Preparation method and application of a hydroxyl-modified boron nitride adsorbent for synergistically removing so2 / no and heavy metals from high-temperature flue gas
By using hydroxyl-modified boron nitride adsorbent to adsorb heavy metals and SO2/NO in high-temperature flue gas, the problem of synergistic removal of SO2/NO and heavy metals in high-temperature flue gas was solved, achieving efficient and economical flue gas purification.
Patent Information
- Application Number
- CN202410716272.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-06-04
AI Technical Summary
Existing technologies are insufficient for the effective synergistic removal of SO2/NO and heavy metals, especially Cd, Pb, and Zn, from high-temperature flue gas, leading to environmental pollution and health threats.
Hydroxyl-modified boron nitride adsorbent is used. Hydroxyl radicals are generated on the surface of active boron nitride by irradiating hydrogen peroxide with ultraviolet light, which increases the active sites. Hydroxyl-modified boron nitride is then used to adsorb heavy metals and SO2/NO in high-temperature flue gas, converting them into particulate matter and capturing them.
It significantly improves the adsorption capacity of heavy metals and SO2/NO, reduces the concentration of harmful substances in flue gas, and is low-cost, clean and efficient, making it suitable for high-temperature flue gas treatment.
Smart Images

Figure BDA0004875672430000071 
Figure BDA0004875672430000072 
Figure BDA0004875672430000073
Abstract
Description
Technical Field
[0001] This invention belongs to the field of materials preparation technology, and in particular relates to a method for preparing and applying a hydroxyl-modified boron nitride adsorbent for synergistic removal of SO2 / NO and heavy metals from high-temperature flue gas. Background Technology
[0002] The emission of heavy metal pollutants is a significant factor contributing to the deterioration of the ecological environment. With the continuous increase in the amount of municipal solid waste incinerated, a large amount of heavy metal pollutants are generated during the incineration process, with Pb, Zn, and Cd being the most common. Non-volatile heavy metals accumulate in the bottom ash of the incinerator after incineration, while volatile heavy metals are released into the atmosphere with the flue gas, causing substantial heavy metal pollution to the environment.
[0003] Because heavy metals are highly toxic, persistent, and bioaccumulative, even low concentrations released into the environment can pose a threat to the ecosystem and human health. Furthermore, heavy metals and their compounds are not biodegradable, meaning they can directly enter the human body through the atmosphere and drinking water, causing damage to human organs.
[0004] Studies have shown that boron nitride has a strong adsorption capacity for heavy metals such as cadmium, lead, and zinc. Some scholars believe that the presence of acidic gases such as SO2 and NO in the flue gas from solid waste incineration can also affect the adsorption of heavy metals by adsorbents. Density functional theory (DFT) calculations have revealed that boron nitride nanosheets can adsorb acidic gases such as SO2 and NO. Since SO2 / NO has reducing properties, while most heavy metal oxides are oxidizing, it is hypothesized that boron nitride can simultaneously adsorb SO2 / NO and heavy metals, and the presence of SO2 / NO can promote the adsorption process of heavy metals by boron nitride.
[0005] Currently, the flue gas treatment technology for solid waste incineration is relatively mature. However, volatile heavy metals are released into the atmosphere along with the flue gas, which also contains toxic gases such as SO2 and NO. There are few reports on methods for the synergistic removal of SO2 / NO and heavy metals from the high-temperature flue gas after incineration.
[0006] In summary, developing a novel adsorbent material that can simultaneously remove SO2 / NO and heavy metals from high-temperature flue gas is an important problem that urgently needs to be solved. Summary of the Invention
[0007] In view of this, the present invention provides a method for preparing and applying a hydroxyl-modified boron nitride adsorbent for synergistic removal of SO2 / NO and heavy metals from high-temperature flue gas, in order to solve the problem that high-temperature flue gas after solid waste incineration contains toxic gases such as NO and SO2, as well as multiple heavy metals such as Cd, Pb, and Zn.
[0008] To achieve the above objectives, the technical solution of the present invention is as follows:
[0009] This invention provides a method for preparing a hydroxyl-modified boron nitride adsorbent that synergistically removes SO2 / NO and heavy metals from high-temperature flue gas. The method utilizes the decomposition of hydrogen peroxide under ultraviolet light to generate hydroxyl functional groups, which are then loaded onto the surface of active boron nitride to obtain hydroxyl-modified active boron nitride.
[0010] Preferably, the method is as follows: active boron nitride is placed in the middle of the lower temperature zone of a dual-temperature zone vertical furnace. Under a protective atmosphere, hydrogen peroxide is heated in the upper temperature zone of the dual-temperature zone vertical furnace and then passed through the active boron nitride. The hydrogen peroxide solution is heated in the upper temperature zone and then turns into hydrogen peroxide vapor. An ultraviolet light source is configured in the lower temperature zone of the dual-temperature zone vertical furnace to maintain a constant temperature for photochemical modification, thereby obtaining a hydroxyl-modified boron nitride adsorbent.
[0011] Preferably, the volume-to-mass ratio of hydrogen peroxide to active boron nitride is 2 ml / g, and the concentration of hydrogen peroxide is 10 wt%.
[0012] Preferably, the evaporation temperature of hydrogen peroxide in the upper temperature zone of the dual-temperature vertical furnace is 50-60℃.
[0013] Preferably, the photochemical modification temperature in the lower temperature zone of the dual-temperature vertical furnace is 80-90℃, and the photochemical modification time is 2-3h.
[0014] Preferably, the ultraviolet light source has a power of 5W and a wavelength of 254nm.
[0015] Preferably, the protective atmosphere is N2, and the gas flow rate is 250 ml / min.
[0016] Preferably, the method for preparing the active boron nitride includes the following steps:
[0017] 1) Weigh out melamine (C3N6H6) and boric acid (H3BO3) and add them to deionized water, stirring until they are evenly mixed;
[0018] 2) Heat and stir the mixture obtained in step 1) in a constant temperature water bath until the solution becomes clear;
[0019] 3) Cool the clear solution obtained in step 2) naturally until the solute has completely precipitated, filter, dry, and grind to obtain a solid powder;
[0020] 4) The solid powder obtained in step 3) is placed in a three-temperature zone tube furnace under a protective atmosphere for high-temperature activation, and then cooled to room temperature to obtain active boron nitride.
[0021] Preferably, in step 1), the molar ratio of melamine (C3N6H6), boric acid (H3BO3), and deionized water is 1:2:55.
[0022] Preferably, in step 1), the stirring time is 10 minutes and the stirring temperature is room temperature.
[0023] Preferably, in step 2), the heating temperature of the constant temperature water bath is 85°C, and the stirring time is 2 hours.
[0024] Preferably, in step 3), the natural cooling time is 4 hours, the drying temperature is 100°C, and the drying time is 24 hours.
[0025] Preferably, in step 4), the high-temperature activation temperature is 1350℃ and the activation time is 4h; the protective atmosphere is N2 and the gas flow rate is 200ml / min.
[0026] Another aspect of the present invention provides an application of the hydroxyl-modified boron nitride adsorbent prepared by the above-mentioned method. Two nozzles are arranged in the temperature zone of 900±50℃ in the furnace of an urban solid waste incinerator. The nozzles are connected to Venturi jets, which inject the hydroxyl-modified boron nitride material BN-OH into the furnace, while simultaneously adsorbing the mixed flue gas of heavy metals and SO2 / NO. The hydroxyl-modified boron nitride converts the gaseous heavy metals and SO2 / NO in the flue gas into particulate matter.
[0027] A bag filter is used at the end of the flue to capture hydroxyl-modified boron nitride and fly ash together, completing the combined capture of SO2 / NO and heavy metals by spraying hydroxyl-modified boron nitride adsorbent.
[0028] The beneficial effects of this invention are as follows:
[0029] 1. This invention utilizes ultraviolet light irradiation to promote the decomposition of hydrogen peroxide, generating hydroxyl radicals which are then loaded onto the surface of active boron nitride. This increases the number of active sites on the boron nitride surface. The hydroxyl radicals break the BN bonds on the boron nitride surface to form B-OH bonds. The B-OH bonds then form coordination bonds with heavy metals, converting the heavy metals into particulate form and promoting adsorption. Therefore, the hydroxyl-modified boron nitride prepared by this invention has a significantly higher adsorption capacity compared to active boron nitride. Specifically, under simulated flue gas conditions of 82% N2 + 12% CO2 + 6% O2, the Cu adsorption capacity increased by 13.5 mg / g, the Zn adsorption capacity increased by 8.8 mg / g, and the Cd adsorption capacity increased by 6.5 mg / g.
[0030] 2. The preparation method of this invention uses low-cost raw materials, consumes minimal reagents, is clean and efficient, and produces no toxic substances. The resulting adsorbent, compared to heavy metal adsorbents such as activated carbon, is heat-resistant and has broad application prospects in the field of high-temperature flue gas adsorption.
[0031] 3. During application, the hydroxyl-modified boron nitride adsorbent injected into the furnace of the municipal solid waste incinerator reacts with heavy metals and SO2 / NO in the high-temperature flue gas, significantly reducing the content of heavy metals and the concentration of SO2 / NO in the flue gas.
[0032] It should be understood that the above general description and the following detailed description are exemplary and explanatory only, and do not limit the disclosure of the present invention. Detailed Implementation
[0033] Exemplary embodiments will be described in detail below. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Rather, they are merely examples of systems consistent with some aspects of the present invention as detailed in the appended claims.
[0034] To address the problem that high-temperature flue gas after incineration contains toxic gases such as SO2 and NO, as well as multiple heavy metals such as Cd, Pb, and Zn, this implementation plan proposes a modified boron nitride adsorbent for the synergistic removal of SO2 / NO and heavy metals from high-temperature flue gas, along with a method for preparing the adsorbent. Furthermore, this adsorbent is applied using a method of spraying modified hydroxyl-modified boron nitride powder to simultaneously remove SO2 / NO and heavy metals such as Cd, Pb, and Zn.
[0035] A method for preparing a hydroxyl-modified boron nitride adsorbent for synergistic removal of SO2 / NO and heavy metals from high-temperature flue gas specifically includes the following steps:
[0036] (1) Weigh out melamine C3N6H6 and boric acid H3BO3 and add them to deionized water, stirring until they are evenly mixed;
[0037] (2) Heat and stir the mixture obtained in step (1) in a constant temperature water bath until the solution is clear;
[0038] (3) Cool the clear solution obtained in step (2) naturally until the solute is completely precipitated, filter, dry, and grind to obtain solid powder;
[0039] (4) The solid powder obtained in step (3) is placed in a three-temperature zone tube furnace under a protective atmosphere for high-temperature activation, and then cooled to room temperature to obtain active boron nitride.
[0040] (5) Place the active boron nitride obtained in step (4) into a quartz tube;
[0041] (6) Place the quartz tube from step (5) in the middle of the lower temperature zone of the dual-temperature vertical furnace. Under a protective atmosphere, heat the hydrogen peroxide in the upper temperature zone of the dual-temperature vertical furnace and then pass it through the active boron nitride. The hydrogen peroxide solution becomes hydrogen peroxide vapor after being heated in the upper temperature zone. An ultraviolet light source is configured in the lower temperature zone of the dual-temperature vertical furnace to maintain a constant temperature for photochemical modification, thereby obtaining a hydroxyl-modified boron nitride adsorbent.
[0042] In step (1), the molar ratio of melamine (C3N6H6), boric acid (H3BO3), and deionized water is 1:2:55; the stirring time is 10 min, and the stirring temperature is room temperature.
[0043] In step (2), the heating temperature of the constant temperature water bath is 85℃ and the stirring time is 2h.
[0044] In step (3), the natural cooling time is 4 hours, the drying temperature is 100°C, and the drying time is 24 hours.
[0045] In step (4), the high-temperature activation temperature is 1350℃ and the activation time is 4h; the protective atmosphere is N2 and the gas flow rate is 200ml / min.
[0046] In step (6), the volume-to-mass ratio of hydrogen peroxide to active boron nitride is 2 ml / g; the evaporation temperature of hydrogen peroxide in the upper temperature zone of the dual-temperature vertical furnace is 50-60℃; the photochemical modification temperature in the lower temperature zone of the dual-temperature vertical furnace is 80-90℃, and the photochemical modification time is 2-3 h; the power of the ultraviolet light source is 5 W, and the wavelength is 254 nm; the protective atmosphere is N2, and its gas flow rate is 250 ml / min.
[0047] This implementation scheme modifies boron nitride by using a precursor method to prepare it with hydroxyl groups, thereby changing the functional groups on the surface of boron nitride, increasing the number of active adsorption sites, and enhancing its chemisorption effect.
[0048] In the application of the above-mentioned hydroxyl-doped boron nitride catalyst, two nozzles are arranged in the temperature zone of 900±50℃ in the furnace of the municipal solid waste incinerator. The nozzles are connected to Venturi jets, which inject hydroxyl-modified boron nitride material BN-OH into the furnace, while simultaneously adsorbing the mixed flue gas of heavy metals and SO2 / NO.
[0049] Hydroxyl-modified boron nitride co-capture converts gaseous heavy metals and SO2 / NO in flue gas into particulate matter;
[0050] A bag filter is used at the end of the flue to capture hydroxyl-doped boron nitride particles and fly ash. The combined capture of SO2 / NO and heavy metals by the injection of hydroxyl-modified boron nitride adsorbent reduces the emission of harmful substances and protects the environment.
[0051] Other embodiments of the invention will readily occur to those skilled in the art upon consideration of the specification and practice of the invention disclosed herein. This application is intended to cover any variations, uses, or adaptations of the invention that follow the general principles of the invention and include common knowledge or customary techniques in the art not disclosed herein. The specification and examples are to be considered exemplary only, and the true scope and spirit of the invention are indicated by the claims.
[0052] To better illustrate the technical means and product effects of the present invention, the preferred embodiments of the present invention will be described below.
[0053] Example 1
[0054] A method for preparing a hydroxyl-modified boron nitride adsorbent for synergistic removal of SO2 / NO and heavy metals from high-temperature flue gas, comprising the following specific steps:
[0055] 1) First, add 19.366g C3N6H6 and 19g H3BO3 to 1000ml of deionized water at room temperature, place the mixture in an ultrasonic instrument and stir for 10 minutes at room temperature until it is evenly mixed to obtain a white liquid mixture;
[0056] 2) Heat the white liquid mixture obtained in step 1) to 85°C in a constant temperature water bath and stir for 2 hours until the solution is clear;
[0057] 3) Cool the clear solution obtained in step 2) naturally for 4 hours until the solute is completely precipitated, filter it and dry it in an oven at 100°C for 24 hours, then grind it to obtain a white solid powder;
[0058] 4) Place the white solid powder obtained in step 3) into a white corundum boat, put the white corundum boat into a three-temperature zone tube furnace and heat it in a nitrogen atmosphere (200 ml / min) at a heating rate of 10℃ / min. Calcinate at 1350℃ for 4 hours, and then cool naturally to room temperature in a nitrogen atmosphere to obtain white solid fiber active boron nitride.
[0059] 5) Weigh 0.1g of the white solid fiber active boron nitride obtained in step 4) and place it into a quartz tube;
[0060] 6) Place the quartz tube from step 5) in the middle of the lower temperature zone (85°C) of a dual-temperature vertical furnace. Under a nitrogen atmosphere (250 ml / min), use a laboratory micro-injection pump to heat 0.2 ml of 10 wt% hydrogen peroxide in the upper temperature zone (50°C) of the dual-temperature vertical furnace and then pass it through active boron nitride. The hydrogen peroxide solution turns into hydrogen peroxide vapor after being heated in the upper temperature zone. The lower temperature zone of the dual-temperature vertical furnace is equipped with a 5W, 254nm ultraviolet light source, and the temperature is kept constant for photochemical modification for 3 hours to obtain hydroxyl-modified boron nitride adsorbent.
[0061] Based on the characteristics of high-temperature flue gas from urban solid waste incinerators, the flue gas composition was simulated using N2 + 12 vol% CO2 + 6 vol% O2 + 500 ppm SO2, N2 + 12 vol% CO2 + 6 vol% O2 + 300 ppm NO, and N2 + 12% CO2 + 6% O2 + 300 ppm NO + 500 ppm SO2. Nitrogen was used as the balance gas, and the gas flow rate was 500 ml / min. Heavy metal chloride salts were added to simulate heavy metals in the flue gas, specifically CuCl2, ZnCl2, and CdCl2, with 5 g each added. The mixture was placed in the left temperature zone of a dual-temperature zone tubular furnace and incinerated at 1000℃. 0.15 g of hydroxyl-modified boron nitride was placed in the right temperature zone of the dual-temperature zone tubular furnace and heated to 400℃ for 2 hours. The experiment was conducted under the same conditions using an atmosphere of 82% N2 + 12% CO2 + 6% O2. The experimental exhaust gas was treated using an absorption method of 10% nitric acid solution + 5% sodium hydroxide solution. During the experiment, after the gas flow stabilized, the SO2 / NO concentration at the tail end was repeatedly measured using a portable infrared flue gas analyzer. The SO2 / NO removal efficiency is shown in Table 1. After the experiment, the heavy metal content in the hydroxyl-modified boron nitride bottom slag was detected using an inductively coupled plasma atomic emission spectrometer after digestion. The results are shown in Table 2.
[0062] Table 1. Removal efficiency of SO2 / NO by hydroxyl-modified boron nitride under simulated flue gas.
[0063]
[0064] Table 2. Adsorption capacity (mg / g) of heavy metals by hydroxyl-modified boron nitride under simulated flue gas.
[0065]
[0066] As shown in Table 1-2, the addition of SO2 and NO to the simulated flue gas significantly increased the heavy metal content in the bottom ash of the hydroxyl-modified boron nitride material. Therefore, it can be concluded that the hydroxyl-modified boron nitride material can jointly adsorb SO2 / NO and various heavy metals. Simultaneously, the presence of SO2 / NO can promote the capture of heavy metals by the hydroxyl-modified boron nitride material, indicating a synergistic effect between the two.
[0067] Example 2
[0068] The operation steps in this embodiment are the same as in Embodiment 1, except that the concentrations of SO2 and NO in the simulated flue gas are increased. Gas mixtures are prepared using N2 + 12% CO2 + 6% O2 + 700ppm SO2, N2 + 12% CO2 + 6% O2 + 400ppm NO, and N2 + 12% CO2 + 6% O2 + 400ppm NO + 700ppm SO2. The SO2 / NO concentration at the tail end is measured multiple times using a portable infrared flue gas analyzer. The SO2 / NO removal efficiency is shown in Table 3. After digestion, the heavy metal content in the hydroxyl-modified boron nitride bottom slag is measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES). The results are shown in Table 4.
[0069] Table 3. Removal efficiency of SO2 / NO by hydroxyl-modified boron nitride under simulated flue gas.
[0070]
[0071]
[0072] Table 4. Adsorption capacity (mg / g) of heavy metals by hydroxyl-modified boron nitride under simulated flue gas.
[0073]
[0074] As shown in Table 3-4, increasing the SO2 / NO concentration in the simulated flue gas significantly increased the heavy metal content in the bottom ash of the hydroxyl-modified boron nitride material. Therefore, it can be concluded that the hydroxyl-modified boron nitride material can jointly adsorb SO2 / NO and various heavy metals. Simultaneously, the presence of SO2 / NO can promote the capture of heavy metals by the modified boron nitride material, indicating a synergistic effect between the two.
[0075] Comparative Example 1
[0076] Using activated boron nitride as the adsorbent, the operation steps were the same as in Example 1. The SO2 / NO concentration at the tail end was measured multiple times using a portable infrared flue gas analyzer, and the SO2 / NO removal efficiency is shown in Table 5. After digestion, the heavy metal content in the activated boron nitride bottom residue was measured using an inductively coupled plasma atomic emission spectrometer, and the results are shown in Table 6.
[0077] Table 5. Removal efficiency of SO2 / NO by hydroxyl-modified boron nitride under simulated flue gas.
[0078]
[0079] Table 6. Adsorption capacity (mg / g) of heavy metals by active boron nitride under simulated flue gas.
[0080]
[0081]
[0082] Based on the data from the above examples, it can be seen that the prepared hydroxyl-modified boron nitride material has outstanding adsorption performance and can effectively adsorb SO2 / NO and various heavy metals in the high-temperature flue gas from municipal solid waste incineration.
[0083] The above embodiments are merely preferred embodiments of the present invention and are not intended to limit the implementation. The scope of protection of the present invention should be determined by the scope defined in the claims. Other variations or modifications can be made based on the above description. Obvious variations or modifications derived therefrom are still within the scope of protection of the present invention.
Claims
1. The application of a hydroxyl-modified boron nitride adsorbent in the synergistic removal of SO2 / NO and heavy metals from high-temperature flue gas, characterized in that, Two nozzles are arranged in the temperature zone of 900±50℃ inside the furnace of the municipal solid waste incinerator. The nozzles are connected to Venturi jets. The Venturi jets inject hydroxyl-modified boron nitride material BN-OH into the furnace, which simultaneously adsorbs the mixed flue gas of heavy metals and SO2 / NO. The hydroxyl-modified boron nitride converts the gaseous heavy metals and SO2 / NO in the flue gas into particulate matter. A bag filter is used at the end of the flue to capture hydroxyl-modified boron nitride and fly ash together, thus completing the combined capture of SO2 / NO and heavy metals by spraying hydroxyl-modified boron nitride adsorbent. The preparation method of the hydroxyl-modified boron nitride adsorbent is as follows: active boron nitride is placed in the middle of the lower temperature zone of a dual-temperature zone vertical furnace. Under a protective atmosphere, hydrogen peroxide is heated in the upper temperature zone of the dual-temperature zone vertical furnace and then passed through the active boron nitride. The hydrogen peroxide solution is heated in the upper temperature zone and then turns into hydrogen peroxide vapor. An ultraviolet light source is configured in the lower temperature zone of the dual-temperature zone vertical furnace to maintain a constant temperature for photochemical modification, thereby obtaining the hydroxyl-modified boron nitride adsorbent.
2. The application according to claim 1, characterized in that, The volume-to-mass ratio of hydrogen peroxide to active boron nitride is 2 ml / g.
3. The application according to claim 1, characterized in that, The evaporation temperature of hydrogen peroxide in the upper temperature zone of the dual-temperature vertical furnace is 50-60℃.
4. The application according to claim 1, characterized in that, The photochemical modification temperature in the lower temperature zone of the dual-temperature vertical furnace is 80-90℃, and the photochemical modification time is 2-3h.
5. The application according to claim 1, characterized in that, The ultraviolet light source has a power of 5W and a wavelength of 254nm.
6. The application according to claim 1, characterized in that, The protective atmosphere is N2, and the gas flow rate is 250 ml / min.
7. The application according to claim 1, characterized in that, The method for preparing the active boron nitride includes the following steps: 1) Weigh out melamine (C3N6H6) and boric acid (H3BO3) and add them to deionized water, stirring until they are evenly mixed; 2) Heat and stir the mixture obtained in step 1) in a constant temperature water bath until the solution becomes clear; 3) Cool the clear solution obtained in step 2) naturally until the solute has completely precipitated, filter, dry, and grind to obtain a solid powder; 4) The solid powder obtained in step 3) is placed in a three-temperature zone tube furnace under a protective atmosphere for high-temperature activation, and then cooled to room temperature to obtain active boron nitride.
Citation Information
Patent Citations
Hexagonal boron nitride nanosheet and preparation method thereof
CN114804042A
Platinum-conductive diamond composite antipolar catalyst, preparation method and fuel cell
CN117199409A