Crystalline silicon solar cell and its preparation method and application

By covering the graphite layer doped with conductive agent on the gate line surface of the crystalline silicon solar cell, the problems of component appearance and thermal effects are solved, and full blackening and performance improvement are achieved.

CN118676223BActive Publication Date: 2024-12-06CANDO SOLARPHOTOELECTRIC TECH (CHANGZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411140272.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-12-06
Estimated Expiration
2044-08-20

Smart Images

  • Figure CN118676223B_ABST
    Figure CN118676223B_ABST
Patent Text Reader

Abstract

The present invention discloses a crystalline silicon solar cell and a preparation method and application thereof, and relates to the field of solar cell technology, wherein the crystalline silicon solar cell comprises: a silicon wafer, a film covering the surface of the silicon wafer, and a grid line arranged on the film, wherein the surface of the grid line is covered with a graphite layer. A graphite layer is arranged on the surface of the grid line, and the graphite layer can cover the grid line to achieve full blackening of the grid line, meeting the customer's full blackening customization needs. At the same time, because graphite has the characteristics of high electrical conductivity and high temperature resistance, it is beneficial to improve the thermal conductivity of the crystalline silicon solar cell and reduce the influence of thermal effects on the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cells, and in particular to a crystalline silicon solar cell sheet and a preparation method and application thereof. Background Art

[0002] Crystalline silicon cells are mainly based on semiconductor materials. Their working principle is to use the photoelectric effect after photoelectric materials absorb light energy to convert light energy into electrical energy. The preparation of crystalline silicon cells mainly includes: first, doping a trace amount of boron, phosphorus, etc. in the crystalline silicon wafer to form a P / N junction on the silicon wafer, and then using the screen printing method to print the silvery white silver paste on the silicon wafer to form a grid line, and then sintering and curing the grid line to make a cell. In order to achieve the integration of color and appearance of photovoltaic modules as much as possible, existing photovoltaic module manufacturers mostly use black backplanes, welding strips and busbars. However, since the grid lines printed by silver paste are silvery white, it is still difficult to achieve a completely black appearance of photovoltaic modules.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] The purpose of the present invention is to provide a crystalline silicon solar cell and a preparation method and application thereof, so as to achieve blackening of the grid lines while ensuring the performance of the solar cell.

[0005] The present invention is achieved in that:

[0006] In a first aspect, the present invention provides a crystalline silicon solar cell, comprising: a silicon wafer, a film covering a surface of the silicon wafer, and a grid line arranged on the film, wherein the surface of the grid line is covered with a graphite layer.

[0007] In an optional embodiment, the graphite layer is doped with a conductive agent, the conductive agent is selected from at least one of silver, copper, gold, and aluminum;

[0008] Preferably, the doping amount is 0.1wt%-1wt%;

[0009] Preferably, the crystalline silicon solar cell is a HJT heterogeneous crystalline silicon solar cell or a topcon crystalline silicon solar cell.

[0010] In a second aspect, the present invention provides a method for preparing the crystalline silicon solar cell described in the aforementioned embodiment, comprising:

[0011] The grid lines are printed on the film covering the surface of the silicon wafer, and then the grid lines are covered with graphite powder. The solar cell covered with graphite powder is annealed and cleaned for the second time in sequence to obtain the crystalline silicon solar cell.

[0012] In an optional embodiment, the method comprises: printing a silver paste on a battery cell to form the grid line, wherein the silver paste comprises 78-82 parts by weight of silver powder, 8-12 parts by weight of epoxy resin and 5-11 parts by weight of an additive;

[0013] Preferably, the average particle size of the silver powder is less than 40 μm.

[0014] In an optional embodiment, the graphite powder also includes the conductive agent powder;

[0015] Preferably, the average particle size of the graphite powder is less than 20 μm.

[0016] In an optional embodiment, the annealing temperature is 100°C-600°C.

[0017] In an optional embodiment, before printing the gate lines, the cell is also first cleaned, and the first cleaning adopts a plasma cleaning method, and specific parameters include: power 300W-500W; process gas is at least one of Ar gas, O2 and CO2;

[0018] And / or, the second cleaning adopts a plasma cleaning method, and specific parameters include: power 100W-200W; process gas is N2 gas.

[0019] In a third aspect, the present invention provides a method for preparing a crystalline silicon solar cell module, wherein the positive and negative electrodes of two or more crystalline silicon solar cells are sequentially connected using a conductive tape to prepare a crystalline silicon cell string;

[0020] After the crystalline silicon cell strings are connected in series and / or in parallel by using busbars, a packaging film and a front plate glass are sequentially laid on the front side, and a packaging film and a back plate material are sequentially laid on the rear side, and then laminated to obtain a crystalline silicon solar cell module.

[0021] The present invention has the following beneficial effects:

[0022] In the embodiment of the present invention, a graphite layer is arranged on the surface of the grid line, and the graphite layer can cover the grid line to achieve full black processing of the grid line, meeting the customer's full black customization needs. At the same time, because graphite has high electrical conductivity and high temperature resistance, it is beneficial to improve the thermal conductivity of crystalline silicon solar cells and reduce the impact of thermal effects on batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0024] Figure 1 This is a flow chart of the preparation of the crystalline silicon solar cell in Example 1. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0026] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0027] The embodiment of the present invention provides a crystalline silicon solar cell, comprising: a silicon wafer, a film covering a surface of the silicon wafer, and a grid line arranged on the film, wherein the surface of the grid line is covered with a graphite layer.

[0028] In the embodiment of the present invention, a graphite layer is arranged on the surface of the grid line, and the graphite layer can cover the grid line to achieve full black processing of the grid line, meeting the customer's full black customization needs. At the same time, because graphite has high electrical conductivity and high temperature resistance, it is beneficial to improve the thermal conductivity of crystalline silicon solar cells and reduce the impact of thermal effects on batteries.

[0029] In an optional embodiment, the graphite layer is doped with a conductive agent, and the conductive agent is selected from at least one of silver, copper, gold, and aluminum. Doping the graphite layer with a conductive agent with good conductivity is beneficial to improving the conductivity of graphite, thereby improving the conversion efficiency of crystalline silicon solar cells. Under standard conditions, the resistivity of pure silver is about 1.6 x 10 -8 Ω·m, the resistivity of graphite is usually 10 -5 to 10 -6 Ω·m, although the resistivity of graphite is slightly lower than that of pure silver, the resistivity of graphite decreases with increasing temperature. The higher the temperature, the stronger the conductivity. The photovoltaic modules in practical application are exposed to sunlight, which can effectively improve the battery conversion efficiency in this environment.

[0030] In an optional embodiment, the doping amount is 0.1wt%-1wt%. If the doping amount is too little, the effect of improving the conversion efficiency of the crystalline silicon solar cell is not obvious. If the doping amount is too much, the color of the graphite layer will be changed, affecting the blackening effect of the grid line.

[0031] In an optional embodiment, the crystalline silicon solar cell is a busbarless crystalline silicon solar cell. In the busbarless crystalline silicon solar cell, the grid line is directly in contact with and connected to the conductive tape, and soldering is not required, which is more conducive to increasing the light receiving area of ​​the crystalline silicon solar cell. The thermal conductivity of graphite is 151 W / (m·K), and the thermal conductivity of tin is 67W / (m·K). The thermal conductivity of graphite is much higher than that of metallic tin, and the electrical conductivity is comparable. Therefore, while changing the color of the grid line, the presence of the graphite layer can replace the tin-plated conductive tape to reduce the cost of raw materials.

[0032] The present invention also provides a method for preparing the crystalline silicon solar cell described in the above embodiment, comprising:

[0033] The grid lines are printed on the film covering the surface of the silicon wafer, and then the grid lines are covered with graphite powder. The solar cell covered with graphite powder is annealed and cleaned for the second time in sequence to obtain the crystalline silicon solar cell.

[0034] In the implementation mode of the present invention, the thin film is deposited on a silicon wafer by PECVD and PVD equipment. First, black graphite powder with high conductivity and high temperature resistance is covered on the surface of the uncured gate line. Liquid will leach out of the gate line before curing, and the leached liquid will soak the graphite powder, which is equivalent to the adhesive initially fixing the graphite powder. Then, after an annealing step, while the gate line is cured, the graphite is also baked to form a graphite layer similar to a graphite electrode. Then, a second cleaning is performed to remove the graphite in the area outside the gate line. Since the graphite in the graphite layer is tightly combined with the gate line after curing, it will be retained, thereby achieving the blackening of the gate line without affecting the surface performance of the silicon wafer outside the gate line.

[0035] The method of covering the grid lines with graphite powder may be spraying or other methods, as long as the graphite powder can be relatively evenly covered in the area where the grid lines are located.

[0036] In an optional embodiment, it also includes: printing silver paste on a silicon wafer to form the gate line, the silver paste includes 78-82 parts by weight of silver powder, 8-12 parts by weight of epoxy resin and 5-11 parts by weight of additives, the additives include 0.1-1 parts by weight of a curing agent methylimidazole, 4-6 parts by weight of an inactive diluent butyl acetate, 1-2 parts by weight of an active diluent 692, 0.1-1 parts by weight of an adhesion promoter tetraethyl titanate, and 0.1-1 parts by weight of an anti-settling agent polyamide wax.

[0037] The different compositions of silver paste and the different adsorption capacities of graphite powder to the leaching solution may affect the connection between the graphite layer and the grid line, and further affect the performance of crystalline silicon solar cells.

[0038] In an optional embodiment, the average particle size of the silver powder is less than 40 μm. Specifically, the silver powder can be selected from at least one of nano silver powder ≤ 0.1 μm, ultrafine silver powder 0.1 μm-0.5 μm, ultrafine silver powder 0.5 μm-10 μm, and fine silver powder 10 μm-40 μm.

[0039] In an optional embodiment, the graphite powder also includes the conductive agent powder to improve the conductivity of the graphite.

[0040] In an optional embodiment, the average particle size of the graphite powder is less than 20 μm. Specifically, the graphite powder can be selected from at least one of subnanometer graphite powder ≤ 1 μm, ultrafine graphite powder 1-5 μm, ultrafine graphite powder 6-10 μm and fine graphite powder 11-20 μm.

[0041] In an optional embodiment, the annealing temperature is 100°C-600°C. The annealing temperature mainly depends on the battery type and the selected silver paste. The annealing temperature selected for low-temperature silver paste can be 100°C-200°C, and the annealing temperature selected for high-temperature silver paste can be 300°C-600°C.

[0042] In an optional embodiment, before printing the gate lines, the cell is also cleaned for the first time, and the first cleaning adopts a plasma cleaning method, and specific parameters include: power 300W-500W; process gas is at least one of Ar gas, O2 and CO2.

[0043] The purpose of the first cleaning is to clean the surface of the battery cell to remove dirt and residues from the previous process. Among the three gases, Ar, O2 and CO2, Ar and CO2 will not react with the battery, but O2 will form HO bonds with the surface of the battery cell, making the surface of the battery cell more susceptible to oxidation. Therefore, if O2 is used for the first cleaning, the subsequent steps need to be carried out as soon as possible.

[0044] In an optional embodiment, the second cleaning adopts a plasma cleaning method, and specific parameters include: power 100W-200W; process gas is N2 gas.

[0045] Use N2 gas for plasma micro-cleaning. The plasma formed by N2 ionization can remove the inorganic matter precipitated around the grid line and the small amount of graphite powder adhering to it, thereby increasing the cell's absorption of light. It can also roughen the surface of the graphite layer to reduce the scattering of light by the grid line surface, which is beneficial to improve the adhesion between the graphite layer and the film during packaging.

[0046] The embodiment of the present invention also provides a method for preparing a crystalline silicon solar cell module, wherein the positive and negative electrodes of two or more crystalline silicon solar cells are sequentially connected using a conductive tape to prepare a crystalline silicon cell string;

[0047] After the crystalline silicon cell strings are connected in series and / or in parallel by using busbars, a packaging film and a front plate glass are sequentially laid on the front side, and a packaging film and a back plate material are sequentially laid on the rear side, and then a crystalline silicon solar cell module is obtained after lamination. Specifically, the material of the conductive tape and the busbar can be selected from the prior art. If it is required to prepare a full black module, the conductive tape and the busbar can be selected from blackened conductive tapes and busbars. If it is not required to prepare a full black module, conductive tapes and busbars of other colors or materials can also be selected.

[0048] Example 1

[0049] This embodiment provides a method for preparing a crystalline silicon solar cell. Figure 1 As shown, the specific steps include:

[0050] 1) Plasma cleaning is used to clean the surface of the cell (including silicon wafer and film) to remove dirt and previous process residues. The specific parameters are: power 400W, process gas is Ar gas;

[0051] 2) After plasma cleaning once, silver paste is printed on the surface of the battery cell by screen printing to form the grid line, and graphite powder is evenly sprayed on the surface of the battery cell. The liquid solvent in the silver paste has adhesion and can stick the graphite powder to the surface of the grid line. The particle size of the graphite powder is ≤1μm. The color of graphite is usually black or dark gray, and graphite is hygroscopic and can absorb moisture in the surrounding or air to wet the graphite powder. The silver paste is composed of: 80 parts by weight of silver powder; 10 parts by weight of epoxy resin, 0.5 parts by weight of methylimidazole, 5 parts by weight of butyl acetate, 6921.5 parts by weight of active diluent, 0.5 parts by weight of tetraethyl titanate and 0.5 parts by weight of polyamide wax; the particle size of the silver powder is ≤0.1μm.

[0052] 3) Annealing treatment, annealing temperature is 100 ° C, time is 40 minutes;

[0053] 4) Plasma secondary cleaning, specific parameters include: power 150W; process gas is N2 gas;

[0054] 5) Using conductive tape to connect the crystalline silicon cells into strings; using bus bars to connect the crystalline silicon cell strings in series and / or in parallel, laying a packaging film and a front glass on the front side, and laying a packaging film and a back panel material on the back side, and then laminating them to obtain a crystalline silicon solar cell module.

[0055] Example 2

[0056] This embodiment provides a method for preparing a crystalline silicon solar cell, which specifically includes the following steps:

[0057] 1) Plasma cleaning is used to clean the surface of the cell (including silicon wafer and film) at one time. The specific parameters are: power 300W, process gas is Ar gas;

[0058] 2) After the plasma cleaning, silver paste is printed on the silicon wafer by screen printing to form the grid line, and graphite powder is evenly sprayed on the surface of the cell, and the particle size of the graphite powder is 11-20 μm, wherein the silver paste is composed of: 82 parts by weight of silver powder; 8 parts by weight of epoxy resin, 0.1 parts by weight of methylimidazole, 6 parts by weight of butyl acetate, 6921 parts by weight of active diluent, 1 part by weight of tetraethyl titanate and 0.1 parts by weight of polyamide wax; the particle size of the silver powder is 0.1 μm-0.5 μm.

[0059] 3) Annealing treatment, annealing temperature is 200 ° C, time is 20 minutes;

[0060] 4) Plasma secondary cleaning, the specific parameters include: power 200W; process gas is N2 gas;

[0061] 5) Using a conductive tape to connect the crystalline silicon cells into strings; using a bus bar to connect the crystalline silicon cell strings in series and / or in parallel, laying a packaging film and a front glass on the front side, and laying a packaging film and a back plate material on the back side, and then laminating them to obtain a crystalline silicon solar cell module.

[0062] Example 3

[0063] This embodiment provides a method for preparing a crystalline silicon solar cell, which specifically includes the following steps:

[0064] 1) Plasma cleaning is used to clean the surface of the cell (including silicon wafer and film) at one time. The specific parameters are: power 500W, process gas is Ar gas;

[0065] 2) After the plasma cleaning, silver paste is printed on the silicon wafer by screen printing to form the gate line, and graphite powder is evenly sprayed on the surface of the cell, and the particle size of the graphite powder is 1-5 μm, wherein the silver paste is composed of: 78 parts by weight of silver powder; 12 parts by weight of epoxy resin, 1 part by weight of methylimidazole, 4 parts by weight of butyl acetate, 2 parts by weight of active diluent 692, 0.1 part by weight of tetraethyl titanate and 1 part by weight of polyamide wax; the particle size of the silver powder is 10 μm-40 μm.

[0066] 3) Annealing treatment, annealing temperature is 600℃, time is 15 minutes;

[0067] 4) Plasma secondary cleaning, the specific parameters include: power 100W; process gas is N2 gas;

[0068] 5) Using a conductive tape to connect the crystalline silicon cells into strings; using a bus bar to connect the crystalline silicon cell strings in series and / or in parallel, laying a packaging film and a front glass on the front side, and laying a packaging film and a back plate material on the back side, and then laminating them to obtain a crystalline silicon solar cell module.

[0069] Example 4

[0070] This embodiment provides a method for preparing a crystalline silicon solar cell, which is different from the first embodiment only in that 0.5 wt % silver powder with a particle size of ≤1 μm is doped into the graphite powder.

[0071] Example 5

[0072] This embodiment provides a method for preparing a crystalline silicon solar cell, which is different from Embodiment 4 only in that 0.1 wt % of silver powder is doped into the graphite powder.

[0073] Example 6

[0074] This embodiment provides a method for preparing a crystalline silicon solar cell, which is different from Embodiment 4 only in that 1 wt % of silver powder is doped into the graphite powder.

[0075] Example 7

[0076] This embodiment provides a method for preparing a crystalline silicon solar cell, which is different from the embodiment 4 only in that the particle size of the graphite powder is 6-10 μm.

[0077] Comparative Example 1

[0078] This embodiment provides a method for preparing a silicon crystalline solar cell, which is different from the embodiment 1 only in that in step 2, graphite powder is not sprayed on the surface of the cell.

[0079] The performance of the crystalline silicon solar cells prepared in the above embodiments and comparative examples was tested, wherein embodiments 1, 2, 4, 5, 6, 7 and the comparative example are all heterojunction cells, and embodiment 3 is a topcon cell, as shown in Table 1.

[0080] Table 1

[0081] Short circuit current Isc(A) Open circuit voltage Voc(V) Filling factor FF(%) Conversion efficiency Efficiency(%) Example 1 8.568 0.7426 80.29 23.17 Example 2 8.541 0.7421 80.89 23.25 Example 3 7.212 0.7079 73.88 22.86 Example 4 8.552 0.7436 81.63 23.54 Example 5 8.568 0.7464 81.63 23.68 Example 6 8.669 0.7463 81.9 24.03 Example 7 8.547 0.7414 81.32 23.46 Comparative Example 1 8.568 0.7426 80.29 23.17

[0082] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A crystalline silicon solar cell, characterized in that: include: A silicon wafer, a film covering a surface of the silicon wafer, and a gate line arranged on the film, wherein a surface of the gate line is covered with a graphite layer; The preparation method comprises: Printing grid lines on the film covering the surface of the silicon wafer, then covering the grid lines with graphite powder, and sequentially annealing and second cleaning the cell covered with graphite powder to obtain the crystalline silicon solar cell; Printing a silver paste on a silicon wafer to form the gate line, the silver paste comprising 78-82 parts by weight of silver powder, 8-12 parts by weight of epoxy resin and 5-11 parts by weight of additives; the additives comprising 0.1-1 parts by weight of a curing agent, methylimidazole, 4-6 parts by weight of an inactive diluent, 1-2 parts by weight of an active diluent 692, 0.1-1 parts by weight of an adhesion promoter, tetraethyl titanate, and 0.1-1 parts by weight of an anti-settling agent, polyamide wax; The graphite powder also includes conductive agent powder, the doping amount of the conductive agent is 0.1wt%-1wt%, and the average particle size of the graphite powder is less than 20μm.

2. The crystalline silicon solar cell according to claim 1, characterized in that: The graphite layer is doped with a conductive agent, and the conductive agent is selected from at least one of silver, copper, gold and aluminum.

3. The crystalline silicon solar cell according to claim 1, characterized in that: The crystalline silicon solar cell is a HJT heterogeneous crystalline silicon solar cell or a topcon crystalline silicon solar cell.

4. The crystalline silicon solar cell according to claim 1, characterized in that: The average particle size of the silver powder is less than 40 μm.

5. The crystalline silicon solar cell according to claim 1, characterized in that: The annealing temperature is 100°C-600°C.

6. The crystalline silicon solar cell according to claim 1, characterized in that: Before printing the gate lines, the cell is first cleaned by a plasma cleaning method, and the specific parameters include: power 300W-500W; process gas is at least one of Ar gas, O2 and CO2; And / or, the second cleaning adopts a plasma cleaning method, and specific parameters include: power 100W-200W; process gas is N2 gas.

7. A method for preparing a crystalline silicon solar cell module, characterized in that: The positive and negative electrodes of two or more crystalline silicon solar cells according to any one of claims 1 to 6 are connected in sequence using a conductive tape to prepare a crystalline silicon cell string; After the crystalline silicon cell strings are connected in series and / or in parallel by using busbars, a packaging film and a front plate glass are sequentially laid on the front side, and a packaging film and a back plate material are sequentially laid on the rear side, and then laminated to obtain a crystalline silicon solar cell module.