Magnetic MOF composite materials for detecting fluoroquinolone antibiotics, preparation and detection methods

Through the use of magnetic MOF composite materials, the synergistic effect of lanthanide organic framework compounds and magnetic nanoparticle cores is achieved, and the low sensitivity and complexity of existing detection methods are solved. Improve detection efficiency and accuracy.

CN118671045BActive Publication Date: 2024-11-12INST OF QUALITY STANDARD & TESTING TECH FOR AGRO PROD OF CAAS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411118579.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-12
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The existing fluoroquinolones antibiotic detection methods have low sensitivity, complex detection methods and low detection efficiency, making it difficult to quickly and accurately evaluate food risks.

Method used

Magnetic MOF composite materials, including the shell of the lanthanide organic framework compound and the core of magnetic nanoparticles, are used to generate fluorescence responses through ultraviolet light excitation, achieving high sensitivity and visual detection.

Benefits of technology

The high-sensitive fluorescence response and visual detection of fluoroquinolone antibiotics are realized, which simplifies the detection methods, improves the detection efficiency, and can quickly and accurately detect fluoroquinolone antibiotics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118671045B_ABST
    Figure CN118671045B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of analytical chemistry, and relates to a magnetic MOF composite material for detecting fluoroquinolone antibiotics, and a preparation and detection method thereof. The composite material comprises an inner core and a shell layer coated on the surface of the inner core, wherein the shell layer comprises a lanthanide organic framework compound, wherein the organic ligand of the lanthanide organic framework compound is a benzoic acid compound having at least two carboxyl groups and a benzene ring structure, and the inner core is a magnetic nanoparticle. When the composite material is used to detect fluoroquinolone antibiotics, a highly sensitive fluorescence response can be achieved, visual detection can be achieved, and detection efficiency can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of analytical chemistry, and in particular, relates to a magnetic MOF composite material for detecting fluoroquinolone antibiotics, and a preparation and detection method thereof. Background Art

[0002] Antibiotics are widely used to treat infectious diseases worldwide and have a wide range of applications in animal husbandry and medicine. Among them, fluoroquinolone antibiotics (FQs) are widely used to treat a variety of Gram-positive and Gram-negative bacteria, and are therefore widely used in clinical medicine, farm animals, and aquaculture. However, their poor bioavailability and biodegradability lead to high residues in food, and these residues, as a type of food and environmental pollutants, pose a serious threat to human health and ecosystems. At the same time, my country, EU countries, the United States and other countries have stipulated maximum residue limits in edible animal tissues, eggs, milk and other foods. Therefore, establishing a simple, rapid and accurate detection method for fluoroquinolone antibiotics is of great significance for assessing food risks. However, the existing detection methods for fluoroquinolone antibiotics have low sensitivity, complex detection methods, and low detection efficiency.

[0003] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the existing detection methods of fluoroquinolone antibiotics, such as low sensitivity, complex detection methods and low detection efficiency, and to provide a magnetic MOF composite material, preparation and detection method for detecting fluoroquinolone antibiotics. When the magnetic MOF composite material is used to detect fluoroquinolone antibiotics, it can achieve highly sensitive fluorescence response and visual detection, and the detection method is simple and the detection efficiency is high.

[0005] In order to achieve the above-mentioned objectives, in a first aspect, the present invention provides a magnetic MOF composite material for fluorescence and visualization detection of fluoroquinolone antibiotics, comprising an inner core and a shell coated on the surface of the inner core, wherein the shell comprises a lanthanide organic framework compound, the organic ligand of the lanthanide organic framework compound is a benzoic acid compound having at least two carboxyl groups and a benzene ring structure, and the inner core is a magnetic nanoparticle.

[0006] In some preferred embodiments, the benzoic acid compound is selected from at least one of 4-(2,5-dicarboxyphenoxy)phthalic acid, 2-aminoterephthalic acid, isophthalic acid, 2,5-dihydroxyterephthalic acid, and trimesic acid; the lanthanide element is selected from at least one of lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium; and the magnetic nanoparticles are selected from at least one of ferroferric oxide nanoparticles and spinel ferrite nanoparticles.

[0007] Preferably, the benzoic acid compound includes 2-aminoterephthalic acid; the lanthanide element includes europium; and the magnetic nanoparticles include ferrosoferric oxide nanoparticles.

[0008] In some preferred embodiments, the shell layer has a porous structure and a uniform pore size, the average thickness and average pore size of the shell layer are 10 nm-50 nm and 5 nm-40 nm, respectively, and the average particle size of the core is 100 nm-500 nm.

[0009] In a second aspect, the present invention provides a method for preparing the magnetic MOF composite material described in the first aspect, preparing a lanthanide organic framework compound, wherein the organic ligand of the lanthanide organic framework compound is a benzoic acid compound having at least two carboxyl groups and a benzene ring structure, so that the lanthanide organic framework compound is coated on the surface of magnetic nanoparticles.

[0010] In some preferred embodiments, during the preparation of the lanthanide organic framework compound, the lanthanide is added in the form of lanthanide nitrate;

[0011] In the raw material composed of magnetic nanoparticles, benzoic acid compounds having at least two carboxyl groups and a benzene ring structure, and lanthanide nitrates, the mass ratio of the magnetic nanoparticles, the benzoic acid compounds, and the lanthanide nitrates is 1:(0.5-8):(1-5).

[0012] In some preferred embodiments, the magnetic nanoparticles are mixed with a benzoic acid compound having at least two carboxyl groups and a benzene ring structure and a lanthanide element as raw materials, and the magnetic MOF composite material is prepared in a one-step method by a first solvothermal reaction.

[0013] Preferably, the temperature of the first solvent thermal reaction is 80°C-180°C, and the time is 12h-72h.

[0014] Preferably, the first solvothermal reaction is carried out in a mixed solution of N'N-dimethylformamide and water, wherein the volume ratio of N'N-dimethylformamide to water in the mixed solution is 1:(0.5-2), and 30mL-100mL of the mixed solution is used for each gram of the magnetic nanoparticles.

[0015] In some preferred embodiments, the metal salt, the weak acid and strong base salt, and the polyol polymer are mixed in an alcohol solvent, and the magnetic nanoparticles are obtained through a second solvothermal reaction.

[0016] Preferably, the metal salt is anhydrous ferric chloride, the weak acid and strong base salt is anhydrous sodium acetate, the polyol polymer is polyethylene glycol, and the alcohol solvent is ethylene glycol;

[0017] When preparing the magnetic nanoparticles, anhydrous ferric chloride, anhydrous sodium acetate, and polyethylene glycol are mixed in a mass ratio of 1: (0.5-5): (0.1-1.5); the amount of ethylene glycol corresponding to each gram of anhydrous ferric chloride is 15mL-30mL, and the temperature of the second solvent thermal reaction is 160°C-220°C, and the time is 8h-24h.

[0018] In a third aspect, the present invention provides a method for detecting fluoroquinolone antibiotics, comprising: mixing the magnetic MOF composite material as described in the first aspect and / or the magnetic MOF composite material prepared by the preparation method as described in the second aspect with a substance to be tested to obtain a mixed solution, placing the mixed solution under an ultraviolet lamp and performing fluorescence measurement, and detecting fluoroquinolone antibiotics by color change and fluorescence response intensity.

[0019] In a fourth aspect, the present invention provides a method for detecting fluoroquinolone antibiotics, comprising: mixing the magnetic MOF composite material described in the first aspect and / or the magnetic MOF composite material prepared by the preparation method described in the second aspect, a substance to be tested and an indicator to obtain a mixed solution, and detecting the fluoroquinolone antibiotics by the color of the mixed solution.

[0020] The magnetic MOF composite material of the present invention comprises a core and a shell layer coated on the surface of the core, wherein the core is a magnetic nanoparticle, and the shell layer comprises a lanthanide organic framework compound whose organic ligand is a benzoic acid compound having at least two carboxyl groups and a benzene ring structure. Under ultraviolet light excitation, the charge carrier separation of the magnetic nanoparticles is enhanced, more electrons and holes are generated, and the fluoroquinolone antibiotic electrons absorb the excited energy and transfer from the ground state to the singlet excited state, and then the energy gap transitions from the singlet excited state to the triplet excited state. Finally, since the triplet excited state energy level of the fluoroquinolone antibiotic is higher than that of the lanthanide element, the magnetic nanoparticles are subjected to the ultraviolet light excitation. 5 D0 energy level, which enables electron transfer from antibiotics to lanthanides 5 D0 energy level and from 5D0 energy level to the ground state, and the hole structure generated in the magnetic nanoparticles is also conducive to the electron transfer of fluoroquinolone. Therefore, the presence of lanthanide elements in the magnetic nanoparticles and MOF shell can achieve a highly sensitive fluorescence response of fluoroquinolone antibiotics and promote the fluorescence excitation and sensing of fluoroquinolone antibiotics. The present invention improves the fluorescence response of fluoroquinolone antibiotics by introducing lanthanide elements, and selects benzoic acid compound organic ligands with good "antenna" effect and electron holes generated by magnetic nanoparticles to absorb photoelectrons, and forms a triplet state through a crossover process, which is conducive to breaking the 4F-4F taboo of lanthanide ions and forming a stronger emission than free ions. The luminescence of benzoic acid compound ligands occurs in a narrow blue or purple region with a wavelength, while photosensitive lanthanide elements, especially Eu 3+ Emission in the long-wavelength red region, the simultaneous use of benzoic acid compound ligands and lanthanide elements can achieve luminescence tuning. The organic ligands of the benzoic acid compounds of the present invention play a connecting role and are also sensitizers for lanthanide ions. Their different luminescence characteristics will lead to different responses. The sub-β-diketone structure based on fluoroquinolone antibiotics is excited to a higher excited state (π*←π) under excitation irradiation, and the β-diketone in the excited state is converted into a triplet state through intersystem cross-action, and then the relatively high triplet state transfers energy to the vibrational energy level of the lanthanide elements in the MOF. By using a lanthanide organic framework compound whose organic ligand is a benzoic acid compound having at least two carboxyl groups and a benzene ring structure, a highly sensitive fluorescence response can be further achieved.

[0021] With magnetic nanoparticles as the core and organic ligands such as lanthanide organic framework compounds of benzoic acid compounds with at least two carboxyl groups and a benzene ring structure as the shell, H2O2 obtains electrons from the surface of the composite material to form ·OH, and at the same time, the Fe in the magnetic nanoparticles 2+ / Fe 3+ Fenton reaction catalyzes H2O2 to form ·OH and ·O2 - , which helps the oxidation of TMB. At the same time, the flow of electrons from the MOF shell to Fe3O4 effectively promotes the 2+ / Fe 3+ Redox system, the composite material has an enzyme-like catalytic effect, which can realize the visual detection of fluoroquinolone antibiotics and improve the detection efficiency of fluoroquinolone antibiotics.

[0022] The method for detecting fluoroquinolone antibiotics by utilizing fluorescence response and color development reaction has the advantages of simple detection method and high detection efficiency.

[0023] The magnetic MOF composite material prepared by the preparation method of the present invention has a magnetic nanoparticle core and a lanthanide organic framework compound shell layer with a benzoic acid compound having at least two carboxyl groups and a benzene ring structure as an organic ligand coated on the surface of the core. With the magnetic nanoparticles inside and the ordered network structure formed by the lanthanide elements and the benzoic acid compounds outside, the synergistic effect of the lanthanide elements, the benzoic acid compounds and the magnetic nanoparticles is utilized to achieve a highly sensitive fluorescence response and an excellent enzyme-like catalytic effect, and further achieve highly sensitive fluorescence and visual detection. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0025] Figure 1 This is a microscopic morphology of the magnetic MOF composite material of Example 1 of the present invention.

[0026] Figure 2 This is a diagram showing the BET characterization results of the magnetic MOF composite material of Example 1 of the present invention.

[0027] Figure 3 This is the element distribution diagram of the magnetic MOF composite material of Example 1 of the present invention.

[0028] Figure 4 This is an elemental full scan spectrum of the X-ray photoelectron spectrum of the magnetic MOF composite material of Example 1 of the present invention.

[0029] Figure 5 This is a C 1s high-resolution spectrum of the X-ray photoelectron spectrum of the magnetic MOF composite material of Example 1 of the present invention.

[0030] Figure 6 This is the O 1s high-resolution spectrum of the X-ray photoelectron spectrum of the magnetic MOF composite material of Example 1 of the present invention.

[0031] Figure 7 This is the N 1s high-resolution spectrum of the X-ray photoelectron spectrum of the magnetic MOF composite material of Example 1 of the present invention.

[0032] Figure 8 This is the Eu 3d high-resolution spectrum of the X-ray photoelectron spectrum of the magnetic MOF composite material in Example 1 of the present invention.

[0033] Fig. 9This is a graph showing the change in fluorescence response intensity of ciprofloxacin detected by the magnetic MOF composite material according to Example 1 of the present invention as a function of ciprofloxacin concentration.

[0034] Fig.10 This is a graph showing the change in fluorescence response intensity of ofloxacin detected by the magnetic MOF composite material according to Example 1 of the present invention as a function of ofloxacin concentration.

[0035] Fig.11 This is a graph showing the change in fluorescence response intensity and color of fluoroquinolone antibiotics in visual detection of fluoroquinolone antibiotics using the magnetic MOF composite material according to Example 1 of the present invention. DETAILED DESCRIPTION

[0036] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0037] The inventors of the present invention have found through research that the existing detection methods for fluoroquinolone antibiotics have low sensitivity, complex detection methods and low detection efficiency.

[0038] In this regard, in the first aspect, the present invention provides a magnetic MOF composite material for fluorescence and visualization detection of fluoroquinolone antibiotics, comprising an inner core and a shell coated on the surface of the inner core, wherein the shell comprises a lanthanide organic framework compound, the organic ligand of the lanthanide organic framework compound is a benzoic acid compound having at least two carboxyl groups and a benzene ring structure, and the inner core is a magnetic nanoparticle.

[0039] The magnetic MOF composite material of the present invention comprises a core and a shell layer coated on the surface of the core, wherein the core is a magnetic nanoparticle, the shell layer comprises a lanthanide organic framework compound, and the ligand of the lanthanide organic framework compound is a benzoic acid compound having at least two carboxyl groups and a benzene ring structure. When detecting fluoroquinolone antibiotics, under ultraviolet light excitation, the charge carrier separation of the magnetic nanoparticles is enhanced, more electrons and holes are generated, and the fluoroquinolone antibiotic electrons absorb the excited energy and transfer from the ground state to the singlet excited state, and then from the singlet excited state to the triplet excited state through intersystem cross action. Finally, since the triplet excited state energy level of the fluoroquinolone antibiotic is higher than that of the lanthanide element, the magnetic nanoparticles are subjected to the ultraviolet light excitation. 5 D0 energy level, which enables electron transfer from antibiotics to lanthanides 5 D0 energy level and from 5At the same time, the hole structure generated in the magnetic nanoparticles is also conducive to the electron transfer of fluoroquinolone. Therefore, the presence of lanthanide elements in the magnetic nanoparticles and MOF shell can achieve a highly sensitive fluorescence response of fluoroquinolone antibiotics and promote the fluorescence excitation and sensing of fluoroquinolone antibiotics.

[0040] The electron holes generated by the benzoic acid organic ligands and magnetic nanoparticles with good "antenna" effect are used to absorb photoelectrons, and the triplet state is formed through the crossover process, which can break the 4F-4F taboo of lanthanide ions and form stronger emission than free ions. The luminescence of benzoic acid ligands occurs in the blue or purple region with a narrow wavelength, while the photosensitive lanthanide elements, especially Eu 3+ Emission in the long-wavelength red region, the simultaneous use of benzoic acid compound ligands and lanthanide elements can achieve luminescence tuning. The organic ligands of the benzoic acid compounds of the present invention not only play a connecting role, but also serve as sensitizers for lanthanide ions, and their different luminescence characteristics will lead to different responses. The sub-β-diketone structure based on fluoroquinolone antibiotics is excited to a higher excited state (π*←π) under excitation irradiation, and the β-diketone in the excited state is converted into a triplet state through intersystem cross-action, and then the relatively high triplet state transfers energy to the vibrational energy level of the lanthanide elements in the MOF. By using a lanthanide organic framework compound whose organic ligand is a benzoic acid compound having at least two carboxyl groups and a benzene ring structure, a highly sensitive fluorescence response can be further achieved.

[0041] With magnetic nanoparticles as the core and organic ligands such as lanthanide organic framework compounds of benzoic acid compounds with at least two carboxyl groups and a benzene ring structure as the shell, H2O2 obtains electrons from the surface of the composite material to form ·OH, and at the same time, the Fe in the magnetic nanoparticles 2+ / Fe 3+ Fenton reaction catalyzes H2O2 to form ·OH and ·O2 - , which helps the oxidation of TMB. At the same time, the flow of electrons from the MOF shell to Fe3O4 effectively promotes the 2+ / Fe 3+ Redox system, the composite material has excellent enzyme-like catalytic effect, specifically enzyme-like oxidation characteristics, which can effectively oxidize the indicator (chromogen reagent such as TMB), thereby forming a color reaction, which can realize the visual detection of fluoroquinolone antibiotics and improve the detection efficiency of fluoroquinolone antibiotics. The magnetic MOF composite material of the present invention can realize the rapid visual detection of fluoroquinolone antibiotics.

[0042] The magnetic MOF composite material of the present invention has a shell layer of a lanthanide organic framework compound of a benzoic acid compound having at least two carboxyl groups and a benzene ring structure, and uses lanthanide elements as hard acids to coordinate with hard bases such as carboxylic acid oxygen in organic functional ligands to form an ordered network structure that can stably coat the inner shell surface of magnetic nanoparticles, maintain the core-shell structure of the magnetic MOF composite material, and enable lanthanide elements, benzoic acid compounds, and magnetic nanoparticles to fully exert their synergistic effects to achieve highly sensitive fluorescence response and excellent enzyme-like catalytic effects, and further achieve highly sensitive fluorescence and visual detection. The present invention can effectively achieve rapid enrichment and separation of materials by combining magnetic materials with MOF materials, thereby increasing the reusability of materials.

[0043] The magnetic MOF nanocomposite material of the present invention has high fluorescence conversion efficiency and visualization effect, can effectively realize efficient and rapid analysis and detection of fluoroquinolone antibiotics, and provides new technology and materials for rapid analysis, detection and evaluation of fluoroquinolone antibiotics in food matrices.

[0044] The present invention does not limit the type of fluoroquinolone antibiotics, for example, it can be ciprofloxacin, ofloxacin, etc.

[0045] The present invention does not limit the organic ligand of the lanthanide organic framework compound, and the benzoic acid compound having at least two carboxyl groups and a benzene ring structure can be used, and the type of magnetic nanoparticles is also not limited. In some preferred embodiments, the benzoic acid compound is selected from at least one of 4-(2,5-dicarboxyphenoxy)phthalic acid, 2-aminoterephthalic acid, isophthalic acid, 2,5-dihydroxyterephthalic acid, and trimesic acid; the lanthanide element is selected from at least one of lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium; the magnetic nanoparticles are selected from at least one of ferroferric oxide nanoparticles and spinel ferrite nanoparticles, and the spinel ferrite nanoparticles include manganese ferrite nanoparticles and cobalt ferrite nanoparticles. In this preferred embodiment, the benzoic acid compound is selected from at least one of 4-(2,5-dicarboxyphenoxy)phthalic acid, 2-aminoterephthalic acid, isophthalic acid, 2,5-dihydroxyterephthalic acid, and trimesic acid, which can induce structural changes inside MOF, increase its porosity and stability, and be more conducive to the enrichment of fluoroquinolone antibiotics in the MOF shell and improve fluorescence response, thereby improving the sensitivity and accuracy of fluorescence detection. The magnetic nanoparticles are selected from at least one of ferroferric oxide nanoparticles, manganese ferrite nanoparticles, and cobalt ferrite nanoparticles, which can generate more electrons and holes under excitation conditions, and the Fenton system formed at the same time is more conducive to composite material enzyme catalysis and visual detection.

[0046] In some preferred embodiments, the benzoic acid compound includes 2-aminoterephthalic acid; the lanthanide element includes europium; and the magnetic nanoparticles include ferroferric oxide nanoparticles. In this preferred embodiment, the lanthanide element includes europium, which is more conducive to improving the fluorescence response sensitivity of fluoroquinolone antibiotics. On the one hand, the triplet excited state electrons of fluoroquinolone antibiotics are transferred to europium. 5 D0 energy level and from europium 5 The energy level transition from D0 level to ground state is easier to occur, which can improve the fluorescence response. On the other hand, Eu 3+ It emits in the long-wavelength red region, and when used with benzoic acid compound ligands, it tunes the luminescence to produce a characteristic fluorescence response signal at a specific wavelength, which can enhance the fluorescence response. Benzoic acid compounds include 2-aminoterephthalic acid, which forms a MOF network structure and excellent characteristic intramolecular charge transfer fluorescence with lanthanide metals, which is more conducive to electron transmission and transfer, forming a stable fluorescence signal; magnetic nanoparticles include ferroferric oxide nanoparticles, and the hole structure and Fenton reaction system formed are more conducive to the formation of charge transfer and enzyme-like catalytic reactions. Based on the MOF network structure and characteristic intramolecular charge transfer fluorescence formed by 2-aminoterephthalic acid, the special luminescence characteristics of europium and the rich energy level transitions, the electron holes and Fenton reaction system of ferroferric oxide nanoparticles, 2-aminoterephthalic acid and europium constitute a metal organic framework compound, which is coated on the surface of ferroferric oxide nanoparticles. Through the antenna effect and enzyme-like catalytic effect, it can sensitize fluoroquinolone antibiotics with strong absorption, produce a unique fluorescence response, and be more conducive to the fluorescence and visualization detection of target compounds.

[0047] In some preferred embodiments, the shell has a porous structure and a uniform pore size, the average thickness and average pore size of the shell are 10 nm-50 nm and 5 nm-40 nm, respectively, and the average particle size of the core is 100 nm-500 nm. Under this preferred embodiment, the average thickness of the shell is 10 nm-50 nm, the shell has a porous structure and a uniform pore size, and the average pore size is 5 nm-40 nm, which is more conducive to the effective extraction of fluoroquinolone compounds, intramolecular charge transfer and transition, and the generation of a stable fluorescence response signal. The average particle size of the core is not less than 100 nm, which is more conducive to improving the magnetic properties and enzyme-like catalytic effect of the composite material, promoting the separation of the composite material and the enzyme-like catalytic reaction, and is not higher than 500 nm. The composite material has a more suitable specific surface area, which is more conducive to maintaining the catalytic efficiency and the hole structure. The average thickness of the shell layer can be, for example, 10 nm, 20 nm, 30 nm, 40 nm and 50 nm, the average pore size of the shell layer can be, for example, 5 nm, 15 nm, 25 nm, 35 nm and 40 nm, and the average particle size of the core can be, for example, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm and 500 nm.

[0048] In the second aspect, the present invention provides a method for preparing the magnetic MOF composite material described in the first aspect, preparing a lanthanide organic framework compound, wherein the organic ligand of the lanthanide organic framework compound is a benzoic acid compound having at least two carboxyl groups and a benzene ring structure, and the lanthanide organic framework compound is coated on the surface of magnetic nanoparticles. The magnetic MOF composite material prepared by the preparation method of the present invention has a magnetic nanoparticle core and a lanthanide organic framework compound shell layer with a benzoic acid compound having at least two carboxyl groups and a benzene ring structure as an organic ligand coated on the surface of the core, with magnetic nanoparticles inside and an ordered network structure formed by lanthanide elements and benzoic acid compounds outside, and through the synergy of lanthanide elements, benzoic acid compounds and magnetic nanoparticles, it is possible to achieve a highly sensitive fluorescence response and an excellent enzyme-like catalytic effect, and further achieve highly sensitive fluorescence and visual detection.

[0049] In some preferred embodiments, during the preparation of the lanthanide organic framework compound, the lanthanide is added in the form of lanthanide nitrate; in the raw material composed of magnetic nanoparticles, benzoic acid compounds having at least two carboxyl groups and a benzene ring structure, and lanthanide nitrate, the mass ratio of magnetic nanoparticles, benzoic acid compounds, and lanthanide nitrate is 1: (0.5-8): (1-5). Under this preferred embodiment, the lanthanide is added in the form of lanthanide nitrate to form a stable and uniform ion source system, which is more conducive to the formation of the MOF shell. The mass ratio of benzoic acid compounds and lanthanide nitrate is (0.5-8): (1-5), and the organic ligand has a good complexing effect with the lanthanide, which is more conducive to the inclusion of the magnetic core surface and the formation of a network structure. The shell has a uniform pore size of 5 nm-40 nm. On this basis, the mass ratio of magnetic nanoparticles, benzoic acid compounds and lanthanide nitrates is 1: (0.5-8): (1-5), forming a magnetic MOF composite material with controllable particle size, and a stable MOF shell structure is uniformly formed on the surface of the magnetic particles, which is more conducive to energy level transition and electron transfer, forming a stable fluorescence signal and color response. The lanthanide nitrate can be in the form of crystal water. In this preferred embodiment, the mass of the lanthanide nitrate includes the mass of crystal water.

[0050] The present invention can adopt a two-step method of first preparing a lanthanide organic framework compound and then coating magnetic nanoparticles, or can simultaneously prepare a lanthanide organic framework compound and coat magnetic nanoparticles. In some preferred embodiments, the magnetic nanoparticles are mixed with a benzoic acid compound having at least two carboxyl groups and a benzene ring structure and a lanthanide element as raw materials, and a magnetic MOF composite material is prepared by a first solvothermal reaction in a one-step method. Under this preferred embodiment, the magnetic nanoparticles are mixed with a benzoic acid compound having at least two carboxyl groups and a benzene ring structure and a lanthanide element, and a first solvothermal reaction is performed to prepare a magnetic MOF composite material in a one-step method. During the solvothermal reaction, the lanthanide element and the benzoic acid compound organic ligand are directly synthesized on the surface of the magnetic nanoparticles, and the lanthanide organic framework compound is synthesized while being coated, and the MOF shell grows in situ on the surface of the magnetic nanoparticles. Compared with the two-step method of first preparing a lanthanide organic framework compound and then coating magnetic nanoparticles, it is more conducive to forming a stable and uniform shell, and the composite material can be prepared and controlled in size, thereby improving the sensitivity and accuracy of fluorescence detection.

[0051] Preferably, the temperature of the first solvent thermal reaction is 80°C-180°C, and the time is 12h-72h. Under this preferred embodiment, the temperature of the first solvent thermal reaction is 80°C-180°C, which is more conducive to the mild and controllable preparation of the MOF shell layer and ensures the stability of the organic ligand. The reaction time is 12h-72h, which is more conducive to the full formation of the MOF shell layer.

[0052] Preferably, the first solvent thermal reaction is carried out in a mixed solution of N'N-dimethylformamide and water, the volume ratio of N'N-dimethylformamide and water in the mixed solution is 1: (0.5-2), and 30mL-100mL of the mixed solution is used for each gram of the magnetic nanoparticles. Under this preferred embodiment, the first solvent thermal reaction is carried out in a mixed solution of N'N-dimethylformamide and water, keeping the reaction system mild, which is more conducive to the dissolution of raw materials and the reaction. The volume ratio of N'N-dimethylformamide and water in the mixed solution is 1: (0.5-2), which is more conducive to the controllable construction of the MOF shell. Relative to using 30mL-100mL of the mixed solution per gram of magnetic nanoparticles, it is more conducive to the uniform dispersion of magnetic nanoparticles, inhibiting particle agglomeration, and forming a uniform shell on the surface of the material.

[0053] In some preferred embodiments, metal salts, weak acid strong base salts, and polyol polymers are mixed in an alcohol solvent, and the magnetic nanoparticles are obtained by a second solvent thermal reaction. Under this preferred embodiment, the use of weak acid strong base salts is more conducive to ensuring the effective preparation and particle size control of magnetic nanoparticles. The solvent adopts an alcohol solvent, which is more conducive to ensuring that the boiling point of the reaction system and the high pressure conditions prevent the generation of heterogeneous phases, and the larger viscosity can reduce the crystal growth rate. The use of polyol polymers is more conducive to fully dispersing the magnetic nanoparticles, preventing agglomeration, forming magnetic nanoparticles with uniform particle size and magnetic response characteristics, controlling the morphology of the magnetic MOF composite material, and ensuring uniform and effective coating, thereby being more conducive to magnetic core protection and composite material electron transfer.

[0054] The present invention does not limit the types of weak acid and strong base salts, such as sodium acetate and sodium citrate, and does not limit the types of alcohol solvents, such as ethanol, n-octanol, propylene glycol, and ethylene glycol. Preferably, the metal salt is anhydrous ferric chloride, the weak acid and strong base salt is anhydrous sodium acetate, the polyol polymer is polyethylene glycol, and the alcohol solvent is ethylene glycol; when preparing the magnetic nanoparticles, anhydrous ferric chloride, anhydrous sodium acetate, and polyethylene glycol are mixed in a mass ratio of 1: (0.5-5): (0.1-1.5); the amount of ethylene glycol per gram of anhydrous ferric chloride is 15mL-30mL, and the temperature of the second solvent thermal reaction is 160℃-220℃, and the time is 8h-24h.

[0055] Under this preferred embodiment, the metal salt is anhydrous ferric chloride, which provides a stable iron source and reacts with the solvent to be reduced to divalent iron, which is more conducive to the formation of magnetic ferrosoferric oxide; the weak acid and strong base salt is anhydrous sodium acetate, which is bonded to the surface of the grains to prevent grain aggregation and affects the surface energy and growth rate of different crystal faces, which is more conducive to the control of the particle size and morphology of the magnetic particles; the polyol polymer is polyethylene glycol, which is more conducive to the dispersion of magnetic nanoparticles; the alcohol solvent is ethylene glycol, which can increase the reaction temperature, reduce the grain nucleation rate, and is more conducive to the formation of magnetic particles; the amount of ethylene glycol corresponding to each gram of anhydrous ferric chloride is not less than 15 mL, which is more conducive to fully dissolving organic compounds and inorganic compounds with higher polarity to form a homogeneous system, and is not higher than 30 mL, which is more conducive to increasing the concentration of metal salts in the system to form magnetic particles. The mass ratio of anhydrous ferric chloride, anhydrous sodium acetate, and polyethylene glycol is 1: (0.5-5): (0.1-1.5), which is more conducive to forming a stable reaction system, controlling the ion concentration, system viscosity, crystal growth conditions, etc. in the reaction, and can control the preparation of magnetic nanoparticles. The temperature of the second solvent thermal reaction is not less than 160°C, which is more conducive to crystal nucleation and growth, and not higher than 220°C, which is more conducive to system pressure control. The reaction time is not less than 8h, which is more conducive to crystal nucleus growth, and not higher than 24h, which is more conducive to the controllable preparation of magnetic nanoparticles with uniform particle size.

[0056] In a third aspect, the present invention provides a method for detecting fluoroquinolone antibiotics, comprising: mixing the magnetic MOF composite material as described in the first aspect and / or the magnetic MOF composite material prepared by the preparation method as described in the second aspect with a substance to be tested to obtain a mixed solution, placing the mixed solution under an ultraviolet lamp and performing fluorescence measurement, and detecting fluoroquinolone antibiotics by color changes and fluorescence response intensity.

[0057] In a fourth aspect, the present invention provides a method for detecting fluoroquinolone antibiotics, comprising: mixing the magnetic MOF composite material described in the first aspect and / or the magnetic MOF composite material prepared by the preparation method described in the second aspect, a substance to be tested and an indicator to obtain a mixed solution, and detecting the fluoroquinolone antibiotics by the color of the mixed solution.

[0058] The present invention is further described in detail below with reference to specific embodiments.

[0059] Example 1

[0060] A method for preparing a magnetic MOF composite material, the steps are as follows:

[0061] Step 1: Weigh 5g of anhydrous ferric chloride, 12.5g of anhydrous sodium acetate, and 3g of polyethylene glycol, mix and dissolve in 100mL of ethylene glycol, ultrasonicate for 10 minutes to fully disperse the mixture, and then place it on a magnetic stirrer to stir evenly. Transfer the above mixed solution to a polytetrafluoroethylene-lined autoclave for a second solvothermal reaction, program the temperature to 200°C, and naturally cool to room temperature after fully reacting for 15 hours. Collect the solid obtained after the reaction through an external magnetic field, and then wash it with deionized water and ethanol several times to obtain ferroferric oxide magnetic nanoparticles;

[0062] Step 2: Weigh 1g of the magnetic nanoparticles obtained in step 1 and fully disperse them in a mixed solution of 70ml DMF and water, where the volume ratio of DMF to water is 1:1. Then weigh 0.75g of 2-aminoterephthalic acid and 2g of europium nitrate hexahydrate into the above solution and stir and mix them thoroughly. The mixed solution is transferred to a polytetrafluoroethylene-lined autoclave for the first solvothermal reaction, and the temperature is raised to 180°C. After fully reacting for 12h, the temperature is naturally lowered to room temperature, and the solid obtained after the reaction is collected by an external magnetic field, and then washed with deionized water and ethanol for multiple times to obtain a magnetic MOF composite material.

[0063] A magnetic MOF composite material comprises a core and a shell coated on the surface of the core, wherein the shell is a lanthanide organic framework compound, the lanthanide element of the lanthanide organic framework compound is europium, the organic ligand is 2-aminoterephthalic acid, and the core is ferrosoferric oxide nanoparticles.

[0064] Example 2

[0065] Referring to Example 1, the difference is that in step 1 of the preparation method, the amount of anhydrous ferric chloride is 2 g, the amount of anhydrous sodium acetate is 2.5 g, the amount of polyethylene glycol is 2 g, and the mixture is dissolved in 60 mL of ethylene glycol after mixing, and the mixture is fully dispersed by ultrasonication for 15 minutes. The temperature of the second solvent thermal reaction is 210° C., and the reaction time is 20 h. In step 2, the amount of the mixed solution of DMF and water is 80 mL, the amount of 2-aminoterephthalic acid is 0.81 g, and the amount of europium nitrate hexahydrate is 1.5 g. The reaction temperature of the first solvent thermal reaction is 120° C., and the reaction time is 24 h. Others remain unchanged.

[0066] Example 3

[0067] Referring to Example 1, the difference is that in step 2 of the preparation method, 4-(2,5-dicarboxyphenoxy)phthalic acid is used instead of 2-aminoterephthalic acid. The organic ligand of the lanthanide organic framework compound of the prepared magnetic MOF composite material is 4-(2,5-dicarboxyphenoxy)phthalic acid.

[0068] Example 4

[0069] Referring to Example 1, the difference is that in step 2 of the preparation method, lanthanum nitrate hexahydrate is used instead of europium nitrate hexahydrate. In the prepared magnetic MOF composite material, the lanthanide element of the lanthanide organic framework compound is lanthanum.

[0070] Example 5

[0071] Refer to Example 1, the difference is that in step 2 of the preparation method, the amount of europium nitrate hexahydrate added is 0.5 g.

[0072] Example 6

[0073] Refer to Example 1, the difference is that in step 2 of the preparation method, the temperature of the first solvent thermal reaction is 70°C.

[0074] Example 7

[0075] Refer to Example 1, the difference is that in step 2 of the preparation method, the volume ratio of DMF and water in the mixed solution is 1:0.2.

[0076] Example 8

[0077] Referring to Example 1, the difference is that in step 2 of the preparation method, a mixed solution of DMF and water is not used, and 1 g of the magnetic nanoparticles obtained in step 1 is weighed and fully dispersed in 70 ml of DMF.

[0078] Example 9

[0079] Refer to Example 1, the difference is that in step 1 of the preparation method, the temperature of the second solvent thermal reaction is 120°C.

[0080] Example 10

[0081] Refer to Example 1, the difference is that in step 1 of the preparation method, the amount of anhydrous ferric chloride is 2 g, the amount of anhydrous sodium acetate is 12 g, and the amount of polyethylene glycol is 4 g.

[0082] Embodiment 11

[0083] Refer to Example 1, the difference is that in step 1 of the preparation method, sodium citrate is used instead of anhydrous sodium acetate.

[0084] Example 12

[0085] Refer to Example 1, the difference is that in step 1 of the preparation method, ethanol is used instead of ethylene glycol.

[0086] Embodiment 13

[0087] Referring to Example 1, the difference is that the method of step 1 is not used to prepare the ferroferric oxide magnetic nanoparticles in the preparation method, and the preparation method of the ferroferric oxide magnetic nanoparticles is a co-precipitation method.

[0088] Comparative Example 1

[0089] A method for preparing a lanthanide organic framework compound, the preparation method is to fully disperse 0.75g of 2-aminoterephthalic acid and 2g of europium nitrate hexahydrate in a mixed solution of 70ml of DMF and water, the volume ratio of DMF to water in the mixed solution is 1:1. Then the mixed solution is transferred to a high-pressure reactor, heated to 180°C, fully reacted for 12h, naturally cooled to room temperature, centrifuged, and washed with deionized water and ethanol for multiple times, and dried for use. A lanthanide organic framework compound, the lanthanide element of the lanthanide organic framework compound is europium, and the organic ligand is 2-aminoterephthalic acid.

[0090] Experimental example

[0091] Experimental Example 1

[0092] The magnetic MOF composite materials of Examples 1 to 13 were scanned by transmission electron microscope. The microscopic morphology of the magnetic MOF composite material of Example 1 is shown in Figure 1 The core of the magnetic nanoparticles is a relatively uniform spherical structure, the surface of the core of the magnetic nanoparticles is relatively uniformly coated with a MOF shell, and the magnetic nanoparticles and the lanthanide organic framework compound form a stable composite structure. The microscopic morphology of the magnetic MOF composite material of Example 2-13 shows that the prepared composite material includes a magnetic nanoparticle core, and the surface of the core is uniformly coated with a shell.

[0093] The magnetic MOF nanocomposites of Examples 1 to 13 were characterized by specific surface area (BET) analysis to verify the material structure and pore size and volume distribution. Figure 2 . The results of specific surface area analysis show that the prepared nanocomposite has a large specific surface area, the shell has a porous structure and uniform pore size, the pore size is distributed between 5-50 nanometers, and the average pore size is 18nm. This shows that the prepared nanocomposite MOF shell has a good mesoporous structure, which is mainly attributed to the uniform network ordered structure of the MOF shell, which is conducive to the adsorption and detection of fluoroquinolone antibiotics by the composite material.

[0094] The characterization results of the core and shell morphology structures of the magnetic MOF composite materials of Examples 1 to 13 are shown in Table 2, where the thickness refers to the average thickness of the shell, the pore size refers to the average pore size of the shell, and the core particle size refers to the average particle size of the core.

[0095] Experimental Example 2

[0096] High-resolution dark-field phase energy dispersion x-ray analysis was performed on the magnetic MOF nanocomposites of Examples 1 to 13. The experimental results of Example 1 are shown in Figure 3 , Figure 3 As shown in the element distribution, the main elements contained in the nanocomposite material, such as Fe, O, N, C, Eu and other elements, can be detected. Among them, Fe and O elements are mainly distributed in the middle magnetic core, indicating that a magnetic core of ferroferric oxide has been prepared. C, N and Eu elements are mainly distributed in the outer wall and shell of the magnetic core, mainly due to the coating formed on the surface of the magnetic core by the prepared lanthanide MOF. High-resolution dark field phase energy dispersion x-ray analysis further illustrates that the surface of the magnetic nanoparticles is coated with lanthanide organic framework compounds, and the present invention can prepare a magnetic MOF nanocomposite material with a core-shell structure. The high-resolution dark field phase energy dispersion x-ray analysis results of the composite materials of Examples 2 to 13 are similar to the analysis results of Example 1.

[0097] Experimental Example 3

[0098] The magnetic MOF nanocomposites of Examples 1 to 13 were characterized by X-ray photoelectron spectroscopy (XPS) to verify the chemical composition of the materials and the chemical states of the relevant elements. Figures 4 to 8 . The full scan spectrum of the elements can be found at Figure 4 The element absorption peaks correspond to the four main elements in the nanocomposite materials, namely Eu (3d, 4d), O 1s, N1s and C 1s. The high-resolution spectrum of C 1s can be found in Figure 5The binding energies are 284.8 eV, 286.2 eV, 288.1 eV and 289.7 eV, which correspond to the C−H / C=C, C−N / C−C, CO and C=O bonds of the nanomaterials, respectively, indicating that the lanthanide organic framework compounds are successfully coated on the surface of the magnetic nanomaterials. The high-resolution spectrum of O 1s is shown in Figure 6 , corresponding to the high-resolution spectra of COOH / CO and Fe-O, N 1s, see Figure 7 , corresponding to the NC / NH bond. This further indicates that the lanthanide organic framework compound is successfully coated on the surface of the magnetic nanomaterial. The high-resolution spectrum of Eu 3d is shown in Figure 8 , it can be fitted into five main absorption peaks, 1126.3 eV, 1135.9 eV and 1165.3 eV correspond to Eu 3+ 3d 5 / 2 , Eu 3+ 3d 5 / 2 and Eu 3+ 3d 3 / 2 , indicating that Eu 3+ is the main valence state of Eu, 1155.5 eV (Eu 2+ 3d 3 / 2 ) is due to the charge compensation in the XPS environment causing Eu 3+ Convert to Eu 2+ , 1144.6 eV corresponds to Eu metal, indicating that Eu does not exist in an oxidized state. The high-resolution spectrum analysis of the characteristic elements of the comprehensive nanocomposite material shows that a magnetic MOF composite material with a core of magnetic nanoparticles and a shell of lanthanide organic framework compounds is prepared. The X-ray photoelectron spectroscopy analysis results of the composite materials of Examples 2 to 13 are similar to the analysis results of Example 1.

[0099] Experimental Example 4

[0100] The magnetic MOF nanocomposites of Examples 1 to 13 and the lanthanide organic framework compound of Comparative Example 1 were used in the application study of fluorescence detection of fluoroquinolone antibiotics.

[0101] Weigh 1 mg of magnetic MOF composite material or lanthanide organic framework compound and ultrasonically disperse it in 10 mL of deionized water to prepare a mixed solution with a concentration of 0.1 mg / mL. Pipette 200 μL of the above mixed solution into deionized water, and add different concentrations of ofloxacin and ciprofloxacin respectively and dilute to 1 mL with deionized water to obtain a series of ofloxacin and ciprofloxacin solutions of different concentrations. Place it under a 365nm ultraviolet lamp and record the fluorescence changes under different concentration conditions. At the same time, the above-mentioned solutions of different concentrations are subjected to fluorescence measurement, and their fluorescence curves are recorded to evaluate the fluorescence test effects of the magnetic MOF nanocomposites of Examples 1 to 13 and the lanthanide organic framework compounds of Comparative Example 1 on the target fluoroquinolone antibiotics. The samples of different concentrations are measured by a multifunctional microplate reader to detect the fluorescence responses of fluoroquinolone antibiotics of different concentrations.

[0102] Under the same condition of fluoroquinolone concentration (50 μM), the composite materials of Examples 1 to 13 and the lanthanide organic framework compounds of the comparative example were used for detection, and the fluorescence response intensity of the detection is shown in Table 2. The detection limits of the composite materials of Examples 1 to 13 and the lanthanide organic framework compounds of the comparative example are shown in Table 2. The fluorescence response intensity and detection limit of the detection are obtained by taking the average value after measuring 7 times, and the detection results of the 7 fluorescence response intensities of Example 1 are shown in Table 1.

[0103] Table 1

[0104]

[0105] From Table 1, after 7 repeated tests, the fluorescence intensity response of the target is relatively consistent, and the RSD value of the 7 measurement results is 0.76%, indicating that the magnetic MOF composite material of Example 1 has good stability and reproducibility when used to detect fluoroquinolone antibiotics. The magnetic MOF composite materials of Examples 2 to 13 also have good stability and reproducibility when used to detect fluoroquinolone antibiotics.

[0106] The test results of the magnetic MOF composite material of Example 1 are shown in Fig. 9 and Fig.10 The figure in the upper right corner shows the color changes of analytes at different concentrations under ultraviolet light. The results show that ciprofloxacin and ofloxacin show different color changes under 365nm ultraviolet light. Ciprofloxacin gradually changes to bright blue under ultraviolet light as its concentration increases, and the fluorescence response intensity also increases accordingly ( Fig. 9 ), as the concentration of ofloxacin increases, it gradually turns into bright green under ultraviolet light, and the fluorescence response intensity also increases ( Fig.10 ). This indicates that the magnetic MOF composite material of Example 1 has a good fluorescence response capability to the target fluoroquinolone compound, has a high detection sensitivity, and can be used for fluorescence detection of samples of different concentrations.

[0107] Experimental Example 5

[0108] The magnetic MOF nanocomposites of Examples 1 to 13 and the lanthanide organic framework compound of Comparative Example 1 were used for the visualization application study of fluoroquinolone antibiotics.

[0109] Prepare a fixed concentration of magnetic MOF composite material or lanthanide organic framework compound solution, and transfer a certain amount of the above solution into a small centrifuge tube, add hydrogen peroxide and TMB solution, then add different concentrations of ciprofloxacin and ofloxacin into the above centrifuge tube, mix thoroughly, and record the color changes under different concentration conditions. At the same time, perform fluorescence measurement on samples at different concentrations, record the relationship between fluorescence response intensity, color and concentration, and measure them using a multifunctional microplate reader.

[0110] The test results of Example 1 are shown in Fig.11 , the upper left corner image corresponds to the visualization detection image of ofloxacin (from left to right, the concentration of ofloxacin gradually increases, and the concentration of ofloxacin in the second row is greater than that in the first row), the lower left corner image corresponds to the change in the fluorescence response signal of ofloxacin, the upper right corner image corresponds to the visualization detection image of ciprofloxacin (from left to right, the concentration of ciprofloxacin gradually increases, and the concentration of ciprofloxacin in the second row is greater than that in the first row), the lower right corner image corresponds to the change in the fluorescence response signal of ciprofloxacin. As the concentration of the sample increases, the sample shows a color change visible to the naked eye, gradually changing from light blue-dark blue-dark green-light green-cyan-cyan. At the same time, its fluorescence spectrum also undergoes a red shift, and its fluorescence response increases accordingly as the concentration increases, which can be detected visually and by instruments at the same time.

[0111] Under the same condition of fluoroquinolone concentration (50 μM), the composite materials of Examples 1 to 13 and the lanthanide organic framework compound of the comparative example were used for detection, and the fluorescence response intensity of the target fluoroquinolone antibiotic after enzyme-like catalysis is shown in Table 2. Since the color change after enzyme-like catalysis affects the fluorescence detection intensity of the target, its fluorescence intensity is reduced compared to direct detection.

[0112] Table 2

[0113]

[0114] The fluorescence response intensity and the fluorescence response intensity after enzyme-like catalysis of Examples 1 to 13 are higher than those of Comparative Example 1, and the detection limits of Examples 1 to 13 are lower than those of Comparative Example 1. The magnetic MOF composite material of the present invention has a magnetic nanoparticle core and a lanthanide organic framework compound shell, which can significantly improve the fluorescence response intensity and enzyme-like catalytic effect, and significantly reduce the detection limit, compared with only using lanthanide organic framework compounds.

[0115] Comparing Examples 1, 3, and 4, the organic ligand of the benzoic acid compound includes 2-aminoterephthalic acid, and the lanthanide element includes europium, which is more conducive to improving the fluorescence response intensity and enzyme-like catalytic effect. Comparing Example 1 and Example 5, the mass ratio of magnetic nanoparticles, benzoic acid compounds, and lanthanide nitrates is 1: (0.5-8): (1-5), which is more conducive to forming a complete MOF structure in the shell layer, obtaining a shell structure with uniform pore size, controlling the thickness of the shell layer, and improving the fluorescence response intensity and enzyme-like catalytic effect. Comparing Example 1 and Example 6, the temperature of the first solvothermal reaction is 80°C to 180°C, which is more conducive to forming a complete MOF structure in the shell layer, obtaining a shell structure with uniform pore size, controlling the thickness of the shell layer, and improving the fluorescence response intensity and enzyme-like catalytic effect. Comparing Examples 1, 7, and 8, the first solvothermal reaction is carried out in a mixed solution of N'N-dimethylformamide and water, and the volume ratio of N'N-dimethylformamide to water is 1: (0.5-2), which is more conducive to forming a complete MOF structure in the shell layer, obtaining a shell structure with uniform pore size, and improving the fluorescence response intensity and enzyme-like catalytic effect. Comparing Example 1 and Example 9, the temperature of the second solvothermal reaction is 160°C-220°C, which is more conducive to crystal nucleation and growth, controlling the magnetic core particle size, and improving the fluorescence response intensity and enzyme-like catalytic effect. Comparing Example 1 and Example 10, when preparing magnetic nanoparticles, anhydrous ferric chloride, anhydrous sodium acetate, and polyethylene glycol are mixed in a mass ratio of 1: (0.5-5): (0.1-1.5), which is more conducive to controlling the magnetic core particle size, improving the fluorescence response intensity and enzyme-like catalytic effect. Comparing Example 1 and Example 11, the weak acid and strong base salt is anhydrous sodium acetate, which is more conducive to improving the fluorescence response intensity and enzyme-like catalytic effect. Comparing Example 1 and Example 12, the alcohol solvent is ethylene glycol, which is more conducive to controlling the particle size of the magnetic core, improving the fluorescence response intensity and the enzyme-like catalytic effect. Comparing Example 1 and Example 13, the metal salt, weak acid and strong base salt, and polyol polymer are mixed in an alcohol solvent by the present invention, and the magnetic nanoparticles are prepared by a second solvent thermal reaction. Compared with the coprecipitation method for preparing magnetic particles, it is more conducive to controlling the particle size of the magnetic core, obtaining a shell structure with uniform pore size, and improving the fluorescence response intensity and the enzyme-like catalytic effect.

[0116] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A magnetic MOF composite material for fluorescence and visualization detection of fluoroquinolone antibiotics, characterized in that: It comprises an inner core and a shell layer coated on the surface of the inner core, wherein the shell layer comprises a lanthanide organic framework compound, the organic ligand of the lanthanide organic framework compound is a benzoic acid compound having at least two carboxyl groups and a benzene ring structure, and the inner core is a magnetic nanoparticle; the benzoic acid compound comprises 2-aminoterephthalic acid; the lanthanide element comprises europium; and the magnetic nanoparticle comprises ferrosoferric oxide nanoparticles.

2. The magnetic MOF composite material according to claim 1, characterized in that: The shell layer has a porous structure and a uniform pore size, the average thickness and average pore size of the shell layer are 10 nm-50 nm and 5 nm-40 nm respectively, and the average particle size of the core is 100 nm-500 nm.

3. A method for preparing a magnetic MOF composite material according to any one of claims 1 to 2, characterized in that: A lanthanide organic framework compound is prepared, wherein the organic ligand of the lanthanide organic framework compound is a benzoic acid compound having at least two carboxyl groups and a benzene ring structure, and the lanthanide organic framework compound is coated on the surface of magnetic nanoparticles.

4. The preparation method according to claim 3, characterized in that: During the preparation of the lanthanide organic framework compound, the lanthanide is added in the form of lanthanide nitrate; In the raw material composed of magnetic nanoparticles, benzoic acid compounds having at least two carboxyl groups and a benzene ring structure, and lanthanide nitrates, the mass ratio of the magnetic nanoparticles, the benzoic acid compounds, and the lanthanide nitrates is 1:(0.5-8):(1-5).

5. The preparation method according to claim 3, characterized in that: The magnetic nanoparticles are mixed with a benzoic acid compound having at least two carboxyl groups and a benzene ring structure and a lanthanide element as raw materials, and the magnetic MOF composite material is prepared by a one-step method through a first solvothermal reaction.

6. The preparation method according to claim 5, characterized in that: The temperature of the first solvent thermal reaction is 80° C.-180° C., and the time is 12 h-72 h.

7. The preparation method according to claim 5, characterized in that: The first solvothermal reaction is carried out in a mixed solution of N'N-dimethylformamide and water, wherein the volume ratio of N'N-dimethylformamide to water in the mixed solution is 1:(0.5-2), and 30mL-100mL of the mixed solution is used for each gram of the magnetic nanoparticles.

8. The preparation method according to claim 3, characterized in that: The metal salt, the weak acid and strong base salt and the polyol polymer are mixed in an alcohol solvent, and the magnetic nanoparticles are obtained through a second solvent thermal reaction.

9. The preparation method according to claim 8, characterized in that: The metal salt is anhydrous ferric chloride, the weak acid and strong base salt is anhydrous sodium acetate, the polyol polymer is polyethylene glycol, and the alcohol solvent is ethylene glycol; When preparing the magnetic nanoparticles, anhydrous ferric chloride, anhydrous sodium acetate, and polyethylene glycol are mixed in a mass ratio of 1: (0.5-5): (0.1-1.5); the amount of ethylene glycol corresponding to each gram of anhydrous ferric chloride is 15mL-30mL, and the temperature of the second solvent thermal reaction is 160°C-220°C, and the time is 8h-24h.

10. A method for detecting fluoroquinolone antibiotics, characterized in that: include: The magnetic MOF composite material according to claim 1 or 2 and / or the magnetic MOF composite material prepared by the preparation method according to any one of claims 3 to 9 is mixed with a substance to be tested to obtain a mixed solution, the mixed solution is placed under an ultraviolet lamp and subjected to fluorescence measurement, and the fluoroquinolone antibiotics are detected by color change and fluorescence response intensity.

11. A method for detecting fluoroquinolone antibiotics, characterized in that: include: The magnetic MOF composite material according to claim 1 or 2 and / or the magnetic MOF composite material prepared by the preparation method according to any one of claims 3 to 9, a substance to be tested and an indicator are mixed to obtain a mixed solution, and fluoroquinolone antibiotics are detected by the color of the mixed solution.