Preparation method of activated carbon, activated carbon and wastewater treatment method

By using tea powder, coffee powder and organic adhesives in the preparation of activated carbon, and impregnating tea polyphenols and caffeine during the activation process, the problem of insufficient strength and adsorption capacity of activated carbon in water treatment is solved, and efficient pollution is achieved Production process for material removal and environmental protection.

CN118949937APending Publication Date: 2024-11-15成都达奇科技股份有限公司

Patent Information

Application Number
CN202411442221.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing activated carbon has poor strength and adsorption capacity in water treatment, and binders such as asphalt and coal tar used in traditional preparation processes lead to high energy consumption and difficult to clean up equipment pollution.

Method used

Use tea powder and/or coffee powder as additives, combined with low-cost and easy-to-get organic adhesives, and prepare activated carbon by ball milling, extrusion molding and activation treatment, and impregnate tea polyphenols and caffeine in the modified solution to enhance adsorption ability.

Benefits of technology

It significantly improves the compressive strength and adsorption capacity of activated carbon, reduces energy consumption, reduces production costs, and enhances the removal effect of heavy metals, organic and inorganic pollutants.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of activated carbon, discloses a preparation method of activated carbon, activated carbon and a wastewater treatment method, and solves the technical problems of poor strength and adsorption capacity of activated carbon in the prior art. The preparation method of the activated carbon comprises the following steps: ball-milling and mixing tea powder and / or coffee powder, a primary carbonized material and a first adhesive solution to obtain a mixture; carrying out ball-milling mixing on the mixture, reinforced resin powder and a second adhesive solution, and then carrying out extrusion molding to obtain a pressed blank; activating the pressed blank to obtain an activated material; the activated material is soaked in a modified solution, filtering and drying treatment are conducted after soaking is completed, and activated carbon is obtained; the modified solution contains a first active component, and the first active component is tea polyphenol and / or caffeine; wherein the flowability of the first adhesive is 20 to 50 mPa * s; and the bonding strength of the second adhesive solution is 1.5 to 3.5 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of activated carbon, and in particular to a method for preparing activated carbon, activated carbon and a method for treating wastewater. Background Art

[0002] With the development of material technology, activated carbon materials are widely used in various fields such as air treatment, water purification, and active carriers. The conventional preparation process of biomass activated carbon is: carbonize the biomass raw material once, then mix and knead the primary carbonized material with additives such as a binder, and then extrude it into shape, and then perform secondary carbonization and activation to obtain biomass activated carbon. Among them, the binder used is usually asphalt or coal tar. Direct activation after extrusion molding will produce oily substances that affect the performance of activated carbon. Only after secondary carbonization can the production of oily substances be reduced. At the same time, a large amount of organic substances such as benzene, naphthalene, and anthracene that overflow during the calcination of tar or asphalt will also coke on the inner wall of the equipment, causing instrument contamination that is difficult to clean. Therefore, it is generally subjected to secondary carbonization before activation to protect the activation equipment. However, secondary carbonization will significantly increase energy consumption and reduce production efficiency. In addition, the use process of coal tar is relatively cumbersome. It not only requires heating and softening, but also requires a large amount of addition and high cost.

[0003] The Chinese invention patent with the patent number ZL202311749749.1, owned by the applicant of this application, discloses a method for preparing activated carbon and activated carbon. It no longer uses oily substances such as asphalt and coal tar as adhesives, but uses low-cost, easily available, and environmentally friendly organic adhesives. The adhesive used does not produce oily substances and harmful gases during the activation process, and there is no need for secondary carbonization treatment. After extrusion molding and drying, it can be directly activated to obtain activated carbon, which significantly reduces energy consumption and is environmentally friendly. However, the applicant found in practice that the strength and adsorption capacity of the activated carbon still need to be further improved when used in water treatment. Summary of the invention

[0004] The main purpose of the present invention is to provide a method for preparing activated carbon, activated carbon and a wastewater treatment method, so as to solve the technical problems of poor strength and adsorption capacity of activated carbon in the prior art.

[0005] In order to achieve the above object, according to the first aspect of the present invention, a method for preparing activated carbon is provided, and the technical scheme is as follows: The method for preparing activated carbon comprises the following steps: ball-milling tea powder and / or coffee powder, primary carbonized material and first adhesive solution to obtain a mixed material; The mixed material, the reinforcing resin powder and the second binder solution are ball-milled and then extruded to obtain a compact; Performing activation treatment on the pressed green sheet to obtain an activated material; The activated material is immersed in a modified solution, and after the immersion is completed, it is filtered and dried to obtain activated carbon; the modified solution contains a first active component, and the first active component is tea polyphenols and / or caffeine; The fluidity of the first adhesive is 20-50 mPa·s; and the bonding strength of the second adhesive solution is 1.5-3.5 MPa.

[0006] As a further improvement of the above-mentioned method for preparing activated carbon: the first adhesive solution contains at least one of sodium carboxymethyl cellulose, polyethylene oxide, hydroxypropyl methylcellulose, methyl cellulose, hydroxyethyl cellulose, gum arabic, and xanthan gum; 200 to 400 mL of the first adhesive solution is added to every 1 kg of the carbonized material.

[0007] As a further improvement of the above-mentioned method for preparing activated carbon: the second adhesive solution contains at least one of syrup, starch paste, polyvinyl alcohol, chitosan, white latex, and dextrin; 100 to 300 mL of the second adhesive solution is added to every 1 kg of the mixture.

[0008] As a further improvement of the above-mentioned activated carbon preparation method: the amount of the tea powder and / or coffee powder used is 2-7% of the amount of the primary carbonized material; the particle size of the tea powder and / or coffee powder is 50-200nm; the primary carbonized material is obtained by carbonizing the biomass raw material at 500-600℃ for 1-2h and then grinding and sieving.

[0009] As a further improvement of the above-mentioned activated carbon preparation method: the reinforcing resin powder is at least one of phenolic resin, polyvinyl acetate, cyanoacrylate, polyurethane resin, epoxy resin, acrylic resin, polystyrene resin, polyetheretherketone resin, polypropylene resin, and modified polyester resin; the amount of the reinforcing resin powder is 1 to 3% of the amount of the mixture.

[0010] As a further improvement of the above-mentioned method for preparing activated carbon: the activation treatment is to activate the pressed green sheet in a water vapor atmosphere at 800-950° C. for 2-3 hours.

[0011] As a further improvement of the above-mentioned method for preparing activated carbon: the mass of the first active component in the modified solution is 1 to 2% of the mass of the activated material; the activated material is immersed in the modified solution for 12 to 24 hours using an equal volume impregnation method; the modified solution also contains a second active component, which is a flavonoid compound or a glycoside of a flavonoid compound.

[0012] As a further improvement of the above-mentioned activated carbon preparation method: the second active component is at least one of luteolin, quercetin, quercetin, isoquercetin, naringin, rutin, baicalin, and flavonol; the mass of the second active component in the modified solution is 1 to 2% of the mass of the activated material.

[0013] In order to achieve the above object, according to a second aspect of the present invention, activated carbon is provided, and the technical scheme is as follows: The activated carbon is prepared by the preparation method described in the first aspect above.

[0014] In order to achieve the above object, according to the third aspect of the present invention, a wastewater treatment method is provided, and the technical scheme is as follows: The wastewater treatment method comprises the steps of: using the preparation method described in the first aspect above to prepare activated carbon to adsorb at least one of heavy metal ions, organic pollutants and inorganic pollutants in the wastewater.

[0015] The activated carbon preparation method, activated carbon and wastewater treatment method of the present invention have the following advantages: (1) The applicant has found that in the process of preparing activated carbon, the fluidity and bonding strength of the adhesive solution are two key parameters that will significantly affect the quality and performance of the final activated carbon. The study found that when the fluidity of the first adhesive solution is high, it can ensure that it can fully penetrate and coat the tea powder and / or coffee powder and the primary carbonized material to form a uniform mixture, which is particularly important for the strength of the activated carbon; at the same time, when the bonding strength of the second adhesive solution is high, it can ensure that a green body with sufficient mechanical strength is formed during the green pressing process, thereby ensuring the strength of the final activated material. Therefore, the present invention significantly improves the compressive strength of the activated material by improving the fluidity and bonding strength of the first adhesive solution and the second adhesive solution.

[0016] (2) The present invention adds tea powder and / or coffee powder to the carbon raw material, preferably waste residue powder, to reduce solid waste and improve resource utilization. Tea powder and / or coffee powder are rich in cellulose, minerals, trace elements and organic compounds, which can form more complex and diverse pore structures and a large number of oxygen-containing functional groups (such as carboxyl, hydroxyl, phenolic hydroxyl, etc.) during the activation process. The complex and diverse pore structure is conducive to the subsequent loading of active components. A large number of oxygen-containing functional groups form active sites, which can improve the hydrophilicity and adsorption capacity of activated carbon, and can retain certain bioactive components such as tea polyphenols and caffeine. These bioactive components have antioxidant and antibacterial properties, which can give activated carbon additional functional properties.

[0017] (3) The present invention further impregnates the modified solution containing tea polyphenols and / or caffeine after activation.

[0018] Tea polyphenols have multiple phenolic hydroxyl groups, which can form stable complexes with heavy metal ions and enhance the adsorption capacity of heavy metal ions; tea polyphenols are rich in aromatic rings and phenolic hydroxyl groups, and can effectively adsorb organic pollutants such as polycyclic aromatic hydrocarbons, phenolic compounds and dyes through π-π interactions and hydrogen bonds; the phenolic hydroxyl groups and other polar groups in tea polyphenols can combine with inorganic ions (such as nitrate and phosphate) through hydrogen bonds and ion exchange to achieve the removal of total nitrogen and total phosphorus.

[0019] Caffeine contains multiple nitrogen atoms (such as amide and imidazole structures), which can form coordination bonds with heavy metal ions, increasing the adsorption capacity for heavy metal ions; the aromatic ring and nitrogen heterocyclic structure of caffeine can interact with organic pollutants through π-π stacking and hydrogen bonding, thereby improving the adsorption effect on organic pollutants; caffeine contains multiple polar groups, which can undergo ion exchange and hydrogen bonding with inorganic ions, thereby improving the removal effect of inorganic pollutants.

[0020] When the raw materials contain tea powder and / or coffee powder, other undecomposed components in tea and coffee may produce a synergistic effect with tea polyphenols and caffeine, thereby increasing the loading intensity of active components and enhancing the overall antioxidant and antibacterial properties.

[0021] (4) The present invention also adds reinforcing resin powder to the green body, which can improve the mechanical strength of the activated carbon material and make it more resistant to wear and breakage during use; the reinforced resin powder can improve the molding properties of the mixture, provide better adhesion and plasticity during the extrusion molding process, and enable the pressed green body to be molded more evenly and stably; in the subsequent high-temperature activation treatment process, the reinforced resin powder can improve the thermal stability of the green body and reduce the damage to the material structure caused by high-temperature treatment, thereby maintaining the structural integrity and pore structure richness of the activated carbon; the reinforced resin powder may also have certain chemical components that can form a more stable combination with active components such as tea polyphenols and / or caffeine, thereby improving the adsorption stability of the final activated carbon.

[0022] It can be seen that the activated carbon preparation method, activated carbon and wastewater treatment method of the present invention provide an activated carbon with high strength, good adsorption capacity and very suitable for wastewater purification, as well as its preparation method and application, which effectively solves the technical problems of poor strength and adsorption capacity of activated carbon in the prior art.

[0023] The following is a further explanation of the embodiments of the invention provided in this specification through specific implementation methods. Additional aspects and advantages of the embodiments of the invention provided in this specification will be partially given in the following description, partially become apparent from the following description, or be understood through the practice of the embodiments of the invention provided in this specification. DETAILED DESCRIPTION

[0024] The following is a clear and complete description of the embodiments of the inventions provided in this specification. A person of ordinary skill in the art will be able to implement the embodiments of the inventions provided in this specification based on these descriptions. Before describing the embodiments of the inventions provided in this specification, it should be particularly noted that: The technical solutions and technical features provided in each part of the embodiments of the invention provided in this specification, including the following description, may be combined with each other if there is no conflict.

[0025] In addition, the embodiments of the inventions provided in this specification involved in the following descriptions are generally only part of the embodiments of the inventions provided in this specification rather than all of the embodiments. Therefore, based on the embodiments of the inventions provided in this specification, all other embodiments obtained by ordinary technicians in this field without making any creative work should fall within the scope of protection of the embodiments of the inventions provided in this specification.

[0026] Regarding the terms and units in the embodiments of the inventions provided in this specification: The terms "including", "comprising", "having" and any variations thereof in the descriptions and claims of the embodiments of the inventions provided in this specification and in the related parts are intended to cover non-exclusive inclusions. In addition, other relevant terms and units in the embodiments of the inventions provided in this specification can be reasonably interpreted based on the relevant contents of the embodiments of the inventions provided in this specification.

[0027] Example 1: Activated carbon and its preparation method include the following steps: Tea powder, coffee powder, primary carbonized material and first adhesive solution are ball-milled to obtain a mixture. The first adhesive is a hydroxypropyl methylcellulose solution with a fluidity of 40 mPa·s. 300 mL of the first adhesive solution is added to every 1 kg of the primary carbonized material. The total amount of tea powder and coffee powder is 6% of the amount of the primary carbonized material. The mass of the tea powder and coffee powder is equal, and the particle size of the tea powder and coffee powder is 50 to 200 nm. The primary carbonized material is obtained by grinding and sieving bamboo after carbonizing at 550°C for 2 hours without oxygen.

[0028] The mixed material, the reinforcing resin powder and the second adhesive solution are ball-milled and mixed, and then extruded to obtain a compact. The second adhesive solution is a chitosan solution with a bonding strength of 2.5 MPa; 200 mL of the second adhesive solution is added to every 1 kg of the mixed material. The reinforcing resin powder is a phenolic resin, and its amount is 2% of the amount of the mixed material.

[0029] The pressed green body was activated in a steam atmosphere at 900°C for 2 hours to obtain an activated material.

[0030] The activated material is immersed in the modified solution, and after the immersion is completed, it is filtered and dried to obtain activated carbon. The modified solution contains a first active component and a second active component; the first active component is tea polyphenols and caffeine, and the total mass of the first active component is 1% of the mass of the activated material, and the mass of tea polyphenols and caffeine is equal; the second active component is an ethanol solution of quercetin and quercetin, and the total mass of the second active component is 1% of the mass of the activated material, and the mass of quercetin and quercetin is equal. The activated material is immersed in the modified solution for 12 hours using an equal volume impregnation method.

[0031] The test showed that the compressive strength of the activated carbon was 273N / cm and the iodine value was 1004mg / g.

[0032] Example 2: Activated carbon and its preparation method include the following steps: Tea powder, coffee powder, primary carbonized material and first adhesive solution are ball-milled and mixed to obtain a mixture. The first adhesive is a gum arabic solution with a fluidity of 20 mPa·s, and 300 mL of the first adhesive solution is added to every 1 kg of primary carbonized material. The total amount of tea powder and coffee powder is 7% of the amount of primary carbonized material, the mass of tea powder and coffee powder is equal, and the particle size of tea powder and coffee powder is 50 to 200 nm. The primary carbonized material is obtained by grinding and sieving bamboo after anaerobic carbonization at 550°C for 2 hours.

[0033] The mixed material, the reinforcing resin powder and the second adhesive solution are ball-milled and mixed, and then extruded to obtain a compact. The second adhesive solution is a polyvinyl alcohol solution with a bonding strength of 3 MPa; 200 mL of the second adhesive solution is added to every 1 kg of the mixed material. The reinforcing resin powder is a polyurethane resin, and its amount is 2% of the amount of the mixed material.

[0034] The pressed green body was activated in a steam atmosphere at 900°C for 2 hours to obtain an activated material.

[0035] The activated material is immersed in the modified solution, and after the immersion is completed, it is filtered and dried to obtain activated carbon. The modified solution contains a first active component and a second active component; the first active component is tea polyphenols and caffeine, and the total mass of the first active component is 1% of the mass of the activated material, and the mass of tea polyphenols and caffeine is equal; the second active component is an ethanol solution of quercetin and quercetin, and the total mass of the second active component is 1% of the mass of the activated material, and the mass of quercetin and quercetin is equal. The activated material is immersed in the modified solution for 12 hours using an equal volume impregnation method.

[0036] The test showed that the compressive strength of the activated carbon was 266N / cm and the iodine value was 1020mg / g.

[0037] Example 3: Activated carbon and its preparation method include the following steps: Tea powder, coffee powder, primary carbonized material and first adhesive solution are ball-milled and mixed to obtain a mixture. The first adhesive is a xanthan gum solution with a fluidity of 50 mPa·s, and 300 mL of the first adhesive solution is added to every 1 kg of the primary carbonized material. The total amount of tea powder and coffee powder is 2% of the amount of the primary carbonized material, the mass of the tea powder and the coffee powder are equal, and the particle size of the tea powder and the coffee powder is 50 to 200 nm. The primary carbonized material is obtained by grinding and sieving bamboo after anaerobic carbonization at 550°C for 2 hours.

[0038] The mixed material, the reinforcing resin powder and the second adhesive solution are ball-milled and mixed, and then extruded to obtain a compact. The second adhesive solution is a white latex solution with a bonding strength of 3.5 MPa; 200 mL of the second adhesive solution is added to every 1 kg of the mixed material. The reinforcing resin powder is an epoxy resin, and its amount is 1% of the amount of the mixed material.

[0039] The pressed green body was activated in a steam atmosphere at 900°C for 2 hours to obtain an activated material.

[0040] The activated material is immersed in the modified solution, and after the immersion is completed, it is filtered and dried to obtain activated carbon. The modified solution contains a first active component and a second active component; the first active component is tea polyphenols and caffeine, and the total mass of the first active component is 1% of the mass of the activated material, and the mass of tea polyphenols and caffeine is equal; the second active component is an ethanol solution of rutin and baicalin, and the total mass of the second active component is 1% of the mass of the activated material, and the mass of rutin and baicalin is equal. The activated material is immersed in the modified solution for 12 hours using the equal volume immersion method.

[0041] The test showed that the compressive strength of the activated carbon was 264N / cm and the iodine value was 1042mg / g.

[0042] Example 4: Activated carbon and its preparation method include the following steps: The tea powder, coffee powder, primary carbonized material and the first adhesive solution are ball-milled to obtain a mixture. The first adhesive is a sodium carboxymethyl cellulose solution with a fluidity of 30 mPa·s. 300 mL of the first adhesive solution is added to every 1 kg of the primary carbonized material. The total amount of tea powder and coffee powder is 4% of the amount of the primary carbonized material. The mass of the tea powder and the coffee powder is equal, and the particle size of the tea powder and the coffee powder is 50 to 200 nm. The primary carbonized material is obtained by grinding and sieving bamboo after carbonizing at 550°C for 2 hours without oxygen.

[0043] The mixed material, the reinforcing resin powder and the second adhesive solution are ball-milled and mixed, and then extruded to obtain a compact. The second adhesive solution is a polyvinyl alcohol solution with a bonding strength of 3 MPa; 200 mL of the second adhesive solution is added to every 1 kg of the mixed material. The reinforcing resin powder is a phenolic resin, and its amount is 2% of the amount of the mixed material.

[0044] The pressed green body was activated in a steam atmosphere at 900°C for 2 hours to obtain an activated material.

[0045] The activated material is immersed in the modified solution, and after the immersion is completed, it is filtered and dried to obtain activated carbon. The modified solution contains a first active component and a second active component; the first active component is tea polyphenols and caffeine, and the total mass of the first active component is 1% of the mass of the activated material, and the mass of tea polyphenols and caffeine is equal; the second active component is an ethanol solution of rutin and baicalin, and the total mass of the second active component is 1% of the mass of the activated material, and the mass of rutin and baicalin is equal. The activated material is immersed in the modified solution for 12 hours using the equal volume immersion method.

[0046] The test showed that the compressive strength of the activated carbon was 277N / cm and the iodine value was 986mg / g.

[0047] Example 5: Activated carbon and its preparation method include the following steps: The tea powder, coffee powder, primary carbonized material and the first adhesive solution are ball-milled to obtain a mixture. The first adhesive is a sodium carboxymethyl cellulose solution with a fluidity of 30 mPa·s. 300 mL of the first adhesive solution is added to every 1 kg of the primary carbonized material. The total amount of tea powder and coffee powder is 5% of the amount of the primary carbonized material. The mass of the tea powder and the coffee powder is equal, and the particle size of the tea powder and the coffee powder is 50 to 200 nm. The primary carbonized material is obtained by grinding and sieving bamboo after anaerobic carbonization at 550°C for 2 hours.

[0048] The mixed material, the reinforcing resin powder and the second adhesive solution are ball-milled and mixed, and then extruded to obtain a compact. The second adhesive solution is a sugarcane molasses solution with a bonding strength of 1.5 MPa; 200 mL of the second adhesive solution is added to every 1 kg of the mixed material. The reinforcing resin powder is an acrylic resin, and its amount is 3% of the amount of the mixed material.

[0049] The pressed green body was activated in a steam atmosphere at 900°C for 2 hours to obtain an activated material.

[0050] The activated material is immersed in the modified solution, and after the immersion is completed, it is filtered and dried to obtain activated carbon. The modified solution contains a first active component, the first active component is tea polyphenols and caffeine, the total mass of the first active component is 1% of the mass of the activated material, and the mass of tea polyphenols and caffeine is equal. The activated material is immersed in the modified solution for 12 hours using an equal volume immersion method.

[0051] The test showed that the compressive strength of the activated carbon was 261N / cm and the iodine value was 1090mg / g.

[0052] Example 6: Activated carbon and its preparation method include the following steps: The tea powder, the primary carbonized material and the first adhesive solution are ball-milled to obtain a mixture. The first adhesive is a hydroxyethyl cellulose solution with a fluidity of 30 mPa·s, and 300 mL of the first adhesive solution is added to every 1 kg of the primary carbonized material. The amount of tea powder used is 3% of the amount of the primary carbonized material, and the particle size of the tea powder is 50 to 200 nm. The primary carbonized material is obtained by grinding and sieving bamboo after carbonizing at 550°C for 2 hours without oxygen.

[0053] The mixed material, the reinforcing resin powder and the second adhesive solution are ball-milled and mixed, and then extruded to obtain a compact. The second adhesive solution is a dextrin solution with a bonding strength of 2 MPa; 200 mL of the second adhesive solution is added to every 1 kg of the mixed material. The reinforcing resin powder is a polystyrene resin, and its amount is 2% of the amount of the mixed material.

[0054] The pressed green body was activated in a steam atmosphere at 900°C for 2 hours to obtain an activated material.

[0055] The activated material is immersed in the modified solution, and after the immersion is completed, it is filtered and dried to obtain activated carbon. The modified solution contains a first active component and a second active component; the first active component is tea polyphenols, and the total mass of the first active component is 1% of the mass of the activated material; the second active component is an ethanol solution of luteolin and naringin, and the total mass of the second active component is 1% of the mass of the activated material, and the masses of luteolin and naringin are equal. The activated material is immersed in the modified solution for 12 hours using an equal volume impregnation method.

[0056] The test showed that the compressive strength of the activated carbon was 262N / cm and the iodine value was 1066mg / g.

[0057] Example 7: Activated carbon and its preparation method include the following steps: The coffee powder, the primary carbonized material and the first adhesive solution are ball-milled to obtain a mixture. The first adhesive is a hydroxyethyl cellulose solution with a fluidity of 30 mPa·s, and 300 mL of the first adhesive solution is added to every 1 kg of the primary carbonized material. The amount of coffee powder used is 5% of the amount of the primary carbonized material, and the particle size of the coffee powder is 50 to 200 nm. The primary carbonized material is obtained by grinding and sieving bamboo after carbonizing at 550°C for 2 hours without oxygen.

[0058] The mixed material, the reinforcing resin powder and the second adhesive solution are ball-milled and mixed, and then extruded to obtain a compact. The second adhesive solution is a starch paste solution with a bonding strength of 2MPa; 200mL of the second adhesive solution is added to every 1kg of the mixed material. The reinforcing resin powder is a polypropylene resin, and its amount is 3% of the amount of the mixed material.

[0059] The pressed green body was activated in a steam atmosphere at 900°C for 2 hours to obtain an activated material.

[0060] The activated material is immersed in the modified solution, filtered and dried after the immersion is completed, and activated carbon is obtained. The modified solution contains a first active component and a second active component; the first active component is caffeine, and the total mass of the first active component is 1% of the mass of the activated material; the second active component is an ethanol solution of luteolin and naringin, and the total mass of the second active component is 1% of the mass of the activated material, and the masses of luteolin and naringin are equal. The activated material is immersed in the modified solution for 12 hours using an equal volume impregnation method.

[0061] The test showed that the compressive strength of the activated carbon was 259N / cm and the iodine value was 1160mg / g.

[0062] The embodiment of the wastewater treatment method of the present invention is to prepare activated carbon adsorbing at least one of heavy metal ions, organic pollutants and inorganic pollutants in wastewater by the preparation method described in any one of the above embodiments. It has been verified that 1L of sewage mixture from the secondary sedimentation tank of a sewage treatment plant is taken in a beaker, 1g of activated carbon is added to the beaker, and the mixture is filtered after magnetic stirring for 30 minutes. The removal rates of COD, total nitrogen and total phosphorus are all above 93% after testing, and no heavy metal ions are detected in the filtrate.

[0063] Comparative Example 1: Compared with Example 4, the activated carbon and its preparation method in this comparative example are different in that tea powder and coffee powder are not used. The compressive strength of the activated carbon obtained by testing is 279N / cm, and the iodine value is 971mg / g.

[0064] Comparative Example 2: Compared with Example 4, the difference between the activated carbon and its preparation method in this comparative example is that no modification solution is used for impregnation modification. The compressive strength of the activated carbon obtained by testing is 277N / cm, and the iodine value is 941mg / g.

[0065] Comparative Example 3: Compared with Example 4, the activated carbon and its preparation method in this comparative example are different in that no reinforcing resin powder is used. The compressive strength of the activated carbon obtained by testing is 251 N / cm, and the iodine value is 981 mg / g.

[0066] Comparative Example 4: Compared with Example 2, the activated carbon and its preparation method in this comparative example are different in that the first adhesive is a gum arabic solution with a fluidity of 15 mPa·s. The compressive strength of the activated carbon obtained by testing is 253 N / cm, and the iodine value is 1012 mg / g.

[0067] Comparative Example 5: Compared with Example 3, the activated carbon and its preparation method in this comparative example have the following differences: the first adhesive is a polyethylene oxide solution with a fluidity of 55 mPa·s. The compressive strength of the activated carbon obtained by testing is 246 N / cm, and the iodine value is 973 mg / g.

[0068] Comparative Example 6: Compared with Example 5, the activated carbon and its preparation method in this comparative example have the following differences: the second adhesive solution is a sugarcane molasses solution, and the bonding strength is 1.2 MPa. The compressive strength of the activated carbon obtained by testing is 241 N / cm, and the iodine value is 999 mg / g.

[0069] Comparative Example 7: Compared with Example 3, the activated carbon and its preparation method in this comparative example have the following differences: the second adhesive solution is a white latex solution, and the bonding strength is 3.7 MPa. The compressive strength of the activated carbon obtained by testing is 275 N / cm, and the iodine value is 985 mg / g.

[0070] In the above embodiment, the tea powder is prepared by heating tea leaves at 100° C. for 12 hours, grinding the tea leaves into fine powder, and sieving the tea leaves through 250-mesh and 500-mesh sieves. The coffee powder is prepared by roasting coffee beans at 200° C. for 12 hours, grinding the coffee beans into fine powder, and sieving the coffee beans through 250-mesh and 500-mesh sieves.

[0071] Flavonoids are a class of polyphenolic compounds with diverse structures and functions. They can introduce groups such as hydroxyl (-OH), carboxyl (-COOH), amino (-NH2), thiol (-SH), and sulfonic acid (-SO3H). Flavonoids such as quercetin, rutin, luteolin, and baicalin usually have good complexing ability, especially by introducing polar groups such as hydroxyl, carboxyl, and amino groups, which can enhance the adsorption effect of heavy metal ions such as lead, cadmium, mercury, copper, and zinc. Flavonoids such as quercetin, luteolin, baicalin, and flavonols have good adsorption effects on organic pollutants such as polycyclic aromatic hydrocarbons (PAHs), phenolic compounds, dyes, and pesticide residues through π-π interactions, hydrogen bonds, and hydrophobic interactions. For inorganic pollutants (such as nitrates and phosphates), flavonoids such as quercetin, isoquercetin, naringin, and rutin can achieve adsorption through ion exchange and complexation.

[0072] The fluidity of the adhesive is tested using the "Method for Determination of Viscosity of Adhesives" (GB / T 2794-2022). The higher the viscosity value, the lower the fluidity.

[0073] The bonding strength of the adhesive is tested using the "Determination of tensile shear strength of adhesives (rigid material to rigid material)" (GB / T 7124-2008). The greater the tensile shear strength value, the greater the bonding strength.

[0074] The compressive strength is tested using the "Test method for wood activated carbon - Determination of strength" (GB / T12496.6-1999).

[0075] The iodine value test is carried out according to the "Test method for wood activated carbon - Determination of iodine adsorption value" (GB / T12496.8-1999).

[0076] COD is chemical oxygen demand, which refers to the amount of reducing substances that need to be oxidized in a water sample measured by chemical methods. It is tested using the "Determination of Chemical Oxygen Demand of Water Quality - Dichromate Method" (GB 11914-1989).

[0077] Total nitrogen, abbreviated as TN, is the total amount of various forms of inorganic and organic nitrogen in water. It is tested using the "Water Quality - Determination of Total Nitrogen - Acid Digestion Ultraviolet Spectrophotometry" (GB 11894-89).

[0078] Total phosphorus, referred to as TP, is the result of converting various forms of phosphorus into orthophosphate after digestion of water samples. It is tested using the "Determination of Total Phosphorus in Water - Ammonium Molybdate Spectrophotometry" (GB 11893-89).

[0079] The above is a description of the relevant contents of the embodiments of the inventions provided in this specification. Based on these descriptions, a person of ordinary skill in the art will be able to implement the embodiments of the inventions provided in this specification. Based on the above contents of the embodiments of the inventions provided in this specification, all other preferred implementations and embodiments obtained by a person of ordinary skill in the art without making any creative work shall fall within the scope of protection of the embodiments of the inventions provided in this specification.

Claims

1. Preparation method of activated carbon, Features: The following steps are involved: ball-milling tea powder and / or coffee powder, primary carbonized material and first adhesive solution to obtain a mixed material; The mixed material, the reinforcing resin powder and the second binder solution are ball-milled and then extruded to obtain a compact; Performing activation treatment on the pressed green sheet to obtain an activated material; The activated material is impregnated in the modified solution, and after the impregnation is completed, it is filtered and dried to obtain activated carbon; The modified solution contains a first active component, and the first active component is tea polyphenols and / or caffeine; The fluidity of the first adhesive is 20-50 mPa·s; and the bonding strength of the second adhesive solution is 1.5-3.5 MPa.

2. The method for preparing activated carbon according to claim 1, Features: The first adhesive solution contains at least one of sodium carboxymethyl cellulose, polyethylene oxide, hydroxypropyl methyl cellulose, methyl cellulose, hydroxyethyl cellulose, gum arabic and xanthan gum; 200-400 mL of the first adhesive solution is added to every 1 kg of the primary carbonized material.

3. The method for preparing activated carbon according to claim 1, Features: The second adhesive solution contains at least one of syrup, starch paste, polyvinyl alcohol, chitosan, white latex and dextrin; 100-300 mL of the second adhesive solution is added to every 1 kg of the mixture.

4. The method for preparing activated carbon according to claim 1, Features: The amount of the tea powder and / or coffee powder is 2-7% of the amount of the primary carbonized material; the particle size of the tea powder and / or coffee powder is 50-200nm; the primary carbonized material is obtained by grinding and sieving the biomass raw material after carbonizing it at 500-600℃ for 1-2h in anoxic state.

5. The method for preparing activated carbon according to claim 1, Features: The reinforcing resin powder is at least one of phenolic resin, polyvinyl acetate, cyanoacrylate, polyurethane resin, epoxy resin, acrylic resin, polystyrene resin, polyetheretherketone resin, polypropylene resin, and modified polyester resin; the amount of the reinforcing resin powder is 1 to 3% of the amount of the mixture.

6. The method for preparing activated carbon according to claim 5, Features: The activation treatment is to activate the compact in a water vapor atmosphere at 800-950° C. for 2-3 hours.

7. The method for preparing activated carbon according to claim 1, Features: The mass of the first active component in the modified solution is 1-2% of the mass of the activated material; the activated material is immersed in the modified solution for 12-24 hours by an equal volume immersion method; The modified solution also contains a second active component, which is a flavonoid compound or a glycoside of a flavonoid compound.

8. The method for preparing activated carbon according to claim 7, Features: The second active component is at least one of luteolin, quercetin, quercetin, isoquercetin, naringin, rutin, baicalin, and flavonols; the mass of the second active component in the modified solution is 1-2% of the mass of the activated material.

9. Activated carbon, Features: The compound is prepared by the preparation method according to any one of claims 1 to 8.

10. Wastewater treatment methods, Features: The method comprises the steps of: using the preparation method described in any one of claims 1 to 8 to prepare activated carbon for adsorbing at least one of heavy metal ions, organic pollutants and inorganic pollutants in wastewater.

Citation Information

Patent Citations

  • Metal ion adsorption sewage separation membrane preparation method

    CN108404686A

  • Sulfydryl modified coffee residue adsorbent as well as preparation method and application thereof

    CN116870874A

  • Tea extract modified activated carbon material as well as preparation method and application thereof

    CN117101608A

  • Preparation method of activated carbon and activated carbon

    CN117416957A

  • Tea-based kitchen waste malodorous gas deodorant and preparation method thereof

    CN117680089A

Cited By

  • Application of baicalin in relieving copper toxicity of duckweed

    CN121948655A