Silica gel-coated porous ceramic-based composite phase change heat storage material and preparation method thereof
The silica gel-coated porous ceramic-based composite phase change heat storage material addresses the limitations of existing materials by enhancing mechanical strength and thermal conductivity, ensuring stable phase change performance and reducing heating energy consumption in building applications.
Patent Information
- Application Number
- CN202411173628.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
Existing capsule composite phase change materials are not suitable for building material preparation due to low strength and poor thermal conductivity, affecting mechanical strength and heat storage efficiency.
A silica gel-coated porous ceramic-based composite phase change heat storage material is prepared using a vacuum adsorption method to fully absorb phase change material, followed by silica sol encapsulation, utilizing high-temperature roasting to enhance mechanical strength and thermal conductivity.
The material achieves high thermal conductivity, excellent corrosion resistance, and stable phase change performance, reducing building heating energy consumption and improving living comfort by replacing fine or coarse aggregate in building mortar.
Smart Images

Figure CN119059752A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of energy-saving heat storage material preparation, and in particular to a silica gel-wrapped porous ceramic-based composite phase-change heat storage material and a preparation method thereof. Background Art
[0002] According to statistics, my country's building energy consumption accounts for about 1 / 3 of the total social energy consumption, and urban heating in northern China also consumes a lot of coal, accounting for about 15% to 20% of my country's non-power generation coal consumption. Building energy consumption mainly refers to energy consumption in heating, air conditioning, hot water supply, cooking, lighting, household appliances, elevators, ventilation, etc., of which heating and air conditioning account for about 65%. However, my country's current power supply is still dominated by thermal power generation, which requires the burning and consumption of a large amount of non-renewable fossil fuels every year, which not only brings expensive production costs, but also aggravates a series of environmental problems, such as urban haze, greenhouse effect, and glacier melting. Therefore, vigorously developing green building energy-saving materials, reducing heating energy consumption, reducing residents' heating costs, and improving housing comfort are of great significance to my country's economic and social development.
[0003] Phase change heat storage materials store and release heat by utilizing the endothermic and exothermic effects associated with the phase change process of materials. There are four types of phase change methods: solid-solid, solid-liquid, solid-gas, and liquid-gas. Among them, solid-liquid phase change materials are considered to be the most promising type of phase change materials for industrial applications due to their advantages such as high phase change latent heat, small volume and pressure changes, and the phase change process can be maintained at an almost constant temperature (hereinafter referred to as solid-liquid phase change materials). According to the different phase change temperatures, phase change materials can be divided into low temperature (<150°C) and high temperature (>150°C), which are suitable for different application scenarios. Among them, low-temperature phase change materials, especially phase change materials with a phase change temperature range of 20-60°C, can help regulate indoor temperature and reduce heating electricity consumption by combining with building materials, and have great application prospects. However, since low-temperature phase change materials are generally paraffin-based organic matter or inorganic water and salt materials, if they are directly combined with building mortar or concrete building materials, both of them will seriously affect the strength of the building. Therefore, it is usually necessary to wrap a corrosion-resistant and stable protective shell on the outside of the phase change material to avoid leakage. For example, Chinese patent 201210181586.7 uses a mini-emulsion polymerization method to prepare phase change microcapsules with polystyrene and polymethyl methacrylate as wall materials and inorganic hydrated salt phase change materials as core materials; Chinese patent 202311364556.4 uses styrene-butadiene-styrene copolymer as capsule wall material and paraffin as capsule core material to prepare a paraffin-based phase change material coated microcapsule. The capsule wall can effectively inhibit the volatilization of the core material paraffin, thereby ensuring that the microcapsule has good heat storage performance and heat storage stability. However, the wall materials of the above-mentioned various capsule-coated composite phase change heat storage materials are mostly made of polymer materials, which have the disadvantages of easy aging, easy corrosion, and large thermal resistance, resulting in slow heat storage / heat release speed, affecting the heat storage efficiency. In addition, there are many domestic patent documents reporting new inventions using inorganic materials as shell materials, such as Chinese patent 202111588436.3, which uses a sol-gel method to prepare silica-encapsulated paraffin phase change nano-microcapsules with silica as wall material and paraffin as core material. The shell material is non-degradable and has good wear resistance and fire resistance; Chinese patent 201510338460.X uses saturated crystalline hydrated salt as phase change material and silica as shell material to prepare microcapsule composite phase change material, which has the advantages of good sealing.
[0004] Although there are many reports on capsule composite phase change materials at home and abroad, they are generally not suitable for use in the field of building material preparation. Both organic and inorganic material shells have disadvantages such as low strength and poor thermal conductivity. When used as building material raw materials, they have an adverse effect on the mechanical strength of the building, and the heat storage efficiency is low. For this reason, we proposed a silica gel-wrapped porous ceramic-based composite phase change heat storage material and its preparation method. Summary of the invention
[0005] The technical problem to be solved by the present invention is that the existing capsule composite phase change materials are generally not suitable for use in the field of building material preparation. Whether it is an organic or inorganic material shell, it has the disadvantages of low strength and poor thermal conductivity. When used as a building material raw material, it has an adverse effect on the mechanical strength of the building, and the heat storage efficiency is low. A silica gel-coated porous ceramic-based composite phase change heat storage material and a preparation method thereof are proposed, which provide a silica gel-coated porous ceramic-based composite phase change heat storage material with high strength and excellent corrosion resistance and a preparation method thereof. The composite phase change material first adopts a vacuum adsorption method to ensure that the porous ceramic ball matrix fully adsorbs the phase change material, and then further encapsulates and seals it with silica sol as a wall material, which can avoid the seepage of the phase change material during the melting / solidification process. Since the porous ceramic ball is made by high-temperature roasting, it has excellent mechanical strength and high thermal conductivity, and can be used as an admixture to replace fine aggregate or coarse aggregate in part of the building mortar. When it serves as a mortar raw material in the process of floor heating laying, it can improve the thermal conductivity of the floor heating material, reduce the set temperature of the floor heating water pipe, reduce heating energy consumption, and improve living comfort.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing a silica gel-coated porous ceramic-based composite phase-change heat storage material, the preparation method comprising the following steps:
[0008] S1, preparing raw materials consisting of fly ash, high-alumina bauxite, clay minerals, binders, and pore-forming agents, wherein the mass ratios of the fly ash, high-alumina bauxite, clay minerals, and binders are 20%-60%, 20%-70%, 10%-20%, and 2%-5%, respectively, and the amount of the pore-forming agent added is 20%-30% of the sum of the above four;
[0009] S2, batching, mixing and balling the raw materials consisting of fly ash, high-alumina bauxite, clay minerals, binders and pore-forming agents to obtain green balls, and then drying and calcining to obtain porous ceramic balls;
[0010] S3, placing the porous ceramic ball and excess phase change material into a vacuum container, then evacuating the container until the vacuum degree is lower than -0.1MPa, and after the vacuum degree is stable, placing it in an oven and heating it to a temperature 10-20°C higher than the melting point of the phase change material to ensure that it is completely melted and becomes liquid, and then slowly opening the vacuum valve to allow air to slowly enter the container until the vacuum degree is 0, and after cooling and solidification, taking out the ceramsite, placing it on a sieve, placing it in an oven and heating it to a temperature 10°C higher than the melting point of the phase change material, and keeping it warm for 12 hours, removing the excess phase change material adhering to the ceramic surface, and obtaining a ceramic ball with a dry surface;
[0011] S4, using sodium silicate as a silicon source, dissolving it in water to form a 0.5 mol / L sodium silicate solution, slowly adding hydrochloric acid until the pH value of the solution stabilizes between 5 and 6, fully stirring to obtain silica sol, and completely immersing the dried ceramic balls obtained in S3 in the prepared silica sol, then taking them out and shaking off the excess sol on the surface, placing them on a drying rack and drying them in an oven at 60°C for 12 hours to obtain the finished product.
[0012] Preferably, the clay minerals include: kaolin, montmorillonite, hydromica, chlorite, etc., and kaolin is most preferred. Kaolin is a common clay mineral in nature, has good plasticity, has been widely used in the field of ceramic production, and has low cost. The amount of pore former added is 20-30% of the sum of the above four. The larger the amount of pore former added, the more pores are produced, and more phase change materials can be adsorbed, but the mechanical strength is weaker. Therefore, according to the strength requirements of the use scenario, the amount of pore former added should be controlled not to be too high.
[0013] Preferably, in S1, the binder is at least one of bentonite, slaked lime, sodium silicate, tetraethyl orthosilicate, and polyvinyl alcohol. The binder is most preferably bentonite, mainly because bentonite is a natural mineral and has a low-cost advantage over commercial reagents. Bentonite has been promoted and used as a pelletizing binder in the field of iron and steel metallurgy for several years. Moreover, the use of bentonite not only helps to improve the strength of the ceramic body, but also can be used as a high-temperature binder to improve the strength of the ceramic after firing; the pore-forming agent is at least one of starch, graphite powder, and coal powder. The particle size of the pore-forming agent is less than 45 microns, and coal powder is most preferably used. Coal powder is cheap and easy to obtain, and can be used after simple fine grinding with a particle size of less than 45 microns. The smaller the particle size of the pore-forming agent, the smaller the diameter of the pores produced, the greater the capillary force, the stronger the adsorption capacity for phase change materials, and the lower the risk of leakage.
[0014] Preferably, in S2, the pelletizing is performed using a disc pelletizing machine or a cylinder pelletizing machine, and a disc pelletizing machine is most preferred, which is convenient for observing and adjusting the pelletizing process. About 10% of water is sprayed during the pelletizing process, and the diameter of the obtained green pellets is greater than 3 mm.
[0015] Preferably, in S2, the calcination conditions are: heating rate 2-5°C / min, calcination temperature 1300-1400°C, calcination time 120-300min, and calcination atmosphere is air atmosphere. During the calcination process, the heating rate should not be too fast to prevent the pore-forming agent from burning violently and producing a large amount of gas overflow in a short time, causing the ceramic to crack. If the calcination temperature is too low, the amount of liquid phase generated in the ceramic is low, which will lead to poor connection between particles, poor strength of the ceramic and easy powdering. If the calcination temperature is higher than 1400°C, the amount of ceramic liquid phase generated is too much, and it is easy to deform and collapse.
[0016] Preferably, in S3, the phase change material is an organic phase change material or an inorganic phase change material, wherein the organic phase change material is at least one of paraffin, polyethylene glycol, n-heptadecane, and n-octadecane, and the inorganic phase change material is at least one of Mn(NO3)2·6H2O, CaCl·6H2O, Na2SO4·10H2O, Na2S2O3·5H2O, and MgCl2·4H2O, and the paraffin has different melting points from low to high according to the number of carbon atoms from small to large, and the melting point range is about 20-60°C. The inorganic phase change material is various hydrated salts with different melting points. When a plurality of hydrated salts are mixed and used, a low eutectic hydrated salt phase change material with a melting point range of 20-60°C can be obtained.
[0017] The present invention also proposes a silica gel coated porous ceramic-based composite phase change heat storage material, which is a silica gel coated porous ceramic-based composite phase change heat storage material prepared according to the above-mentioned silica gel coated porous ceramic-based composite phase change heat storage material preparation method.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. The silica gel-coated porous ceramic-based composite phase change heat storage material and its preparation method provided by the technical solution of the present invention utilize typical bulk industrial solid waste fly ash as the main raw material, the raw material cost is extremely low, and the preparation process is simple, and has industrial application prospects.
[0020] 2. The silica gel-coated porous ceramic-based composite phase change heat storage material and its preparation method provided by the technical solution of the present invention utilize high-temperature roasting solid-phase reaction to realize the phase transformation of fly ash and the solidification of harmful substances, and at the same time realize the resource utilization of industrial solid waste to obtain high-performance porous ceramic matrix materials. In the high-temperature solid-phase reaction process, the mineral phase in the fly ash can be transformed to obtain a mineral phase mainly composed of mullite, corundum, and calcium feldspar, among which mullite and corundum have high thermal conductivity and mechanical strength. Therefore, the prepared porous ceramic material exhibits excellent compressive strength and heat transfer performance, and has good compatibility with phase change materials. It can utilize the rich porous structure to adsorb phase change materials to prevent leakage during the phase change process.
[0021] 3. The silica gel-wrapped porous ceramic-based composite phase change heat storage material provided by the technical solution of the present invention not only uses porous ceramic balls as the phase change material matrix to reduce its leakage, but also adds silica gel for secondary sealing treatment, which greatly reduces the risk of phase change material leakage. Moreover, the composite material has a uniform appearance and a stable shape. There is no leakage of phase change material during the phase change process, and the phase change heat storage material can maintain its original shape. It can undergo multiple thermal cycles and has good thermal stability, phase change latent heat and phase change temperature stability. The spherical appearance, size and strength make it suitable for partially replacing fine aggregate or coarse aggregate in building mortar, which is of great benefit to reducing building heating energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The DSC curve of Example 1 of a silica gel-coated porous ceramic-based composite phase-change heat storage material and a preparation method thereof proposed in the present invention;
[0023] Figure 2 The DSC curve of the comparative example 1 of the silica gel-wrapped porous ceramic-based composite phase-change heat storage material and the preparation method thereof proposed in the present invention;
[0024] Figure 3 This is the DSC curve of comparative example 2 of a silica gel-coated porous ceramic-based composite phase-change heat storage material and a preparation method thereof proposed in the present invention. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0026] In the following examples and comparative examples:
[0027] The main components of fly ash (in terms of oxides) are: Al2O3 34.3%, SiO2 54.5%, MgO 0.5%, CaO 3.8%, Na2O+K2O 0.3%, etc.
[0028] The main components of high-alumina bauxite (in terms of oxides) are: Al2O3 is 68.5%, SiO2 is 10.7%, MgO is 0.2%, CaO is 0.1%, Fe2O3 is 1.3%, TiO2 is 3.1%, Na2O+K2O is 0.6%, etc.
[0029] The main components of kaolin (in terms of oxides): Al2O3 is 36.1%, SiO2 is 47.2%, MgO is 0.1%, CaO is 0.2%, Fe2O3 is 0.6%, TiO2 is 0.6%, etc.
[0030] The coal powder is anthracite powder with an ash content of less than 10%.
[0031] Example 1
[0032] The fly ash, high-alumina bauxite, kaolin, bentonite and coal powder were mixed in the ratio of 40:45:10:5:20, and the mixture was mixed and ground in a planetary ball mill at a speed of 300 rpm for 2 hours. Then, a disc ball making machine was used to roll the obtained mixture into small balls with a diameter of about 10 mm. Then, the green balls were placed in a drying oven and kept at 105°C for 12 hours. The dried balls were placed in a muffle furnace and slowly heated to 1350°C at 2°C / min in an air atmosphere and kept warm for 180 minutes to obtain porous ceramic balls. Then, the balls were naturally cooled to room temperature and taken out. The porous ceramic balls and excess paraffin were put into a suction flask, evacuated to -0.1MPa and then the vacuum valve was closed. The balls were placed in a drying oven and heated to 80°C. After keeping warm for 2 hours, the vacuum valve was slowly opened to let air enter the suction flask. After cooling, the balls were taken out, moved to the sieve, and put back into the drying oven and kept warm at 70°C for 12 hours. After cooling, ceramic balls saturated with paraffin were obtained. Subsequently, the ceramic balls were immersed in the prepared silica sol, soaked for 1 hour, taken out and the excess silica gel was shaken off, and then placed in a drying oven and kept warm at 60°C for 12 hours to obtain a silica gel-coated porous ceramic-based composite phase change heat storage material with a compressive strength greater than 3500N.
[0033] Sampling was carried out for DSC testing, and the results showed that the melting temperature was 49.5°C, the heat storage was 51.19 J / g, the solidification temperature was 39.7°C, and the heat release was 50.65 J / g. After 100 melting-solidification cycles, the melting temperature was 51.2°C, the heat storage was 50.32 J / g, the solidification temperature was 40.1°C, and the heat release was 49.77 J / g. The heat storage capacity remained above 98.3%, indicating that the product has excellent heat storage capacity and excellent stability, and can achieve temperature regulation in the range of 40-60°C.
[0034] Example 2
[0035] The fly ash, high-alumina bauxite, kaolin, bentonite and coal powder were mixed in the ratio of 40:45:10:5:30, and the mixture was mixed and ground in a planetary ball mill at a speed of 300 rpm for 2 hours. Then, a disc ball making machine was used to roll the obtained mixture into small balls with a diameter of about 15 mm. The green balls were placed in a drying oven and kept at 105°C for 12 hours. The dried balls were placed in a muffle furnace and slowly heated to 1350°C at 2°C / min in an air atmosphere and kept warm for 180 minutes to obtain porous ceramic balls. Then, the balls were naturally cooled to room temperature and taken out. The porous ceramic balls and excess paraffin were put into a suction flask, evacuated to -0.1MPa and then the vacuum valve was closed. The balls were placed in a drying oven and heated to 80°C. After keeping warm for 2 hours, the vacuum valve was slowly opened to let air enter the suction flask. After cooling, the balls were taken out, moved to the sieve, and put back into the drying oven and kept warm at 70°C for 12 hours. After cooling, ceramic balls saturated with paraffin were obtained. Subsequently, the ceramic balls were immersed in the prepared silica sol, soaked for 1 hour, taken out and the excess silica gel was shaken off, and then placed in a drying oven and kept warm at 60°C for 12 hours to obtain a silica gel-coated porous ceramic-based composite phase change heat storage material with a compressive strength greater than 4000N.
[0036] Sampling was carried out for DSC testing, and the results showed that the melting temperature was 49.60°C, the heat storage was 71.9 J / g, the solidification temperature was 40.1°C, and the heat release was 70.7 J / g. After 100 melting-solidification cycles, the melting temperature was 50.3°C, the heat storage was 70.21 J / g, the solidification temperature was 40.3°C, and the heat release was 69.08 J / g. The heat storage capacity remained above 97.5%.
[0037] Example 3
[0038] The fly ash, high-alumina bauxite, kaolin, bentonite and coal powder were mixed in a ratio of 60:20:15:5:20, and the mixture was mixed and ground in a planetary ball mill at a speed of 300 rpm for 2 hours. Then, a disc ball making machine was used to roll the obtained mixture into small balls with a diameter of about 20 mm. The green balls were placed in a drying oven and kept at 105°C for 12 hours. The dried balls were placed in a muffle furnace and slowly heated to 1300°C at 2°C / min in an air atmosphere and kept warm for 300 minutes to obtain porous ceramic balls. Then, the balls were naturally cooled to room temperature and taken out. The porous ceramic balls and excess paraffin were put into a suction flask, evacuated to -0.1MPa and then the vacuum valve was closed. The balls were placed in a drying oven and heated to 80°C. After keeping warm for 2 hours, the vacuum valve was slowly opened to let air enter the suction flask. After cooling, the balls were taken out, moved to the sieve, and put back into the drying oven and kept warm at 70°C for 12 hours. After cooling, ceramic balls saturated with paraffin were obtained. Subsequently, the ceramic balls were immersed in the prepared silica sol, soaked for 1 hour, taken out and the excess silica gel was shaken off, and then placed in a drying oven and kept warm at 60°C for 12 hours to obtain a silica gel-coated porous ceramic-based composite phase change heat storage material with a compressive strength greater than 3500N.
[0039] Sampling was carried out for DSC testing, and the results showed that the melting temperature was 50.1°C, the heat storage was 49.7 J / g, the solidification temperature was 41.1°C, and the heat release was 49.2 J / g. After 100 melting-solidification cycles, the melting temperature was 50.4°C, the heat storage was 48.21 J / g, the solidification temperature was 42.1°C, and the heat release was 47.87 J / g. The heat storage capacity remained above 97%.
[0040] Example 4
[0041] The fly ash, high alumina, kaolin, bentonite and coal powder were mixed in the ratio of 20:60:15:5:20, and the mixture was mixed and ground in a planetary ball mill at a speed of 300 rpm for 2 hours. Then, a disc ball making machine was used to roll the obtained mixture into small balls with a diameter of about 15 mm. Then, the green balls were placed in a drying oven and kept at 105°C for 12 hours. The dried balls were placed in a muffle furnace and slowly heated to 1400°C at 5°C / min in an air atmosphere and kept warm for 120 minutes to obtain porous ceramic balls. Then, the balls were naturally cooled to room temperature and taken out. The porous ceramic balls and excess paraffin were put into a suction flask, evacuated to -0.1MPa and then the vacuum valve was closed. The balls were placed in a drying oven and heated to 80°C. After keeping warm for 2 hours, the vacuum valve was slowly opened to let air enter the suction flask. After cooling, the balls were taken out, moved to the sieve, and put back into the drying oven and kept warm at 70°C for 12 hours. After cooling, ceramic balls saturated with paraffin were obtained. Subsequently, the ceramic balls were immersed in the prepared silica sol, soaked for 1 hour, taken out and the excess silica gel was shaken off, and then placed in a drying oven and kept warm at 60°C for 12 hours to obtain a silica gel-coated porous ceramic-based composite phase change heat storage material with a compressive strength greater than 4000N.
[0042] Sampling was carried out for DSC testing, and the results showed that the melting temperature was 50.5°C, the heat storage was 51.2 J / g, the solidification temperature was 39.7°C, and the heat release was 50.9 J / g. After 100 melting-solidification cycles, the melting temperature was 51.1°C, the heat storage was 49.77 J / g, the solidification temperature was 40.4°C, and the heat release was 49.39 J / g. The heat storage capacity remained above 97%.
[0043] Example 5
[0044] The fly ash, high-alumina bauxite, kaolin, bentonite and coal powder were mixed in the ratio of 20:58:20:2:30, and the mixture was mixed and ground in a planetary ball mill at a speed of 300 rpm for 2 hours. Then, a disc ball making machine was used to roll the obtained mixture into small balls with a diameter of about 15 mm. The green balls were placed in a drying oven and kept at 105°C for 12 hours. The dried balls were placed in a muffle furnace and slowly heated to 1400°C at 5°C / min in an air atmosphere and kept warm for 180 minutes to obtain porous ceramic balls. Then, the balls were naturally cooled to room temperature and taken out. The porous ceramic balls and excess paraffin were put into a suction flask, evacuated to -0.1MPa and then the vacuum valve was closed. The balls were placed in a drying oven and heated to 80°C. After keeping warm for 2 hours, the vacuum valve was slowly opened to let air enter the suction flask. After cooling, the balls were taken out, moved to the sieve, and put back into the drying oven and kept warm at 70°C for 12 hours. After cooling, ceramic balls saturated with paraffin were obtained. Subsequently, the ceramic balls were immersed in the prepared silica sol, soaked for 1 hour, taken out and the excess silica gel was shaken off, and then placed in a drying oven and kept warm at 60°C for 12 hours to obtain a silica gel-coated porous ceramic-based composite phase change heat storage material with a compressive strength greater than 4000N.
[0045] Sampling was carried out for DSC testing, and the results showed that the melting temperature was 50.7°C, the heat storage was 71.3 J / g, the solidification temperature was 40.4°C, and the heat release was 70.4 J / g. After 100 melting-solidification cycles, the melting temperature was 51.2°C, the heat storage was 69.75 J / g, the solidification temperature was 40.7°C, and the heat release was 68.68 J / g. The heat storage capacity remained above 97%.
[0046] The beneficial effects of the present technical solution are further described below by using a number of comparative examples with Example 1:
[0047] Comparative Example 1
[0048] The fly ash, high-alumina bauxite, kaolin, bentonite and coal powder were mixed in the ratio of 40:45:10:5:20, and the mixture was mixed and ground in a planetary ball mill at a speed of 300 rpm for 2 hours. Then, a disc ball making machine was used to roll the obtained mixture into small balls with a diameter of about 10 mm. Then, the green balls were placed in a drying oven and kept at 105°C for 12 hours. The dried balls were placed in a muffle furnace and slowly heated to 1350°C at 2°C / min in an air atmosphere and kept warm for 180 minutes to obtain porous ceramic balls. Then, the balls were naturally cooled to room temperature and taken out. The porous ceramic balls and excess paraffin were put into a suction flask, evacuated to -0.1MPa and then the vacuum valve was closed. The balls were placed in a drying oven and heated to 80°C. After keeping warm for 2 hours, the vacuum valve was slowly opened to let air enter the suction flask. After cooling, the balls were taken out, moved to the sieve, and put back into the drying oven and kept warm at 70°C for 12 hours. After cooling, ceramic balls saturated with paraffin were obtained.
[0049] Sampling was carried out for DSC testing, and the results showed that the melting temperature was 50.7°C, the heat storage was 50.72 J / g, the solidification temperature was 40.6°C, and the heat release was 50.16 J / g. After 100 melting-solidification cycles, the melting temperature was 51.4°C, the heat storage was 40.93 J / g, the solidification temperature was 41.1°C, and the heat release was 39.73 J / g. The heat storage capacity was only about 80.7%.
[0050] Compared with Example 1, the ceramic balls in this comparative example 1 were not subjected to the silica gel coating process. In this comparative example 1, the phase change material loss during the heat storage-release cycle was relatively large, indicating that significant leakage occurred. Not only did the heat storage capacity decrease, but the leaked phase change material would also corrode the building materials. This further illustrates that the silica gel coating process of the present invention can significantly improve the leakage problem that occurs when the phase change material is used for a long time.
[0051] Comparative Example 2
[0052] The fly ash, high-alumina bauxite, kaolin, bentonite and coal powder were mixed in the ratio of 40:45:10:5:10, and the mixture was mixed and ground in a planetary ball mill at a speed of 300 rpm for 2 h. The mixture was then rolled into small balls with a diameter of about 10 mm using a disc ball making machine. The green balls were then placed in a drying oven and kept at 105°C for 12 hours. The dried balls were placed in a muffle furnace and slowly heated to 1350°C at 2°C / min in an air atmosphere and kept warm for 180 minutes to obtain porous ceramic balls. The balls were then naturally cooled to room temperature and taken out. The porous ceramic balls and excess paraffin were placed in a suction flask, evacuated to -0.1 MPa and then the vacuum valve was closed. The balls were placed in a drying oven and heated to 80°C. After keeping warm for 2 hours, the vacuum valve was slowly opened to allow air to enter the suction flask. After cooling, the balls were taken out, moved to a sieve, and put back into the drying oven and kept warm at 70°C for 12 hours. After cooling, ceramic balls saturated with paraffin were obtained. Subsequently, the ceramic balls were immersed in the prepared silica sol, soaked for 1 hour, taken out and the excess silica gel was shaken off, and then placed in a drying oven and kept warm at 60°C for 12 hours to obtain a silica gel-coated porous ceramic-based composite phase change heat storage material.
[0053] The samples were taken for DSC testing, and the results showed that the melting temperature was 42.1°C, the heat storage was 8.60 J / g, the solidification temperature was 50.7°C, and the heat release was 8.13 J / g.
[0054] Compared with Example 1, the amount of coal powder (pore-forming agent) used in this comparative example 2 is lower. In this comparative example 2, the product quality is poor, indicating that too low an amount of pore-forming agent used will significantly reduce the penetration of the phase change material and the product has poor heat storage capacity.
[0055] Comparative Example 3
[0056] The fly ash, high alumina, kaolin, bentonite and coal powder were mixed in the ratio of 40:45:10:5:20, and the mixture was mixed and ground in a planetary ball mill at a speed of 300 rpm for 2 h. The mixture was then rolled into small balls with a diameter of about 10 mm using a disc ball making machine. The green balls were then placed in a drying oven and kept at 105°C for 12 hours. The dried balls were placed in a muffle furnace and slowly heated to 1250°C at 2°C / min in an air atmosphere and kept warm for 120 minutes to obtain porous ceramic balls. The balls were then naturally cooled to room temperature and taken out. The porous ceramic balls and excess paraffin were placed in a suction flask, evacuated to -0.1 MPa and then the vacuum valve was closed. The balls were placed in a drying oven and heated to 80°C. After keeping warm for 2 hours, the vacuum valve was slowly opened to allow air to enter the suction flask. After cooling, the balls were taken out, moved to a sieve, and put back into the drying oven and kept warm at 70°C for 12 hours. After cooling, ceramic balls saturated with paraffin were obtained. Subsequently, the ceramic balls were immersed in the prepared silica sol, soaked for 1 hour, taken out and the excess silica gel was shaken off, and then placed in a drying oven and kept warm at 60°C for 12 hours to obtain a silica gel-coated porous ceramic-based composite phase change heat storage material with a compressive strength of less than 2000N.
[0057] Compared with Example 1, in this comparative example 3, the calcination temperature is lower. In this comparative example 3, the compressive strength of the obtained silica gel-wrapped porous ceramic-based composite phase change heat storage material is lower than 2000N, indicating that the calcination temperature is too low, and the liquid phase content generated in the ceramic is too low to form a good connection with the powder particles, resulting in poor mechanical strength of the ceramic balls, which are prone to powder loss and breakage during transportation and use, affecting the heat storage performance.
[0058] It can be seen from the data of the above comparative examples that the silica gel-coated porous ceramic-based composite phase change heat storage material and its preparation method provided by the present technical solution utilize high-temperature roasting solid-phase reaction to achieve the phase transformation of fly ash and the solidification of harmful substances. Therefore, the prepared porous ceramic material exhibits excellent compressive strength and heat transfer performance, and has good compatibility with the phase change material. It can utilize the rich porous structure to adsorb the phase change material to prevent leakage during the phase change process. It also adds silica gel for secondary sealing treatment, which greatly reduces the risk of leakage of the phase change material. It has good thermal stability, phase change latent heat and phase change temperature stability.
[0059] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a silica gel-coated porous ceramic-based composite phase change thermal storage material, characterized in that: The preparation method comprises the following steps: S1, preparing raw materials consisting of fly ash, high-alumina bauxite, clay minerals, binders, and pore-forming agents, wherein the mass ratios of the fly ash, high-alumina bauxite, clay minerals, and binders are 20%-60%, 20%-70%, 10%-20%, and 2%-5%, respectively, and the amount of the pore-forming agent added is 20%-30% of the sum of the above four; S2, batching, mixing and balling the raw materials consisting of fly ash, high-alumina bauxite, clay minerals, binders and pore-forming agents to obtain green balls, and then drying and calcining to obtain porous ceramic balls; S3, placing the porous ceramic ball and excess phase change material into a vacuum container, then evacuating the container until the vacuum degree is lower than -0.1MPa, and after the vacuum degree is stable, placing it in an oven and heating it to a temperature 10-20°C higher than the melting point of the phase change material to ensure that it is completely melted and becomes liquid, and then slowly opening the vacuum valve to allow air to slowly enter the container until the vacuum degree is 0, and after cooling and solidification, taking out the ceramsite, placing it on a sieve, placing it in an oven and heating it to a temperature 10°C higher than the melting point of the phase change material, and keeping it warm for 12 hours, removing the excess phase change material adhering to the ceramic surface, and obtaining a ceramic ball with a dry surface; S4, using sodium silicate as a silicon source, dissolving it in water to form a 0.5 mol / L sodium silicate solution, slowly adding hydrochloric acid until the pH value of the solution stabilizes between 5 and 6, fully stirring to obtain silica sol, and completely immersing the dried ceramic balls obtained in S3 in the prepared silica sol, then taking them out and shaking off the excess sol on the surface, placing them on a drying rack and drying them in an oven at 60°C for 12 hours to obtain the finished product.
2. The method for preparing a silica gel-coated porous ceramic-based composite phase change thermal storage material according to claim 1, characterized in that: In S1, the binder is at least one of bentonite, slaked lime, sodium silicate, tetraethyl orthosilicate, and polyvinyl alcohol; the pore-forming agent is at least one of starch, graphite powder, and coal powder; and the particle size of the pore-forming agent is less than 45 microns.
3. The method for preparing a silica gel-coated porous ceramic-based composite phase change thermal storage material according to claim 1, characterized in that: In S2, the pelletizing is performed using a disc pelletizing machine, during which about 10% of water is sprayed and added, and the diameter of the obtained green pellets is greater than 3 mm.
4. The method for preparing a silica gel-coated porous ceramic-based composite phase change thermal storage material according to claim 1, characterized in that: In S2, the calcination conditions are: a heating rate of 2-5°C / min, a calcination temperature of 1300-1400°C, a calcination time of 120-300min, and an air atmosphere.
5. The method for preparing a silica gel-coated porous ceramic-based composite phase change thermal storage material according to claim 1, characterized in that: In S3, the phase change material is an organic phase change material or an inorganic phase change material, wherein the organic phase change material is at least one of paraffin, polyethylene glycol, n-heptadecane, and n-octadecane, and the inorganic phase change material is at least one of Mn(NO3)2·6H2O, CaCl·6H2O, Na2SO4·10H2O, Na2S2O3·5H2O, and MgCl2·4H2O.
6. The silica gel coated porous ceramic-based composite phase change heat storage material according to claim 1, characterized in that: The silica gel coated porous ceramic-based composite phase change heat storage material is a silica gel coated porous ceramic-based composite phase change heat storage material prepared according to the preparation method of the silica gel coated porous ceramic-based composite phase change heat storage material according to any one of claims 1 to 5.
Citation Information
Cited By
Heat storage lava solid particulate matter with good heat stability and preparation method of heat storage lava solid particulate matter
CN121450307A
Heat-stable hot-melt lava solid-state granular material and preparation method thereof
CN121450307B
Desert sand-based low-cost composite heat storage material as well as preparation method and application thereof
CN121801545A