination, and forms an aerogel composite fabric that can be directly cut to make various textiles. The aerogel powder will not overflow, which improves the flexibility of the use of aerogel materials. The intermediate layer is made by mixing aerogel and foaming material, and foaming them together to form a porous aerogel composite material. Although the thermal insulation performance of the composite fabric is improved, the energy storage, heat storage and temperature regulation ability of the fabric itself needs to be improved, and the antibacterial performance of the fabric is poor, which limits its application. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a heat-insulating and warm composite fabric, a preparation method and its application in clothing. The composite fabric has antibacterial effect, excellent heat-insulating performance, and can store energy and regulate temperature. It has a long-lasting heat storage and warmth effect and can be applied to winter clothing.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0006] A method for preparing a heat-insulating and warm-keeping composite fabric comprises the following steps:
[0007] Step 1, preparing inner layer fabric and outer layer fabric;
[0008] Cotton fiber, carboxymethyl chitosan, L-arginine and water are mixed, immersed, taken out after the immersion, reacted, and dried after the reaction to obtain modified cotton fiber; hollow polyester fiber, 1,6-hexanediamine and water are mixed, immersed, reacted, taken out after the reaction, washed to neutrality, and dried to obtain modified hollow polyester fiber;
[0009] The modified hollow polyester fiber is spun into yarn as warp yarn, and the modified cotton fiber is spun into yarn as weft yarn, and the yarns are woven to obtain a modified hollow polyester / cotton fabric;
[0010] The modified hollow polyester / cotton fabric is impregnated in an antibacterial finishing agent, and after the impregnation, the fabric is baked and dried to obtain an inner layer fabric and an outer layer fabric respectively;
[0011] Wherein, the antibacterial finishing agent is prepared by the following steps:
[0012] Step (1), mixing an ethanol aqueous solution with 3-(2,3-epoxypropoxy)propyltrimethoxysilane, adding a regulator to adjust the pH value, adding nano zirconium carbide, ultrasonically dispersing, reacting, and after the reaction is completed, filtering, washing, and drying to obtain epoxy nano zirconium carbide;
[0013] Step (2), mixing dodecyldimethyl tertiary amine and 3-bromo-1-propanol, reacting, washing, filtering, taking the filter cake, and drying to obtain an antibacterial agent; mixing epoxy nano zirconium carbide, the antibacterial agent, and isopropanol, reacting, filtering, and washing to obtain antibacterial functionalized nano zirconium carbide; mixing the antibacterial functionalized nano zirconium carbide with water to obtain an antibacterial finishing agent;
[0014] Step 2: preparing the intermediate layer material;
[0015] Heat eicosane until it melts, immerse the modified cellulose aerogel in the eicosane, and take it out after the immersion is completed to obtain an intermediate layer material;
[0016] The modified cellulose aerogel is prepared by the following steps:
[0017] Step (1), mixing isocyanate prepolymer and amino nano-silica, reacting, adding octafluoropentanol after the reaction, continuing the reaction, adding imidazole after the reaction, reacting again, cooling after the reaction, and obtaining a blocked isocyanate;
[0018] Step (2), mixing cellulose acetate, acetone and N,N-dimethylformamide, stirring until completely dissolved, standing, adding blocked isocyanate and mixing evenly to obtain a modified cellulose spinning solution; injecting the modified cellulose spinning solution into a syringe of an electrospinning device, spinning through the electrospinning instrument, and drying after spinning to obtain a modified cellulose nanofiber membrane;
[0019] The modified cellulose nanofiber film is sheared and crushed, water is added, and the dispersion is homogeneously dispersed to obtain a modified cellulose nanofiber dispersion, and the dispersion is freeze-dried, and after drying, the dispersion is reacted to obtain a modified cellulose aerogel;
[0020] Step 3: Compound the inner layer fabric, the middle layer material and the surface layer fabric to obtain a heat-insulating and warm composite fabric.
[0021] Preferably, in the step 1, the mass ratio of cotton fiber, carboxymethyl chitosan, L-arginine and water is 10:0.3-0.4:0.3-0.4:150-180; when preparing the modified cotton fiber, the impregnation conditions are: impregnation at room temperature for 2-3 hours, and the reaction conditions are: reaction at 170-180°C for 3-4 minutes; the mass ratio of hollow polyester fiber, 1,6-hexanediamine and water is 10:1.5-1.8:150-180; when preparing the modified hollow polyester fiber, the impregnation conditions are: impregnation at 60-70°C for 40-60 minutes, and the reaction conditions are: reaction at 150-160°C for 10-15 minutes.
[0022] Preferably, in step 1: the yarn count of the modified hollow polyester fiber is 40-60S in British standard; the yarn count of the modified cotton fiber is 40-60S in British standard; the gram weight of the modified hollow polyester / cotton fabric is 120-140g / m 2 The bath ratio of the modified hollow polyester / cotton fabric to the antibacterial finishing agent is 1:10-15; the dipping operation is: dipping at room temperature for 20-30 minutes, double dipping and double rolling, and the rolling rate is 78-82%; the baking conditions are: baking at 100-120°C for 3-5 minutes.
[0023] Preferably, in the preparation of the antibacterial finishing agent in step 1, in step (1): the mass ratio of ethanol aqueous solution, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, and nano zirconium carbide is 100:6-8:1-1.5, and the ethanol aqueous solution is 50 vol% ethanol aqueous solution; the reaction conditions are: reacting at a pH value of 4-4.5 and a temperature of 55-65°C for 2-3 hours.
[0024] Preferably, the regulator comprises a 1 mol / L acetic acid aqueous solution.
[0025] Preferably, in the preparation of the antibacterial finishing agent in step 1, in step (2): the mass ratio of dodecyldimethyl tertiary amine to 3-bromo-1-propanol is 2-2.1:1.4-1.6; when preparing the antibacterial agent, the reaction conditions are: reacting at a temperature of 60-70°C for 12-14h; the mass ratio of epoxy nano-zirconium carbide, antibacterial agent, and isopropanol is 1-1.2:1:80-100; when preparing antibacterial functionalized nano-zirconium carbide, the reaction conditions are: reacting at a temperature of 70-80°C for 3-4h; the mass ratio of antibacterial functionalized nano-zirconium carbide to water is 1:40-50.
[0026] Preferably, when preparing the antimicrobial agent, the detergent used in the washing operation includes ether.
[0027] Preferably, in step 2: the solid-liquid ratio of the modified cellulose aerogel to eicosane is 1:4-5; the impregnation conditions are: vacuum impregnation at 40-45° C. for 30-40 hours; and the thickness of the intermediate layer material is 0.3-0.4 mm.
[0028] Preferably, in the preparation of the modified cellulose aerogel in step 2, in step (1): the mass ratio of isocyanate prepolymer, octafluoropentanol, amino nano-silica and imidazole is 30:3.9-4:1.8-2:5-6; the reaction conditions are: reacting in a nitrogen atmosphere at a temperature of 55-65°C for 1-2h; continuing the reaction conditions are: continuing the reaction in a nitrogen atmosphere at a temperature of 70-75°C for 2-3h; and the second reaction conditions are: reacting again in a nitrogen atmosphere at a temperature of 50-60°C for 3-4h.
[0029] Preferably, in the preparation of the modified cellulose aerogel in step 2, in step (2): the mass ratio of cellulose acetate, acetone, N,N-dimethylformamide, and blocked isocyanate is 10:28-30:28-30:8-10; in the electrospinning operation, the propulsion speed of the modified cellulose spinning solution is 1.0 ml / h, the spinning voltage is 20 kV, and the distance from the spinning needle to the receiving screen is 15 cm; the receiving screen for electrospinning is aluminum foil.
[0030] Preferably, in the preparation of the modified cellulose aerogel in step 2, in step (2): the mass ratio of the modified cellulose nanofiber membrane to water is 1:15-18; the freeze-drying operation comprises: freezing the modified cellulose nanofiber dispersion at -80°C for 4-4.5 hours, and after freezing, freeze-drying in a freeze dryer at a temperature of -80°C and a pressure of 0.5 Pa for 45-48 hours; the reaction conditions are: reacting at a temperature of 140-150°C for 4-5 hours.
[0031] Preferably, a heat insulating and thermal insulation composite fabric is prepared by the preparation method of the heat insulating and thermal insulation composite fabric as described above.
[0032] Preferably, the thermal insulation and warmth-keeping composite fabric as described above is used in clothing.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The present invention prepares modified hollow polyester / cotton fabrics, and impregnates the fabrics with an antibacterial finishing agent containing antibacterial functionalized nano zirconium carbide to prepare inner and outer fabrics with antibacterial properties and light-absorbing and heating functions; prepares modified cellulose aerogel, and composites the aerogel with a phase change material eicosane, and composites the obtained intermediate layer material with the inner and outer fabrics to prepare a composite fabric with antibacterial effect, excellent heat insulation performance, energy storage and temperature regulation, and lasting heat storage and warmth-keeping effect, and can be applied to winter clothing.
[0035] Nano zirconium carbide is a photothermal conversion material that can enhance the light absorption and heating function of fabrics. In the present invention, the surface of nano zirconium carbide is modified by an epoxy silane coupling agent to obtain epoxy nano zirconium carbide, and a quaternization reaction is carried out between dodecyl dimethyl tertiary amine and 3-bromo-1-propanol to obtain an organic quaternary ammonium salt antibacterial agent with a hydroxyl active group. The organic quaternary ammonium salt antibacterial agent is mixed with the epoxy nano zirconium carbide to undergo a ring-opening reaction, so that the antibacterial agent and the nano zirconium carbide as a carrier are grafted and compounded through chemical bonds, which can not only improve the dispersibility of the nano zirconium carbide, but also improve the stability of the antibacterial agent, making it difficult to migrate, and the obtained antibacterial functionalized nano zirconium carbide has a lasting antibacterial property and a light absorption and heating function.
[0036] The present invention mixes cotton fiber with carboxymethyl chitosan and L-arginine, and esterifies the hydroxyl groups on the surface of the cotton fiber with the carboxyl groups on the surfaces of the carboxymethyl chitosan and the L-arginine, so that the carboxymethyl chitosan and the L-arginine with antibacterial property are loaded on the surface of the cotton fiber, so as to prepare the modified cotton fiber with antibacterial function; 1,6-hexanediamine is used to perform surface treatment on the hollow polyester fiber, and amino active groups are introduced to prepare the modified hollow polyester fiber with amino groups; the modified hollow polyester fiber and the modified cotton fiber are respectively spun into yarns, and the modified hollow polyester / cotton fabric is obtained after weaving, and the modified hollow polyester / cotton fabric is impregnated with an antibacterial finishing agent, and the unreacted epoxy groups on the surface of the antibacterial functionalized nano zirconium carbide in the antibacterial finishing agent can further undergo a ring-opening reaction with the active groups on the surface of the modified hollow polyester / cotton fabric during the impregnation process, so that the organic antibacterial component and the inorganic carrier nano zirconium carbide are firmly attached to the surface of the fabric, and the obtained inner layer fabric and outer layer fabric not only have a lasting antibacterial property, but also have a lasting heat storage and warmth-keeping effect.
[0037] Polymer aerogel has the advantages of low thermal conductivity, high specific surface area, low density, etc. As a lightweight thermal insulation material, it can improve the thermal insulation effect of fabrics; cellulose nanofiber aerogel has low density, low thermal conductivity and better flexibility. It can be used as a thermal insulation interlayer of composite fabrics to effectively improve the thermal insulation ability of fabrics; the present invention reacts the isocyanate group of isocyanate prepolymer with the amino group of amino nano-silica, and after the reaction, octafluoropentanol and imidazole are added for end-capping to obtain blocked isocyanate, and the introduction of rigid particle nano-silica and hydrophobic octafluoropentanol makes the blocked isocyanate have It has better mechanical properties and hydrophobicity; the blocked polyurethane is introduced into the cellulose spinning solution as a cross-linking agent, and the modified cellulose aerogel with better mechanical properties and hydrophobicity is obtained through electrospinning, crushing and homogenization, freeze drying, and in-situ cross-linking; among them, imidazole as a blocking agent can temporarily block the isocyanate group, and can unblock and release the isocyanate group again at high temperature. In the process of in-situ cross-linking, the isocyanate group of the blocked isocyanate reacts with the hydroxyl group of cellulose acetate to form a cross-linking structure, which improves the flexibility and hydrophobicity of the modified cellulose aerogel, and can be better used in the thermal insulation interlayer of composite fabrics;
[0038] The middle layer material in the present invention is prepared by vacuum impregnation and compounding modified cellulose aerogel and phase change material eicosane, and the inner layer fabric, the middle layer material and the outer layer fabric are compounded to obtain a heat-insulating and warm composite fabric; wherein, since the middle layer material contains the phase change material, when the outer layer fabric and the inner layer fabric absorb light and generate heat, and the ambient temperature is higher than the phase change temperature of the phase change material, the middle layer material can first absorb and store the heat, and when the ambient temperature drops below the phase change temperature, the middle layer material will slowly release the stored energy to achieve the effects of energy storage and temperature regulation, heat generation and warmth preservation, so that the prepared heat-insulating and warm composite fabric not only has excellent thermal insulation performance, but also can store energy and regulate temperature, and has a lasting heat storage and warmth preservation effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a process flow chart for preparing heat-insulating and warm-keeping composite fabrics in the present invention;
[0040] Figure 2 It is a schematic structural diagram of the heat-insulating and warm-keeping composite fabric prepared in the present invention;
[0041] Figure 3 It is a bar graph of thermal enthalpy values of Examples 1-5 and Comparative Examples 1-2 in the performance test of the present invention;
[0042] Figure 4 It is a temperature difference bar graph of Examples 1-5 and Comparative Examples 1-2 in the performance test of the present invention;
[0043] Figure 5It is a bar graph of the antibacterial rates of Examples 1-5 and Comparative Examples 1-2 in the performance test of the present invention;
[0044] In the figure:
[0045] 1. Outer layer fabric; 2. Middle layer material; 3. Inner layer fabric. DETAILED DESCRIPTION
[0046] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0047] Example 1
[0048] This embodiment discloses a method for preparing a heat-insulating and warm-keeping composite fabric, comprising the following steps:
[0049] Step 1, preparing inner layer fabric and outer layer fabric;
[0050] Cotton fiber, carboxymethyl chitosan, L-arginine and water were mixed in a mass ratio of 10:0.3:0.3:150, immersed at room temperature for 2 hours, taken out after the immersion, reacted at 170°C for 4 minutes, and dried at 90°C for 10 hours after the reaction to obtain modified cotton fiber; hollow polyester fiber, 1,6-hexanediamine and water were mixed in a mass ratio of 10:1.5:150, immersed at 60°C for 60 minutes, reacted at 150°C for 15 minutes, taken out after the reaction, washed with water until neutral, and dried at 50°C for 2 hours to obtain modified hollow polyester fiber;
[0051] The modified hollow polyester fiber was spun into yarn as the warp yarn, the yarn count was 40S in British standard, and the modified cotton fiber was spun into yarn as the weft yarn, the yarn count was 40S in British standard, and the weft yarn was woven to obtain a gram weight of 120g / m 2 Modified hollow polyester / cotton fabric;
[0052] The modified hollow polyester / cotton fabric was impregnated in an antibacterial finishing agent at a bath ratio of 1:10, and was impregnated for 20 minutes at room temperature, and then double-impregnated and double-rolled, with a rolling rate of 78%. After the impregnation, the fabric was baked at 100°C for 5 minutes and dried at 50°C for 6 hours to obtain an inner layer fabric and an outer layer fabric, respectively.
[0053] Wherein, the antibacterial finishing agent is prepared by the following steps:
[0054] Step (1), mixing 50 vol% ethanol aqueous solution and 3-(2,3-epoxypropoxy)propyltrimethoxysilane, adding 1 mol / L acetic acid aqueous solution to adjust the pH value to 4, adding nano zirconium carbide, ultrasonically dispersing for 15 minutes, reacting at 60°C for 2.5 hours, after the reaction, filtering, taking the filter cake, adding acetone 6 times the mass of the filter cake to wash three times, and drying at 75°C for 8 hours to obtain epoxy nano zirconium carbide;
[0055] The mass ratio of 50 vol% ethanol aqueous solution, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, and nano zirconium carbide is 100:7:1.3;
[0056] Step (2), mixing dodecyldimethyl tertiary amine and 3-bromo-1-propanol in a mass ratio of 2:1.4, reacting at 60°C for 14 hours, after the reaction is completed, obtaining a reaction product, adding ether 3 times the mass of the reaction product to wash three times, filtering, taking the filter cake, and drying at 40°C for 16 hours to obtain an antibacterial agent; mixing epoxy nano zirconium carbide, antibacterial agent, and isopropanol in a mass ratio of 1:1:80, reacting at 70°C for 4 hours, after the reaction is completed, filtering, taking the filter cake, and adding water 5 times the mass of the filter cake to wash to obtain antibacterial functionalized nano zirconium carbide; mixing the antibacterial functionalized nano zirconium carbide and water in a mass ratio of 1:50 to obtain an antibacterial finishing agent;
[0057] Step 2: preparing the intermediate layer material;
[0058] Heat eicosane at 40°C until it melts, immerse the modified cellulose aerogel in eicosane, the solid-liquid ratio of the modified cellulose aerogel to eicosane is 1:4, and vacuum immerse the aerogel at 40°C for 40 hours. After the immersion is completed, the aerogel is taken out to obtain an intermediate layer material with a thickness of 0.3 mm.
[0059] The modified cellulose aerogel is prepared by the following steps:
[0060] Step (1), mixing the isocyanate prepolymer with amino nano-silica, reacting for 1.5 hours in a nitrogen atmosphere at 60°C, adding octafluoropentanol, reacting for 2 hours at 75°C, adding imidazole, reacting for another 3.5 hours at 55°C, and cooling to room temperature to obtain a blocked isocyanate;
[0061] Among them, the mass ratio of isocyanate prepolymer, octafluoropentanol, amino nano-silica, and imidazole is 30:3.9:1.9:5.5;
[0062] Step (2), mixing cellulose acetate, acetone and N,N-dimethylformamide, stirring at room temperature until completely dissolved, standing for 5 hours, adding blocked isocyanate and mixing evenly, wherein the mass ratio of cellulose acetate, acetone, N,N-dimethylformamide and blocked isocyanate is 10:28:28:8, to obtain a modified cellulose spinning solution; injecting the modified cellulose spinning solution into a syringe of an electrospinning device, spinning at 20° C. through an electrospinning instrument, and drying at room temperature for 8 hours after spinning to obtain a modified cellulose nanofiber membrane;
[0063] The propulsion speed of the modified cellulose spinning solution was 1.0 ml / h, the spinning voltage was 20 kV, the distance from the spinning needle to the receiving screen was 15 cm, and the receiving screen for electrospinning was aluminum foil.
[0064] The modified cellulose nanofiber membrane was sheared and crushed, and water was added, the mass ratio of the modified cellulose nanofiber membrane to water was 1:18, and the modified cellulose nanofiber dispersion was obtained by homogenizing and dispersing at a speed of 8000r / min for 20min in a homogenizer to obtain a modified cellulose nanofiber dispersion, and the modified cellulose nanofiber dispersion was frozen at -80°C for 4h, and after freezing, freeze-dried in a freeze dryer at a temperature of -80°C and a pressure of 0.5Pa for 45h, and after drying, reacted at a temperature of 140°C for 5h to obtain a modified cellulose aerogel;
[0065] Step 3: Lay the inner layer fabric, the middle layer material, and the outer layer fabric together in sequence, align the layers, use pure cotton sewing thread as the sewing thread, and sew the inner layer fabric, the middle layer material, and the outer layer fabric through a multi-layer fabric quilting machine to obtain a heat-insulating and warm composite fabric.
[0066] Example 2
[0067] This embodiment discloses a method for preparing a heat-insulating and warm-keeping composite fabric, comprising the following steps:
[0068] Step 1, preparing inner layer fabric and outer layer fabric;
[0069] Cotton fiber, carboxymethyl chitosan, L-arginine and water were mixed in a mass ratio of 10:0.32:0.32:160, immersed at room temperature for 2 hours, taken out after the immersion, reacted at 175°C for 3.5 minutes, dried at 95°C for 9 hours after the reaction, and obtained modified cotton fiber; hollow polyester fiber, 1,6-hexanediamine and water were mixed in a mass ratio of 10:1.55:155, immersed at 65°C for 50 minutes, reacted at 155°C for 13 minutes, taken out after the reaction, washed with water until neutral, and dried at 55°C for 1 hour to obtain modified hollow polyester fiber;
[0070] The modified hollow polyester fiber was spun into yarn as the warp yarn, the yarn count was British 45S, and the modified cotton fiber was spun into yarn as the weft yarn, the yarn count was British 45S, and the weft yarn was woven to obtain a gram weight of 125g / m 2 Modified hollow polyester / cotton fabric;
[0071] The modified hollow polyester / cotton fabric was impregnated in an antibacterial finishing agent at a bath ratio of 1:10, and was impregnated for 25 minutes at room temperature, and then double-impregnated and double-rolled, with a rolling rate of 79%. After the impregnation, the fabric was baked at 110°C for 4 minutes and dried at 55°C for 5.5 hours to obtain an inner layer fabric and an outer layer fabric, respectively.
[0072] Wherein, the antibacterial finishing agent is prepared by the following steps:
[0073] Dodecyldimethyl tertiary amine and 3-bromo-1-propanol were mixed in a mass ratio of 2.03:1.45, reacted at 65°C for 13 hours, and after the reaction was completed, a reaction product was obtained, and ether was added in an amount 3 times the mass of the reaction product to wash three times, and the mixture was filtered off with suction, and the filter cake was taken and dried at 45°C for 14 hours to obtain an antibacterial agent; epoxy nano zirconium carbide, antibacterial agent, and isopropanol were mixed in a mass ratio of 1.05:1:85, and the preparation of epoxy nano zirconium carbide was the same as that in Example 1, and the mixture was reacted at 75°C for 3.5 hours. After the reaction was completed, the mixture was filtered, the filter cake was taken, and water 6 times the mass of the filter cake was added to wash the mixture to obtain antibacterial functionalized nano zirconium carbide; the antibacterial functionalized nano zirconium carbide was mixed with water in a mass ratio of 1:48 to obtain an antibacterial finishing agent;
[0074] Step 2: preparing the intermediate layer material;
[0075] Heat eicosane at 40°C until it melts, and immerse the modified cellulose aerogel in eicosane, with the solid-liquid ratio of the modified cellulose aerogel to eicosane being 1:4. Vacuum immerse the aerogel at 40°C for 35 hours, and take it out after immersion to obtain an intermediate layer material with a thickness of 0.33 mm.
[0076] The modified cellulose aerogel is prepared by the following steps:
[0077] Mix cellulose acetate, acetone and N,N-dimethylformamide, stir at room temperature until completely dissolved, let stand for 5.5 hours, add blocked isocyanate and mix evenly, the mass ratio of cellulose acetate, acetone, N,N-dimethylformamide and blocked isocyanate is 10:28.5:28.5:8.5, and obtain a modified cellulose spinning solution; inject the modified cellulose spinning solution into a syringe of an electrospinning device, spin through an electrospinning instrument at a temperature of 25°C, and after spinning, dry at room temperature for 9 hours to obtain a modified cellulose nanofiber membrane;
[0078] The preparation of blocked isocyanate was the same as that in Example 1; the propulsion speed of the modified cellulose spinning solution was 1.0 ml / h, the spinning voltage was 20 kV, the distance from the spinning needle to the receiving screen was 15 cm; the receiving screen for electrospinning was aluminum foil;
[0079] The modified cellulose nanofiber membrane was sheared and crushed, and water was added, the mass ratio of the modified cellulose nanofiber membrane to water was 1:17, and the modified cellulose nanofiber dispersion was obtained by homogenizing and dispersing at a speed of 8500r / min for 18min in a homogenizer to obtain a modified cellulose nanofiber dispersion, and the modified cellulose nanofiber dispersion was frozen at -80°C for 4h, and after freezing, freeze-dried in a freeze dryer at a temperature of -80°C and a pressure of 0.5Pa for 46h, and after drying, reacted at a temperature of 145°C for 5h to obtain a modified cellulose aerogel;
[0080] Step 3: Lay the inner layer fabric, the middle layer material, and the outer layer fabric together in sequence, align the layers, use pure cotton sewing thread as the sewing thread, and sew the inner layer fabric, the middle layer material, and the outer layer fabric through a multi-layer fabric quilting machine to obtain a heat-insulating and warm composite fabric.
[0081] Example 3
[0082] This embodiment discloses a method for preparing a heat-insulating and warm-keeping composite fabric, comprising the following steps:
[0083] Step 1, preparing inner layer fabric and outer layer fabric;
[0084] Cotton fiber, carboxymethyl chitosan, L-arginine and water were mixed in a mass ratio of 10:0.35:0.35:165, immersed at room temperature for 2.5 hours, taken out after the immersion, reacted at 175°C for 3.5 minutes, dried at 95°C for 9 hours after the reaction, and obtained modified cotton fiber; hollow polyester fiber, 1,6-hexanediamine and water were mixed in a mass ratio of 10:1.6:160, immersed at 65°C for 50 minutes, reacted at 155°C for 13 minutes, taken out after the reaction, washed with water until neutral, and dried at 55°C for 1.2 hours to obtain modified hollow polyester fiber;
[0085] The modified hollow polyester fiber was spun into yarn as the warp yarn, the yarn count was 50S in British standard, and the modified cotton fiber was spun into yarn as the weft yarn, the yarn count was 50S in British standard, and the weft yarn was woven to obtain a gram weight of 130g / m 2 Modified hollow polyester / cotton fabric;
[0086] The modified hollow polyester / cotton fabric was immersed in the antibacterial finishing agent at a bath ratio of 1:12, immersed at room temperature for 25 minutes, immersed twice and rolled twice, and the rolling rate was 80%. After the dipping, it was baked at 110°C for 4 minutes and dried at 55°C for 5.5 hours to obtain the inner layer fabric and the outer layer fabric respectively;
[0087] Wherein, the antibacterial finishing agent is prepared by the following steps:
[0088] Dodecyldimethyl tertiary amine and 3-bromo-1-propanol were mixed in a mass ratio of 2.05:1.5, reacted at 65°C for 13 hours, and after the reaction was completed, a reaction product was obtained, and ether was added in an amount 3 times the mass of the reaction product to wash three times, and the mixture was filtered off with suction, and the filter cake was taken and dried at 45°C for 14 hours to obtain an antibacterial agent; epoxy nano zirconium carbide, antibacterial agent, and isopropanol were mixed in a mass ratio of 1.1:1:90, and the preparation of epoxy nano zirconium carbide was the same as that in Example 1, and the mixture was reacted at 75°C for 3.5 hours. After the reaction was completed, the mixture was filtered, the filter cake was taken, and water 6 times the mass of the filter cake was added to wash the mixture to obtain antibacterial functionalized nano zirconium carbide; the antibacterial functionalized nano zirconium carbide was mixed with water in a mass ratio of 1:45 to obtain an antibacterial finishing agent;
[0089] Step 2: preparing the intermediate layer material;
[0090] Heat eicosane at 40°C until it melts, immerse the modified cellulose aerogel in eicosane, the solid-liquid ratio of the modified cellulose aerogel to eicosane is 1:4.5, and vacuum immerse for 35 hours at 40°C. After the immersion is completed, take out to obtain an intermediate layer material with a thickness of 0.35 mm;
[0091] The modified cellulose aerogel is prepared by the following steps:
[0092] Mix cellulose acetate, acetone and N,N-dimethylformamide, stir at room temperature until completely dissolved, let stand for 5.5 hours, add blocked isocyanate and mix evenly, the mass ratio of cellulose acetate, acetone, N,N-dimethylformamide and blocked isocyanate is 10:29:29:9, and obtain a modified cellulose spinning solution; inject the modified cellulose spinning solution into a syringe of an electrospinning device, spin through an electrospinning instrument at a temperature of 25°C, and after spinning, dry at room temperature for 9 hours to obtain a modified cellulose nanofiber membrane;
[0093] The preparation of blocked isocyanate was the same as that in Example 1; the propulsion speed of the modified cellulose spinning solution was 1.0 ml / h, the spinning voltage was 20 kV, the distance from the spinning needle to the receiving screen was 15 cm; the receiving screen for electrospinning was aluminum foil;
[0094] The modified cellulose nanofiber membrane was sheared and crushed, and water was added, the mass ratio of the modified cellulose nanofiber membrane to water was 1:16, and the modified cellulose nanofiber dispersion was obtained by homogenizing and dispersing at a speed of 9000r / min for 18min in a homogenizer to obtain a modified cellulose nanofiber dispersion, and the modified cellulose nanofiber dispersion was frozen at -80°C for 4h, and after freezing, freeze-dried in a freeze dryer at a temperature of -80°C and a pressure of 0.5Pa for 46h, and after drying, reacted at a temperature of 145°C for 4.5h to obtain a modified cellulose aerogel;
[0095] Step 3: Lay the inner layer fabric, the middle layer material, and the outer layer fabric together in sequence, align the layers, use pure cotton sewing thread as the sewing thread, and sew the inner layer fabric, the middle layer material, and the outer layer fabric through a multi-layer fabric quilting machine to obtain a heat-insulating and warm composite fabric.
[0096] Example 4
[0097] This embodiment discloses a method for preparing a heat-insulating and warm-keeping composite fabric, comprising the following steps:
[0098] Step 1, preparing inner layer fabric and outer layer fabric;
[0099] Cotton fiber, carboxymethyl chitosan, L-arginine and water were mixed in a mass ratio of 10:0.38:0.38:175, immersed at room temperature for 3 hours, taken out after the immersion, reacted at 175°C for 3.5 minutes, dried at 95°C for 9 hours after the reaction, and obtained modified cotton fiber; hollow polyester fiber, 1,6-hexanediamine and water were mixed in a mass ratio of 10:1.7:170, immersed at 65°C for 50 minutes, reacted at 155°C for 13 minutes, taken out after the reaction, washed with water until neutral, and dried at 50°C for 2 hours to obtain modified hollow polyester fiber;
[0100] The modified hollow polyester fiber was spun into yarn as the warp yarn, the yarn count was 55S in British standard, and the modified cotton fiber was spun into yarn as the weft yarn, the yarn count was 55S in British standard, and the weft yarn was woven to obtain a gram weight of 135g / m 2 Modified hollow polyester / cotton fabric;
[0101] The modified hollow polyester / cotton fabric was impregnated in an antibacterial finishing agent at a bath ratio of 1:15, and was impregnated for 30 minutes at room temperature, and then subjected to two impregnations and two rollings, with a rolling rate of 81%. After the impregnation, the fabric was baked at 110°C for 4 minutes and dried at 60°C for 5 hours to obtain an inner layer fabric and an outer layer fabric, respectively.
[0102] Wherein, the antibacterial finishing agent is prepared by the following steps:
[0103] Dodecyldimethyl tertiary amine and 3-bromo-1-propanol were mixed in a mass ratio of 2.08:1.55, reacted at 65°C for 13 hours, and after the reaction was completed, a reaction product was obtained, and ether was added in an amount 3 times the mass of the reaction product to wash three times, filtered, and the filter cake was taken and dried at 45°C for 14 hours to obtain an antibacterial agent; epoxy nano zirconium carbide, antibacterial agent, and isopropanol were mixed in a mass ratio of 1.15:1:95, and the preparation of epoxy nano zirconium carbide was the same as that in Example 1, and the reaction was carried out at 75°C for 4 hours. After the reaction was completed, the filter cake was taken and washed with water 8 times the mass of the filter cake to obtain antibacterial functionalized nano zirconium carbide; antibacterial functionalized nano zirconium carbide and water were mixed in a mass ratio of 1:43 to obtain an antibacterial finishing agent;
[0104] Step 2: preparing the intermediate layer material;
[0105] Heat eicosane at 45°C until it melts, immerse the modified cellulose aerogel in eicosane, the solid-liquid ratio of the modified cellulose aerogel to eicosane is 1:5, and vacuum immerse for 35 hours at 40°C. After the immersion, take out the material to obtain an intermediate layer material with a thickness of 0.38 mm.
[0106] The modified cellulose aerogel is prepared by the following steps:
[0107] Mix cellulose acetate, acetone and N,N-dimethylformamide, stir at room temperature until completely dissolved, let stand for 6 hours, add blocked isocyanate and mix evenly, the mass ratio of cellulose acetate, acetone, N,N-dimethylformamide and blocked isocyanate is 10:29.5:29.5:9.5, and obtain modified cellulose spinning solution; inject the modified cellulose spinning solution into the syringe of the electrospinning equipment, spin through the electrospinning instrument at a temperature of 25°C, and after spinning, dry at room temperature for 10 hours to obtain a modified cellulose nanofiber membrane;
[0108] The preparation of blocked isocyanate was the same as that in Example 1; the propulsion speed of the modified cellulose spinning solution was 1.0 ml / h, the spinning voltage was 20 kV, the distance from the spinning needle to the receiving screen was 15 cm; the receiving screen for electrospinning was aluminum foil;
[0109] The modified cellulose nanofiber membrane was sheared and crushed, and water was added, with the mass ratio of the modified cellulose nanofiber membrane to water being 1:15.5. The modified cellulose nanofiber dispersion was obtained by homogenizing and dispersing the dispersion at 9500 r / min for 18 min using a homogenizer, and the modified cellulose nanofiber dispersion was frozen at -80°C for 4.5 h. After freezing, the dispersion was freeze-dried in a freeze dryer at -80°C and 0.5 Pa for 48 h. After drying, the dispersion was reacted at 145°C for 4.5 h to obtain a modified cellulose aerogel.
[0110] Step 3: Lay the inner layer fabric, the middle layer material, and the outer layer fabric together in sequence, align the layers, use pure cotton sewing thread as the sewing thread, and sew the inner layer fabric, the middle layer material, and the outer layer fabric through a multi-layer fabric quilting machine to obtain a heat-insulating and warm composite fabric.
[0111] Example 5
[0112] This embodiment discloses a method for preparing a heat-insulating and warm-keeping composite fabric, comprising the following steps:
[0113] Step 1, preparing inner layer fabric and outer layer fabric;
[0114] Cotton fiber, carboxymethyl chitosan, L-arginine and water were mixed in a mass ratio of 10:0.4:0.4:180, immersed at room temperature for 3 hours, taken out after the immersion, reacted at 180°C for 3 minutes, dried at 100°C for 8 hours, and obtained modified cotton fiber; hollow polyester fiber, 1,6-hexanediamine and water were mixed in a mass ratio of 10:1.8:180, immersed at 70°C for 40 minutes, reacted at 160°C for 10 minutes, taken out after the reaction, washed with water until neutral, and dried at 60°C for 1 hour to obtain modified hollow polyester fiber;
[0115] The modified hollow polyester fiber was spun into yarn as the warp yarn, the yarn count was 60S in British standard, and the modified cotton fiber was spun into yarn as the weft yarn, the yarn count was 60S in British standard, and the weft yarn was woven to obtain a gram weight of 140g / m 2 Modified hollow polyester / cotton fabric;
[0116] The modified hollow polyester / cotton fabric was impregnated in an antibacterial finishing agent at a bath ratio of 1:15, and was impregnated for 30 minutes at room temperature, and then subjected to two impregnations and two rollings, with a rolling rate of 82%. After the impregnation, the fabric was baked at 120°C for 3 minutes and dried at 60°C for 5 hours to obtain an inner layer fabric and an outer layer fabric, respectively.
[0117] Wherein, the antibacterial finishing agent is prepared by the following steps:
[0118] Dodecyldimethyl tertiary amine and 3-bromo-1-propanol were mixed in a mass ratio of 2.1:1.6, reacted at 70°C for 12 hours, and after the reaction, a reaction product was obtained. Ether 3 times the mass of the reaction product was added to wash three times, filtered, and the filter cake was taken. It was dried at 50°C for 12 hours to obtain an antibacterial agent; epoxy nano zirconium carbide, antibacterial agent, and isopropanol were mixed in a mass ratio of 1.2:1:100. The preparation of epoxy nano zirconium carbide was the same as that in Example 1. The reaction was carried out at 80°C for 3 hours. After the reaction was completed, it was filtered, the filter cake was taken, and water 8 times the mass of the filter cake was added to wash to obtain antibacterial functionalized nano zirconium carbide; the antibacterial functionalized nano zirconium carbide was mixed with water in a mass ratio of 1:40 to obtain an antibacterial finishing agent;
[0119] Step 2: preparing the intermediate layer material;
[0120] Heat eicosane at 45°C until it melts, immerse the modified cellulose aerogel in eicosane, the solid-liquid ratio of the modified cellulose aerogel to eicosane is 1:5, and vacuum immerse for 30 hours at 45°C. After the immersion is completed, take out to obtain an intermediate layer material with a thickness of 0.4 mm;
[0121] The modified cellulose aerogel is prepared by the following steps:
[0122] Mix cellulose acetate, acetone and N,N-dimethylformamide, stir at room temperature until completely dissolved, let stand for 6 hours, add blocked isocyanate and mix evenly, the mass ratio of cellulose acetate, acetone, N,N-dimethylformamide and blocked isocyanate is 10:30:30:10, and obtain modified cellulose spinning solution; inject the modified cellulose spinning solution into the syringe of the electrospinning equipment, spin through the electrospinning instrument at a temperature of 30°C, and after spinning, dry at room temperature for 10 hours to obtain a modified cellulose nanofiber membrane;
[0123] The preparation of blocked isocyanate was the same as that in Example 1; the propulsion speed of the modified cellulose spinning solution was 1.0 ml / h, the spinning voltage was 20 kV, the distance from the spinning needle to the receiving screen was 15 cm; the receiving screen for electrospinning was aluminum foil;
[0124] The modified cellulose nanofiber membrane was sheared and crushed, and water was added, with the mass ratio of the modified cellulose nanofiber membrane to water being 1:15. The modified cellulose nanofiber dispersion was obtained by homogenizing and dispersing the dispersion at a speed of 10000 r / min for 15 min in a homogenizer, and the modified cellulose nanofiber dispersion was frozen at -80°C for 4.5 h. After freezing, the dispersion was freeze-dried in a freeze dryer at a temperature of -80°C and a pressure of 0.5 Pa for 48 h. After drying, the dispersion was reacted at a temperature of 150°C for 4 h to obtain a modified cellulose aerogel.
[0125] Step 3: Lay the inner layer fabric, the middle layer material, and the outer layer fabric together in sequence, align the layers, use pure cotton sewing thread as the sewing thread, and sew the inner layer fabric, the middle layer material, and the outer layer fabric through a multi-layer fabric quilting machine to obtain a heat-insulating and warm composite fabric.
[0126] Comparative Example 1
[0127] This embodiment discloses a method for preparing a composite fabric, comprising the following steps:
[0128] Step 1, preparing inner layer fabric and outer layer fabric;
[0129] Cotton fiber, carboxymethyl chitosan, L-arginine and water were mixed in a mass ratio of 10:0.3:0.3:150, immersed at room temperature for 2 hours, taken out after the immersion, reacted at 170°C for 4 minutes, and dried at 90°C for 10 hours after the reaction to obtain modified cotton fiber; hollow polyester fiber, 1,6-hexanediamine and water were mixed in a mass ratio of 10:1.5:150, immersed at 60°C for 60 minutes, reacted at 150°C for 15 minutes, taken out after the reaction, washed with water until neutral, and dried at 50°C for 2 hours to obtain modified hollow polyester fiber;
[0130] The modified hollow polyester fiber was spun into yarn as the warp yarn, the yarn count was 40S in British standard, and the modified cotton fiber was spun into yarn as the weft yarn, the yarn count was 40S in British standard, and the weft yarn was woven to obtain a gram weight of 120g / m 2 Modified hollow polyester / cotton fabric;
[0131] The modified hollow polyester / cotton fabric was impregnated in an antibacterial finishing agent at a bath ratio of 1:10, and was impregnated for 20 minutes at room temperature, and then double-impregnated and double-rolled, with a rolling rate of 78%. After the impregnation, the fabric was baked at 100°C for 5 minutes and dried at 50°C for 6 hours to obtain an inner layer fabric and an outer layer fabric, respectively.
[0132] Wherein, the antibacterial finishing agent is prepared by the following steps:
[0133] Dodecyldimethyl tertiary amine and 3-bromo-1-propanol were mixed in a mass ratio of 2:1.4, reacted at 60°C for 14 hours, and after the reaction was completed, a reaction product was obtained, and ether was added in an amount 3 times the mass of the reaction product to wash three times, and the mixture was filtered off with suction, and the filter cake was taken and dried at 40°C for 16 hours to obtain an antibacterial agent; epoxy nano-zirconium carbide, antibacterial agent, and isopropanol were mixed in a mass ratio of 1:1:80, and the preparation of epoxy nano-zirconium carbide was the same as that in Example 1, and the mixture was reacted at 70°C for 4 hours. After the reaction was completed, the mixture was filtered, the filter cake was taken, and water 5 times the mass of the filter cake was added to wash the mixture to obtain antibacterial functionalized nano-zirconium carbide; the antibacterial functionalized nano-zirconium carbide was mixed with water in a mass ratio of 1:50 to obtain an antibacterial finishing agent;
[0134] Step 3: Lay the inner layer fabric and the outer layer fabric together in sequence, align the layers, use pure cotton sewing thread as the sewing thread, and sew the inner layer fabric and the outer layer fabric together through a multi-layer fabric quilting machine to obtain a composite fabric.
[0135] Comparative Example 2
[0136] This embodiment discloses a method for preparing a composite fabric, comprising the following steps:
[0137] Step 1, preparing inner layer fabric and outer layer fabric;
[0138] Cotton fiber, carboxymethyl chitosan, L-arginine and water were mixed in a mass ratio of 10:0.3:0.3:150, immersed at room temperature for 2 hours, taken out after the immersion, reacted at 170°C for 4 minutes, dried at 90°C for 10 hours after the reaction, and obtained modified cotton fiber; hollow polyester fiber, 1,6-hexanediamine and water were mixed in a mass ratio of 10:1.5:150, immersed at 60°C for 60 minutes, reacted at 150°C for 15 minutes, taken out after the reaction, washed with water until neutral, and dried at 50°C for 2 hours to obtain modified hollow polyester fiber;
[0139] The modified hollow polyester fiber was spun into yarn as the warp yarn, the yarn count was 40S in British standard, and the modified cotton fiber was spun into yarn as the weft yarn, the yarn count was 40S in British standard, and the weft yarn was woven to obtain a gram weight of 120g / m 2 Modified hollow polyester / cotton fabric;
[0140] The modified hollow polyester / cotton fabric was impregnated in the finishing agent, impregnated at room temperature for 20 minutes, and double-impregnated and double-rolled, with a rolling rate of 78%. After the impregnation, it was baked at 100°C for 5 minutes and dried at 50°C for 6 hours to obtain an inner layer fabric and an outer layer fabric respectively.
[0141] Wherein, the antibacterial finishing agent is prepared by the following steps:
[0142] Dodecyldimethyl tertiary amine and 3-bromo-1-propanol were mixed in a mass ratio of 2:1.4, and reacted at 60°C for 14 hours. After the reaction was completed, a reaction product was obtained, and ether was added in an amount of 3 times the mass of the reaction product to wash three times, and the filter cake was taken out by suction and dried at 40°C for 16 hours to obtain an antibacterial agent; nano zirconium carbide, the antibacterial agent, and water were mixed in a mass ratio of 1:1:50 to obtain an antibacterial finishing agent;
[0143] Step 2: preparing the intermediate layer material;
[0144] Heat eicosane at 40°C until it melts, immerse the modified cellulose aerogel in eicosane, the solid-liquid ratio of the modified cellulose aerogel to eicosane is 1:4, and vacuum immerse the aerogel at 40°C for 40 hours. After the immersion is completed, the aerogel is taken out to obtain an intermediate layer material with a thickness of 0.3 mm.
[0145] The modified cellulose aerogel is prepared by the following steps:
[0146] Mix cellulose acetate, acetone and N,N-dimethylformamide, stir until completely dissolved at room temperature, let stand for 5 hours, add blocked isocyanate and mix evenly, the mass ratio of cellulose acetate, acetone, N,N-dimethylformamide and blocked isocyanate is 10:28:28:8, and obtain a modified cellulose spinning solution; inject the modified cellulose spinning solution into a syringe of an electrospinning device, spin through an electrospinning instrument at a temperature of 20°C, and after spinning, dry at room temperature for 8 hours to obtain a modified cellulose nanofiber membrane;
[0147] The preparation of blocked isocyanate was the same as that in Example 1; the propulsion speed of the modified cellulose spinning solution was 1.0 ml / h, the spinning voltage was 20 kV, the distance from the spinning needle to the receiving screen was 15 cm; the receiving screen for electrospinning was aluminum foil;
[0148] The modified cellulose nanofiber membrane was sheared and crushed, and water was added, the mass ratio of the modified cellulose nanofiber membrane to water was 1:18, and the modified cellulose nanofiber dispersion was obtained by homogenizing and dispersing at a speed of 8000r / min for 20min in a homogenizer to obtain a modified cellulose nanofiber dispersion, and the modified cellulose nanofiber dispersion was frozen at -80°C for 4h, and after freezing, freeze-dried in a freeze dryer at a temperature of -80°C and a pressure of 0.5Pa for 45h, and after drying, reacted at a temperature of 140°C for 5h to obtain a modified cellulose aerogel;
[0149] Step 3: Lay the inner layer fabric, the middle layer material, and the outer layer fabric together in sequence, align the layers, use pure cotton sewing thread as the sewing thread, and sew the inner layer fabric, the middle layer material, and the outer layer fabric through a multi-layer fabric quilting machine to obtain a composite fabric.
[0150] In the above embodiments and comparative examples: the cotton fiber is long-staple cotton with a fiber length of 38-39 mm; carboxymethyl chitosan comes from Shanghai Zhongfeng Biotechnology Co., Ltd. with a carboxylation degree of 80% and a CAS number of 83512-85-0; L-arginine comes from Alfa Aesar with a CAS number of 74-79-3; the hollow polyester fiber comes from Nantong Luolai Chemical Fiber Co., Ltd., which is a hollow polyester staple fiber with an average fiber length of 32 mm, a fineness of 15D, and a hollow fiber cross section; 1,6-hexanediamine comes from Shanghai McLean Biochemical Technology Co., Ltd. with a CAS number of 124-09-4; nano zirconium carbide comes from Hebei Teng Bimetallic Materials Co., Ltd. with a particle size of 50 nm and a CAS number of 12070-14-3; dodecyl dimethyl tertiary amine comes from Jinan Kaichuang Chemical Co., Ltd. with a CAS number of: 112-18-5; 3-bromo-1-propanol is from Shanghai MacLean Biochemical Technology Co., Ltd., CAS number: 627-18-9; isocyanate prepolymer is from Wuhan Shiquanxing New Materials Technology Co., Ltd., model D-100 non-ionic HDI water-based isocyanate curing agent, the supplied NCO content is 18.0±0.5%; amino nano-silica is from Qinghe Chaotai Metal Materials Co., Ltd., item number JL-SiO2-N22, particle size 20nm, model KH550 surface modified nano-silica; octafluoropentanol is from Alfa Aesar, CAS number: 355-80-6; imidazole is from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS number: 288-32-4; cellulose acetate is from Shanghai Aladdin Biochemical Technology Co., Ltd., Mn=30000, CAS number: 9004-35-7.
[0151] Test example
[0152] like Figure 3-5 As shown, the composite fabrics prepared in Examples 1-5 and Comparative Examples 1-2 were subjected to comprehensive performance tests. The specific test results are shown in Table 1:
[0153] Table 1
[0154]
[0155] The detection of each indicator in Table 1 is based on the following standards:
[0156] The warmth retention rate is determined by GB / T 11048-1989 "Test method for thermal insulation performance of textiles"; the thermal enthalpy value is determined by EN16806-1 "Textiles and textile products-Textiles containing phase change materials Part 1 Determination of heat storage and release capacity"; the thermal insulation performance is represented by the temperature difference, and the test method is: placing the composite fabrics prepared in Examples 1-5 and Comparative Examples 1-2 on the heating platform of a thermocouple thermometer, heating the fabrics to 40°C, and testing the temperature difference between the front and back of the fabrics; the antibacterial rate is determined by GB / T20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method", in which the bacterial species selected is Escherichia coli.
[0157] It can be seen from the test results in Table 1 that the heat-insulating and warm-keeping composite fabric prepared by the present invention has an antibacterial effect, excellent heat-insulating performance, and can store energy and regulate temperature, and has a lasting heat-storing and warm-keeping effect.
[0158] By preparing an organic quaternary ammonium salt antibacterial agent, the antibacterial agent is grafted and compounded with nano zirconium carbide as a carrier through chemical bonds, which can not only improve the dispersibility of nano zirconium carbide, but also improve the stability of the antibacterial agent, making it less likely to migrate, and the obtained antibacterial functionalized nano zirconium carbide has long-lasting antibacterial and light-absorbing and heat-generating functions; by preparing modified cotton fibers with antibacterial functions and modified hollow polyester fibers with amino groups, the two are spun and woven, and the obtained modified hollow polyester / cotton fabric is impregnated with an antibacterial finishing agent, and the unreacted epoxy groups on the surface of the antibacterial functionalized nano zirconium carbide in the antibacterial finishing agent can further undergo a ring-opening reaction with the active groups on the surface of the modified hollow polyester / cotton fabric during the impregnation process, thereby firmly attaching the organic antibacterial component and the inorganic carrier nano zirconium carbide to the surface of the fabric, and the obtained inner and outer fabrics not only have long-lasting antibacterial properties, but also have long-lasting heat storage and warmth-keeping effects.
[0159] The middle layer material is made by vacuum impregnation of modified cellulose aerogel with flexibility and hydrophobicity and phase change material eicosane. The inner layer fabric, the middle layer material and the outer layer fabric are compounded to obtain a heat-insulating and warm composite fabric; among them, the modified cellulose aerogel has better flexibility while having low density and low thermal conductivity. Using it as a thermal insulation interlayer of the composite fabric can effectively improve the thermal insulation and warmth-keeping ability of the fabric. Specifically, in the thermal insulation performance test, the side of the composite fabric away from the heating platform is the upper surface, and the side of the composite fabric in contact with the heating platform is the lower surface. During the heating process, the temperature of the upper surface of the composite fabric is always lower than the temperature of the lower surface of the composite fabric. There is a temperature difference between the two. The greater the temperature difference, the better the thermal insulation performance of the fabric. Because the middle layer material contains phase change material, when the outer layer fabric and the inner layer fabric absorb light and generate heat, and the ambient temperature is higher than the phase change temperature of the phase change material, the middle layer material can first absorb and store the heat. When the ambient temperature drops below the phase change temperature, the middle layer material will slowly release the stored energy to achieve the effect of energy storage, temperature regulation, heating and warmth preservation.
[0160] In Comparative Example 1, no intermediate layer material is added, and the modified cellulose aerogel and phase change material eicosane in the intermediate layer material are lacking in improving the heat insulation and warmth retention of the composite fabric and the energy storage and temperature regulation capabilities. Therefore, the warmth retention rate, thermal enthalpy value, and temperature difference in Comparative Example 1 are all lower than those in the embodiment;
[0161] In Comparative Example 2, the surface of the nano-zirconium carbide was not modified using an epoxy silane coupling agent, no ring-opening reaction occurred between the nano-zirconium carbide and the antibacterial agent, the binding ability of the nano-zirconium carbide, the antibacterial agent and the fabric decreased, and the antibacterial performance of the fabric decreased after washing.
[0162] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a heat-insulating and warm-keeping composite fabric, characterized in that: The following steps are involved: Step 1: Prepare the inner layer fabric, outer layer fabric, and middle layer material respectively; The modified hollow polyester fiber is spun into yarn as warp yarn, and the modified cotton fiber is spun into yarn as weft yarn, and the yarns are woven to obtain a modified hollow polyester / cotton fabric; The modified hollow polyester / cotton fabric is impregnated in an antibacterial finishing agent, and after the impregnation, the fabric is baked and dried to obtain an inner layer fabric and an outer layer fabric respectively; Wherein, the antibacterial finishing agent is prepared by the following steps: The dodecyl dimethyl tertiary amine and 3-bromo-1-propanol are mixed and reacted, and after the reaction is completed, the mixture is washed, filtered, and the filter cake is taken and dried to obtain an antibacterial agent; the epoxy nano zirconium carbide, the antibacterial agent, and isopropanol are mixed and reacted, and after the reaction is completed, the mixture is filtered and washed to obtain an antibacterial functionalized nano zirconium carbide; the antibacterial functionalized nano zirconium carbide is mixed with water to obtain an antibacterial finishing agent; Heat eicosane until it melts, immerse the modified cellulose aerogel in the eicosane, and take it out after the immersion is completed to obtain an intermediate layer material; The modified cellulose aerogel is prepared by the following steps: The cellulose acetate is dissolved in an organic solvent, and a blocked isocyanate is added to obtain a modified cellulose spinning solution; and the modified cellulose spinning solution is treated by an electrospinning technique to obtain a modified cellulose nanofiber membrane; The modified cellulose nanofiber membrane is treated in an aqueous environment and freeze-dried to obtain a modified cellulose aerogel after reaction; Step 2: Compound the inner layer fabric, the middle layer material and the surface layer fabric to obtain a heat-insulating and warm composite fabric.
2. The method for preparing a heat-insulating and warm-keeping composite fabric according to claim 1, characterized in that: In the step 1, the modified cotton fiber and the modified hollow polyester fiber are prepared by the following steps: Cotton fiber, carboxymethyl chitosan, L-arginine and water are mixed, immersed, taken out after the immersion, reacted, and dried after the reaction to obtain modified cotton fiber; hollow polyester fiber, 1,6-hexanediamine and water are mixed, immersed, reacted, taken out after the reaction, washed to neutrality, and dried to obtain modified hollow polyester fiber; Among them, the mass ratio of cotton fiber, carboxymethyl chitosan, L-arginine and water is 10:0.3-0.4:0.3-0.4:150-180; when preparing modified cotton fiber, the impregnation conditions are: impregnation at room temperature for 2-3 hours, and the reaction conditions are: reaction at 170-180°C for 3-4 minutes; the mass ratio of hollow polyester fiber, 1,6-hexanediamine and water is 10:1.5-1.8:150-180; when preparing modified hollow polyester fiber, the impregnation conditions are: impregnation at 60-70°C for 40-60 minutes, and the reaction conditions are: reaction at 150-160°C for 10-15 minutes.
3. The method for preparing a heat-insulating and warm-keeping composite fabric according to claim 1, characterized in that: In the step 1, the yarn count of the modified hollow polyester fiber is 40-60S in British standard; the yarn count of the modified cotton fiber is 40-60S in British standard; the gram weight of the modified hollow polyester / cotton fabric is 120-140g / m 2 The bath ratio of the modified hollow polyester / cotton fabric to the antibacterial finishing agent is 1:10-15; the dipping operation is: dipping at room temperature for 20-30 minutes, double dipping and double rolling, and the rolling rate is 78-82%; the baking conditions are: baking at 100-120°C for 3-5 minutes.
4. The method for preparing a heat-insulating and warm-keeping composite fabric according to claim 1, characterized in that: In the preparation of the antibacterial finishing agent in step 1, the epoxy nano zirconium carbide is prepared by the following steps: Mixing an ethanol aqueous solution with 3-(2,3-epoxypropoxy)propyltrimethoxysilane, adding a regulator to adjust the pH value, adding nano zirconium carbide, ultrasonically dispersing, reacting, and after the reaction is completed, filtering, washing, and drying to obtain epoxy nano zirconium carbide; The mass ratio of ethanol aqueous solution, 3-(2,3-epoxypropoxy)propyltrimethoxysilane and nano zirconium carbide is 100:6-8:1-1.5, and the ethanol aqueous solution is 50 vol% ethanol aqueous solution; the reaction conditions are: reacting at a pH value of 4-4.5 and a temperature of 55-65° C. for 2-3 hours.
5. The method for preparing a heat-insulating and warm-keeping composite fabric according to claim 1, characterized in that: In the preparation of the antibacterial finishing agent in step 1, the mass ratio of dodecyldimethyl tertiary amine to 3-bromo-1-propanol is 2-2.1:1.4-1.6; when preparing the antibacterial agent, the reaction conditions are: reacting at a temperature of 60-70°C for 12-14h; the mass ratio of epoxy nano-zirconium carbide, antibacterial agent, and isopropanol is 1-1.2:1:80-100; when preparing antibacterial functionalized nano-zirconium carbide, the reaction conditions are: reacting at a temperature of 70-80°C for 3-4h; the mass ratio of antibacterial functionalized nano-zirconium carbide to water is 1:40-50.
6. The method for preparing a heat-insulating and warm-keeping composite fabric according to claim 1, characterized in that: In the step 1, the solid-liquid ratio of the modified cellulose aerogel to eicosane is 1:4-5; the impregnation conditions are: vacuum impregnation at a temperature of 40-45° C. for 30-40 hours; and the thickness of the intermediate layer material is 0.3-0.4 mm.
7. The method for preparing a heat-insulating and warm-keeping composite fabric according to claim 1, characterized in that: In the preparation of the modified cellulose aerogel in step 1, the blocked isocyanate is prepared by the following steps: The isocyanate prepolymer is mixed with amino nano-silica, and reacted. After the reaction is completed, octafluoropentanol is added to continue the reaction. After the reaction is completed, imidazole is added to react again. After the reaction is completed, the mixture is cooled to obtain a blocked isocyanate. Among them, the mass ratio of isocyanate prepolymer, octafluoropentanol, amino nano-silica and imidazole is 30:3.9-4:1.8-2:5-6; the reaction conditions are: react for 1-2 hours in a nitrogen atmosphere at a temperature of 55-65°C; the continued reaction conditions are: continue to react for 2-3 hours in a nitrogen atmosphere at a temperature of 70-75°C; the second reaction conditions are: react again for 3-4 hours in a nitrogen atmosphere at a temperature of 50-60°C.
8. The method for preparing a heat-insulating and warm-keeping composite fabric according to claim 1, characterized in that: In the step 1, the modified cellulose aerogel is prepared by the following steps: Mixing cellulose acetate, acetone and N,N-dimethylformamide, stirring until completely dissolved, standing, adding blocked isocyanate and mixing evenly to obtain a modified cellulose spinning solution; injecting the modified cellulose spinning solution into a syringe of an electrospinning device, spinning through the electrospinning instrument, and drying after spinning to obtain a modified cellulose nanofiber membrane; The modified cellulose nanofiber film is sheared and crushed, water is added, and the dispersion is homogeneously dispersed to obtain a modified cellulose nanofiber dispersion, and the dispersion is freeze-dried, and after drying, the dispersion is reacted to obtain a modified cellulose aerogel; The mass ratio of cellulose acetate, acetone, N,N-dimethylformamide and blocked isocyanate is 10:28-30:28-30:8-10; in the electrospinning operation, the propulsion speed of the modified cellulose spinning solution is 1.0 ml / h, the spinning voltage is 20 kV, and the distance from the spinning needle to the receiving screen is 15 cm; the receiving screen of the electrospinning is aluminum foil; The mass ratio of the modified cellulose nanofiber membrane to water is 1:15-18; the freeze-drying operation includes: freezing the modified cellulose nanofiber dispersion at -80°C for 4-4.5 hours, and then freeze-drying it in a freeze dryer at -80°C and 0.5Pa for 45-48 hours; the reaction conditions are: reacting at 140-150°C for 4-5 hours.
9. A thermal insulation and thermal insulation composite fabric prepared by the method for preparing a thermal insulation and thermal insulation composite fabric as claimed in any one of claims 1 to 8.
10. Use of the heat-insulating and warm-keeping composite fabric according to claim 9 in clothing.