Temperature-resistant and salt-resistant fluid loss reducer for drilling fluid and preparation method and application method thereof

By combining copolymers such as acrylamide and materials such as polyaryletherketone, a temperature-resistant and salt-resistant filtration loss agent that maintains high performance under high temperature and high salt conditions is solved, and the temperature resistance and resistance of the filter loss agent in the prior art is solved. The problem of poor salt performance significantly reduces the filtration loss of drilling fluid and improves the stability of drilling fluid.

CN118685155BActive Publication Date: 2024-12-06DONGYING XINLIN PETROLEUM TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411194422.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The current filtration reduction agent for drilling fluid has poor performance under high temperature and high salt conditions, especially inadequate temperature and salt resistance, and has poor performance when used in combination with coating inhibitors.

Method used

The combined effect of acrylamide, vinylpyrrolidone, 2-acrylamide-2-methylpropanesulfonic acid, polyaryletherketone, hydrolyzed polyacrylonitrile-ammonium salt, bentonite, and octadecyltrimethylammonium chloride , a temperature and salt filtration loss agent that maintains high performance under high salt conditions of 245°C was prepared, and a dense membrane layer was formed by polyaryletherketone to reduce filtration loss and protect the drilling fluid.

Benefits of technology

Under high salt conditions of 245℃, the filter reduction loss agent did not decompose or degrade, maintaining high performance, significantly reducing the filtration loss of the drilling fluid, improving the stability and performance of the drilling fluid, and is suitable for coating inhibitors containing amide groups. drilling fluid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to the technical field of fluid loss reducer production, specifically to a temperature-resistant and salt-resistant fluid loss reducer for drilling fluid, and a preparation method and an application method thereof. The temperature-resistant and salt-resistant fluid loss reducer for drilling fluid is composed of the following raw materials in parts by weight: 20-30 parts of acrylamide; 10-15 parts of vinyl pyrrolidone; 3-5 parts of hydrolyzed polyacrylonitrile-ammonium salt; 4-6 parts of polyaryletherketone; 5-7 parts of octadecyltrimethylammonium chloride; 40-50 parts of 2-acrylamide-2-methylpropanesulfonic acid; 15-20 parts of bentonite; 1-3 parts of ammonium persulfate; 1-3 parts of sodium bisulfite; and 5-8 parts of phenylenediamine. The fluid loss reducer prepared by the present invention can still maintain high performance under high-salt conditions of 245°C without decomposition or degradation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fluid loss reducer production, in particular to a temperature-resistant and salt-resistant fluid loss reducer for drilling fluid and a preparation method and an application method thereof. Background Art

[0002] Fluid loss additives are key treatment agents in drilling fluids, primarily used to reduce fluid loss during the drilling process. They play a crucial role in maintaining stable drilling fluid performance, ensuring safe and efficient drilling and production, and protecting reservoirs and oil formations. A key issue facing fluid loss additives in drilling fluids is their poor temperature and salt tolerance. This is particularly true under high-temperature and high-salinity conditions, severely impacting the performance of traditional polymer fluid loss additives.

[0003] Under high-temperature and high-salinity conditions, performance issues with fluid loss additives primarily manifest in several areas: First, high temperatures can cause polymer degradation or cross-linking, leading to rheological deterioration such as thickening, gelling, solidification, or thickening, resulting in instability in the drilling fluid system. Second, in high-salinity environments, insufficient salt tolerance of polymers can cause clay particles in the drilling fluid to aggregate and grow, reducing their surface area and inhibiting the dispersion of clay particles, thereby increasing fluid loss. Furthermore, when fluid loss additives are applied to drilling fluids, they are often used in conjunction with coated inhibitors. High temperature and high salinity conditions can also affect the performance of coated inhibitors (especially those containing amide groups, which are widely used on the market), potentially causing them to decompose or degrade, reducing their effectiveness and, in turn, affecting the performance of the drilling fluid.

[0004] Chinese patent application CN111875758A, published on November 3, 2020, discloses a method for preparing an environmentally friendly, ultra-high-temperature-resistant fluid loss additive for water-based drilling fluids. The method involves first reacting nano-hectorite with a silane coupling agent to produce a nano-crosslinker. Subsequently, in the presence of the nano-crosslinker and an initiator, an inverse emulsion polymerization process is used to polymerize an amide monomer, a high-temperature-resistant monomer, a cationic monomer, and a polyene monomer to produce the environmentally friendly, ultra-high-temperature-resistant fluid loss additive. While this method provides a high-temperature-resistant fluid loss additive, it is not suitable for use in high-salinity environments. Chinese patent application CN110437361A, published on November 12, 2019, discloses a high-temperature-resistant and salt-resistant copolymer-based water-based drilling fluid fluid loss reducer, its preparation method, and its application. The preparation method comprises: (1) dissolving the polymer monomer in water and adjusting the pH value to 5-8; (2) adding an initiator to the above solution and reacting it at 60-80°C for 2-5 hours under mechanical stirring; (3) freeze-drying and crushing the viscous polymer aqueous solution after the reaction to obtain a solid water-based drilling fluid fluid loss reducer. Although the polymer has certain high-temperature and salt-resistant properties, its temperature resistance is only up to 180°C, which is obviously insufficient.

[0005] In summary, the filtrate reducers prepared by the prior art still have the problem of poor high temperature and salt resistance, and the problem of poor drilling fluid performance when used in combination with coated inhibitors. Summary of the Invention

[0006] In view of the above deficiencies in the prior art, the object of the present invention is to provide a temperature-resistant and salt-resistant fluid loss reducer for drilling fluid, which is copolymerized with acrylamide and vinyl pyrrolidone, 2-acrylamide-2-methylpropane sulfonic acid, and the combined effects of polyaryletherketone, hydrolyzed polyacrylonitrile-ammonium salt, bentonite, octadecyltrimethylammonium chloride and bentonite, so that it can still maintain high performance under high-salt conditions of 245°C without decomposition or degradation.

[0007] Another object of the present invention is to provide a method for preparing a temperature-resistant and salt-resistant fluid loss reducer for drilling fluid, which has mild preparation conditions, fewer steps, and is conducive to industrial production.

[0008] The third object of the present invention is to provide an application method of a temperature-resistant and salt-resistant fluid loss reducer for drilling fluid, which is used for the preparation of drilling fluid, especially for the preparation of drilling fluid containing an amide group-coated inhibitor.

[0009] The present invention is achieved by adopting the following technical solutions:

[0010] The temperature-resistant and salt-resistant fluid loss reducer for drilling fluid is composed of the following raw materials in parts by weight: 20-30 parts of acrylamide; 10-15 parts of vinyl pyrrolidone; 3-5 parts of hydrolyzed polyacrylonitrile-ammonium salt; 4-6 parts of polyaryletherketone; 5-7 parts of octadecyltrimethylammonium chloride; 40-50 parts of 2-acrylamide-2-methylpropanesulfonic acid; 15-20 parts of bentonite; 1-3 parts of ammonium persulfate; 1-3 parts of sodium bisulfite; and 5-8 parts of phenylenediamine.

[0011] The number average molecular weight of the polyaryletherketone is 30,000-50,000, and the particle size is 30-45 μm; the polyaryletherketone is one of polyetheretherketone or polyetherketoneketone.

[0012] The bentonite is sodium bentonite with a particle size of 25-45 μm.

[0013] The phenylenediamine is 3,5-dinitro-1,2-phenylenediamine.

[0014] The preparation method of the temperature-resistant and salt-resistant fluid loss reducer for drilling fluid comprises the following steps:

[0015] (1) Dissolve 2-acrylamide-2-methylpropanesulfonic acid in water according to the mass ratio, control the system temperature at 15-18°C, adjust the pH to 6-7, then add acrylamide and vinyl pyrrolidone, adjust the pH to 7-9, add octadecyltrimethylammonium chloride to the system, then introduce nitrogen and heat to 54-56°C;

[0016] (2) Keeping the temperature of step (1) unchanged, add phenylenediamine, ammonium persulfate and sodium bisulfite to the reaction system according to the mass ratio, and continue the reaction at 54-56°C for 1-1.5 hours to obtain a gel product;

[0017] (3) Dissolve the gel product in water, heat it to 70-73°C, add hydrolyzed polyacrylonitrile-ammonium salt and polyaryletherketone according to the mass ratio, react for 1-1.5 hours, add bentonite with stirring, and continue to react for 2-4 hours. After the reaction is completed, wash, dry and crush the product to obtain a temperature-resistant and salt-resistant fluid loss reducer for drilling fluid.

[0018] In the step (1), the nitrogen gas is introduced for 10-12 minutes; and the pH value is adjusted using NaOH.

[0019] The step (2) further comprises washing, precipitating and filtering the gel-like product; washing is performed using acetone for 0.5-1 h.

[0020] The application method of the temperature-resistant and salt-resistant fluid loss reducer for drilling fluid comprises the following steps:

[0021] a. Bentonite and sodium carbonate were added to water and stirred for 6-8h, and allowed to stand for 20-24h to obtain a pre-hydrated base slurry;

[0022] b. Add the drilling fluid temperature and salt resistance fluid loss reducer, polyethylene glycol, sulfonated phenolic resin, tartaric acid, coating inhibitor, and barite powder to the pre-hydrated base slurry in sequence, and adjust the pH value of the system to 9-10 with NaOH to obtain the drilling fluid.

[0023] The weight proportions of the raw materials in step a and step b are: 5-8 parts of bentonite; 0.3-0.8 parts of sodium carbonate; 95-103 parts of water; 2-5 parts of a temperature-resistant and salt-resistant fluid loss reducer for drilling fluid; 3-5 parts of polyethylene glycol; 5-6 parts of a sulfonated phenolic resin; 0.1-0.2 parts of tartaric acid; 0.1-0.2 parts of a coating inhibitor; and 50-55 parts of barite powder.

[0024] The coating inhibitor is a coating inhibitor containing an amide group.

[0025] Acrylamide is copolymerized with vinyl pyrrolidone and 2-acrylamido-2-methylpropanesulfonic acid to form a salt-tolerant, hydrophilic, and high-temperature resistant polymer chain, providing the basic backbone for the fluid loss additive. Furthermore, the interaction between polyaryletherketone (PEK) and hydrolyzed polyacrylonitrile-ammonium salt creates a stable network structure within the system, improving the overall performance of the drilling fluid. The interaction between bentonite, hydrolyzed polyacrylonitrile-ammonium salt, and octadecyltrimethylammonium chloride creates a stable colloidal system, preventing particle aggregation and sedimentation. PEEK has the ability to form a dense film on the surface of the drilling fluid or filter cake, sealing pores and reducing fluid loss. Under high temperature conditions, the film-forming properties of PEEK are further enhanced, forming a more stable and dense film. The PEEK film acts as a physical barrier, preventing water and solid particles in the drilling fluid from leaching through the wellbore wall into the formation. This barrier effect helps reduce fluid loss, maintain wellbore stability, and prevent formation damage. Bentonite can introduce functional groups between clay layers through ion exchange, enhancing the performance of the fluid loss additive and serving as support points for the macromolecular chain, increasing its thermal stability and mechanical strength. Functional groups (such as amide groups) in the fluid loss additive may strengthen the double electron layer of the bentonite layer, increasing the repulsive force between bentonite layers and contributing to the formation of a stable structure. Ammonium persulfate and sodium bisulfite are used as initiators to initiate the polymerization of monomers such as acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, and vinyl pyrrolidone, controlling the rate and extent of the polymerization reaction. Ammonium persulfate and sodium bisulfite decompose to produce free radicals, initiating polymerization between monomers. Phenylenediamine is used as a crosslinker to increase the crosslink density of the polymer.

[0026] When the fluid loss control agent prepared in this invention is used in drilling fluids prepared with an amide-containing coating inhibitor, the amide group (-CONH-) is subject to hydrolysis under high-temperature, high-salinity conditions, severely impacting its performance. However, poly(aryletherketone) forms a dense protective film on the surface of the amide-coated inhibitor. Specific groups (such as ether and ketone groups) within the poly(aryletherketone) molecules adsorb to the amide-coated inhibitor molecules or particle surfaces, forming an initial bond. As adsorption proceeds, the poly(aryletherketone) molecules gradually diffuse across the coating inhibitor surface and form an ordered film. This film not only protects the amide-coated inhibitor from degradation by the high-temperature, high-salinity environment but also reduces its direct contact with drilling fluids or formation fluids. The molecular structure of poly(aryletherketone) lends it a certain adsorption capacity for amide-coated inhibitor molecules. This adsorption may be enhanced under high-temperature, high-salinity conditions, contributing to the formation of a more stable coating and preventing the dispersion and aggregation of solid particles. After forming a film on the surface of the coated inhibitor, polyaryletherketone does not reduce the effect of the coated inhibitor, but rather enhances its effect. The film-formed polyaryletherketone can provide an additional protective layer to prevent the coated inhibitor from failing in harsh environments such as high temperature and high salt. At the same time, the polyaryletherketone film layer can also improve the interaction between the coated inhibitor and the drilling fluid or formation fluid, thereby improving the stability and performance of the drilling fluid.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The present invention prepares a temperature-resistant and salt-resistant fluid loss reducer for drilling fluid by copolymerizing acrylamide with vinyl pyrrolidone and 2-acrylamide-2-methylpropane sulfonic acid, and the combined action of polyaryletherketone, hydrolyzed polyacrylonitrile-ammonium salt, bentonite, octadecyltrimethylammonium chloride and bentonite, so that the drilling fluid can still maintain high performance under high-salt conditions of 245°C without decomposition or degradation.

[0029] (2) The preparation method of the present invention has mild preparation conditions and fewer steps, which is conducive to industrial production.

[0030] (3) The temperature-resistant and salt-resistant fluid loss reducer for drilling fluid prepared by the present invention is used for the preparation of drilling fluid, especially for the preparation of drilling fluid containing an amide group-coated inhibitor. DETAILED DESCRIPTION

[0031] The present invention is further described below with reference to the following examples, but they do not limit the implementation of the present invention.

[0032] Example 1

[0033] A temperature- and salt-resistant fluid loss reducer for drilling fluids is composed of the following raw materials in parts by weight: 25 parts acrylamide; 13 parts vinyl pyrrolidone; 4 parts hydrolyzed polyacrylonitrile ammonium salt; 5 parts polyaryletherketone; 6 parts octadecyltrimethylammonium chloride; 45 parts 2-acrylamido-2-methylpropanesulfonic acid; 18 parts bentonite; 2 parts ammonium persulfate; 2 parts sodium bisulfite; and 6 parts phenylenediamine. The polyaryletherketone has a number-average molecular weight of 40,000 and a particle size of 40 μm; the polyaryletherketone is polyetheretherketone. The bentonite is sodium bentonite with a particle size of 40 μm. The phenylenediamine is 3,5-dinitro-1,2-phenylenediamine.

[0034] The preparation method of the above-mentioned temperature-resistant and salt-resistant fluid loss reducer for drilling fluid comprises the following steps:

[0035] (1) 2-Acrylamide-2-methylpropanesulfonic acid was dissolved in water according to the mass ratio. The system temperature was controlled at 16°C and the pH was adjusted to 7. Then, acrylamide and vinyl pyrrolidone were added and the pH was adjusted to 8. Octadecyltrimethylammonium chloride was added to the system and nitrogen was introduced. The temperature was raised to 55°C. The nitrogen introduction time was 11 minutes. NaOH was used to adjust the pH value.

[0036] (2) Keeping the temperature of step (1) unchanged, add phenylenediamine, ammonium persulfate and sodium bisulfite to the reaction system according to the mass ratio, continue to react at 55°C for 1.5 hours to obtain a gel product, wash the gel product with acetone for 1 hour, and then precipitate and filter;

[0037] (3) The filtered gel product is dissolved in water, heated to 72°C, and then hydrolyzed polyacrylonitrile-ammonium salt and polyaryletherketone are added according to the mass ratio. The reaction is carried out for 1.5 hours. Bentonite is added with stirring and the reaction is continued for 3 hours. After the reaction is completed, the product is washed, dried, and crushed to obtain a temperature-resistant and salt-resistant fluid loss reducer for drilling fluid.

[0038] Example 2

[0039] A temperature- and salt-resistant fluid loss reducer for drilling fluids is composed of the following raw materials in parts by weight: 30 parts acrylamide; 15 parts vinyl pyrrolidone; 5 parts hydrolyzed polyacrylonitrile ammonium salt; 6 parts polyaryletherketone; 7 parts octadecyltrimethylammonium chloride; 50 parts 2-acrylamido-2-methylpropanesulfonic acid; 20 parts bentonite; 3 parts ammonium persulfate; 3 parts sodium bisulfite; and 8 parts phenylenediamine. The polyaryletherketone has a number-average molecular weight of 50,000 and a particle size of 45 μm; the polyaryletherketone is polyetherketoneketone. The bentonite is sodium bentonite with a particle size of 45 μm. The phenylenediamine is 3,5-dinitro-1,2-phenylenediamine.

[0040] The preparation method of the above-mentioned temperature-resistant and salt-resistant fluid loss reducer for drilling fluid comprises the following steps:

[0041] (1) Dissolve 2-acrylamide-2-methylpropanesulfonic acid in water according to the mass ratio, control the system temperature at 15°C, adjust the pH to 6, then add acrylamide and vinyl pyrrolidone, adjust the pH to 7, add octadecyltrimethylammonium chloride to the system, then introduce nitrogen, and raise the temperature to 54°C. The nitrogen introduction time is 10 minutes; NaOH is used to adjust the pH value;

[0042] (2) Keeping the temperature of step (1) unchanged, add phenylenediamine, ammonium persulfate and sodium bisulfite to the reaction system according to the mass ratio, continue to react at 54°C for 1 hour to obtain a gel product, wash the gel product with acetone for 0.5 hours, and then precipitate and filter;

[0043] (3) The filtered gel product is dissolved in water, heated to 70°C, and then hydrolyzed polyacrylonitrile-ammonium salt and polyaryletherketone are added according to the mass ratio. The reaction is continued for 1 hour, and bentonite is added with stirring. The reaction is continued for 2 hours. After the reaction is completed, the product is washed, dried, and crushed to obtain a temperature-resistant and salt-resistant fluid loss reducer for drilling fluid.

[0044] Example 3

[0045] A temperature- and salt-resistant fluid loss reducer for drilling fluids is composed of the following raw materials in parts by weight: 20 parts acrylamide; 10 parts vinyl pyrrolidone; 3 parts hydrolyzed polyacrylonitrile ammonium salt; 4 parts polyaryletherketone; 5 parts octadecyltrimethylammonium chloride; 40 parts 2-acrylamido-2-methylpropanesulfonic acid; 15 parts bentonite; 1 part ammonium persulfate; 1 part sodium bisulfite; and 5 parts phenylenediamine. The polyaryletherketone has a number-average molecular weight of 30,000 and a particle size of 30 μm; the polyaryletherketone is polyetheretherketone. The bentonite is sodium bentonite with a particle size of 25 μm. The phenylenediamine is 3,5-dinitro-1,2-phenylenediamine.

[0046] The preparation method of the above-mentioned temperature-resistant and salt-resistant fluid loss reducer for drilling fluid comprises the following steps:

[0047] (1) Dissolve 2-acrylamide-2-methylpropanesulfonic acid in water according to the mass ratio, control the system temperature at 18°C, adjust the pH to 7, then add acrylamide and vinyl pyrrolidone, adjust the pH to 9, add octadecyltrimethylammonium chloride to the system, then introduce nitrogen, and raise the temperature to 56°C. The nitrogen introduction time is 12 minutes; NaOH is used to adjust the pH value;

[0048] (2) Keeping the temperature of step (1) unchanged, add phenylenediamine, ammonium persulfate and sodium bisulfite to the reaction system according to the mass ratio, continue to react at 56°C for 1.5 hours to obtain a gel product, wash the gel product with acetone for 1 hour, and then precipitate and filter;

[0049] (3) The filtered gel product is dissolved in water, heated to 73°C, and then hydrolyzed polyacrylonitrile-ammonium salt and polyaryletherketone are added according to the mass ratio. The reaction is carried out for 1.5 hours. Bentonite is added with stirring and the reaction is continued for 4 hours. After the reaction is completed, the product is washed, dried, and crushed to obtain a temperature-resistant and salt-resistant fluid loss reducer for drilling fluid.

[0050] Example 4

[0051] A temperature- and salt-resistant fluid loss reducer for drilling fluids is composed of the following raw materials in parts by weight: 28 parts acrylamide; 14 parts vinyl pyrrolidone; 5 parts hydrolyzed polyacrylonitrile ammonium salt; 6 parts polyaryletherketone; 7 parts octadecyltrimethylammonium chloride; 48 parts 2-acrylamido-2-methylpropanesulfonic acid; 17 parts bentonite; 3 parts ammonium persulfate; 3 parts sodium bisulfite; and 8 parts phenylenediamine. The polyaryletherketone has a number-average molecular weight of 70,000 and a particle size of 60 μm; the polyaryletherketone is polyetherketone. The bentonite is sodium bentonite with a particle size of 30 μm. The phenylenediamine is 3,5-dinitro-1,2-phenylenediamine.

[0052] The preparation method of the above-mentioned temperature-resistant and salt-resistant fluid loss reducer for drilling fluid comprises the following steps:

[0053] (1) Dissolve 2-acrylamide-2-methylpropanesulfonic acid in water according to the mass ratio, control the system temperature at 15°C, adjust the pH to 6-7, then add acrylamide and vinyl pyrrolidone, adjust the pH to 7, add octadecyltrimethylammonium chloride to the system, then introduce nitrogen, and raise the temperature to 54°C. The nitrogen introduction time is 10 minutes; NaOH is used to adjust the pH value;

[0054] (2) Keeping the temperature of step (1) unchanged, add phenylenediamine, ammonium persulfate and sodium bisulfite to the reaction system according to the mass ratio, continue to react at 54°C for 1 hour to obtain a gel product, wash the gel product with acetone for 0.5 hours, and then precipitate and filter;

[0055] (3) The filtered gel product is dissolved in water, heated to 70°C, and then hydrolyzed polyacrylonitrile-ammonium salt and polyaryletherketone are added according to the mass ratio. The reaction is continued for 1 hour, and bentonite is added with stirring. The reaction is continued for 2 hours. After the reaction is completed, the product is washed, dried, and crushed to obtain a temperature-resistant and salt-resistant fluid loss reducer for drilling fluid.

[0056] Example 5

[0057] A temperature- and salt-resistant fluid loss reducer for drilling fluids is composed of the following raw materials in parts by weight: 28 parts acrylamide; 10 parts vinyl pyrrolidone; 5 parts hydrolyzed polyacrylonitrile ammonium salt; 6 parts polyaryletherketone; 7 parts octadecyltrimethylammonium chloride; 50 parts 2-acrylamido-2-methylpropanesulfonic acid; 20 parts bentonite; 3 parts ammonium persulfate; 3 parts sodium bisulfite; and 8 parts phenylenediamine. The polyaryletherketone has a number-average molecular weight of 50,000 and a particle size of 45 μm; the polyaryletherketone is polyetherketoneketone. The bentonite is calcium-based bentonite with a particle size of 80 μm. The phenylenediamine is 3,5-dinitro-1,2-phenylenediamine.

[0058] The preparation method of the above-mentioned temperature-resistant and salt-resistant fluid loss reducer for drilling fluid comprises the following steps:

[0059] (1) Dissolve 2-acrylamide-2-methylpropanesulfonic acid in water according to the mass ratio, control the system temperature at 15°C, adjust the pH to 6, then add acrylamide and vinyl pyrrolidone, adjust the pH to 7, add octadecyltrimethylammonium chloride to the system, then introduce nitrogen, and raise the temperature to 54°C. The nitrogen introduction time is 10 minutes; NaOH is used to adjust the pH value;

[0060] (2) Keeping the temperature of step (1) unchanged, add phenylenediamine, ammonium persulfate and sodium bisulfite to the reaction system according to the mass ratio, continue to react at 54°C for 1 hour to obtain a gel product, wash the gel product with acetone for 0.5 hours, and then precipitate and filter;

[0061] (3) The filtered gel product is dissolved in water, heated to 70°C, and then hydrolyzed polyacrylonitrile-ammonium salt and polyaryletherketone are added according to the mass ratio. The reaction is continued for 1 hour, and bentonite is added with stirring. The reaction is continued for 2 hours. After the reaction is completed, the product is washed, dried, and crushed to obtain a temperature-resistant and salt-resistant fluid loss reducer for drilling fluid.

[0062] Example 6

[0063] A temperature- and salt-resistant fluid loss reducer for drilling fluid is composed of the following raw materials in parts by weight: 25 parts acrylamide; 10 parts vinyl pyrrolidone; 3 parts hydrolyzed polyacrylonitrile ammonium salt; 4 parts polyaryletherketone; 7 parts octadecyltrimethylammonium chloride; 40 parts 2-acrylamido-2-methylpropanesulfonic acid; 15 parts bentonite; 1 part ammonium persulfate; 1 part sodium bisulfite; and 8 parts phenylenediamine. The polyaryletherketone has a number-average molecular weight of 30,000 and a particle size of 30 μm; the polyaryletherketone is polyetheretherketone. The bentonite is sodium bentonite with a particle size of 25 μm. The phenylenediamine is 1,3-phenylenediamine.

[0064] The preparation method of the above-mentioned temperature-resistant and salt-resistant fluid loss reducer for drilling fluid comprises the following steps:

[0065] (1) Dissolve 2-acrylamide-2-methylpropanesulfonic acid in water according to the mass ratio, control the system temperature at 18°C, adjust the pH to 7, then add acrylamide and vinyl pyrrolidone, adjust the pH to 9, add octadecyltrimethylammonium chloride to the system, then introduce nitrogen, and raise the temperature to 56°C. The nitrogen introduction time is 12 minutes; NaOH is used to adjust the pH value;

[0066] (2) Keeping the temperature of step (1) unchanged, add phenylenediamine, ammonium persulfate and sodium bisulfite to the reaction system according to the mass ratio, continue to react at 56°C for 1.5 hours to obtain a gel product, wash the gel product with acetone for 1 hour, and then precipitate and filter;

[0067] (3) The filtered gel product is dissolved in water, heated to 73°C, and then hydrolyzed polyacrylonitrile-ammonium salt and polyaryletherketone are added according to the mass ratio. The reaction is carried out for 1.5 hours. Bentonite is added with stirring and the reaction is continued for 4 hours. After the reaction is completed, the product is washed, dried, and crushed to obtain a temperature-resistant and salt-resistant fluid loss reducer for drilling fluid.

[0068] Example 7

[0069] A temperature- and salt-resistant fluid loss reducer for drilling fluids is composed of the following raw materials in parts by weight: 30 parts acrylamide; 12 parts vinyl pyrrolidone; 5 parts hydrolyzed polyacrylonitrile ammonium salt; 4 parts polyaryletherketone; 7 parts octadecyltrimethylammonium chloride; 50 parts 2-acrylamido-2-methylpropanesulfonic acid; 20 parts bentonite; 3 parts ammonium persulfate; 3 parts sodium bisulfite; and 5 parts phenylenediamine. The polyaryletherketone has a number-average molecular weight of 50,000 and a particle size of 45 μm; the polyaryletherketone is polyetherketoneketone. The bentonite is sodium bentonite with a particle size of 45 μm. The phenylenediamine is 3,5-dinitro-1,2-phenylenediamine.

[0070] The preparation method of the above-mentioned temperature-resistant and salt-resistant fluid loss reducer for drilling fluid comprises the following steps:

[0071] (1) Dissolve 2-acrylamide-2-methylpropanesulfonic acid in water according to the mass ratio, control the system temperature at 15°C, adjust the pH to 6, then add acrylamide and vinyl pyrrolidone, adjust the pH to 7, add octadecyltrimethylammonium chloride to the system, then introduce nitrogen, and raise the temperature to 54°C. The nitrogen introduction time is 5 minutes; the pH value is adjusted by KOH;

[0072] (2) Keeping the temperature of step (1) unchanged, add phenylenediamine, ammonium persulfate and sodium bisulfite to the reaction system according to the mass ratio, continue to react at 54°C for 1 hour to obtain a gel product, wash the gel product with acetone for 0.5 hours, and then precipitate and filter;

[0073] (3) The filtered gel product is dissolved in water, heated to 70°C, and then hydrolyzed polyacrylonitrile-ammonium salt and polyaryletherketone are added according to the mass ratio. The reaction is continued for 1 hour, and bentonite is added with stirring. The reaction is continued for 2 hours. After the reaction is completed, the product is washed, dried, and crushed to obtain a temperature-resistant and salt-resistant fluid loss reducer for drilling fluid.

[0074] Example 8

[0075] A temperature- and salt-resistant fluid loss reducer for drilling fluids is composed of the following raw materials in parts by weight: 30 parts acrylamide; 10 parts vinyl pyrrolidone; 3 parts hydrolyzed polyacrylonitrile ammonium salt; 4 parts polyaryletherketone; 7 parts octadecyltrimethylammonium chloride; 40 parts 2-acrylamido-2-methylpropanesulfonic acid; 15 parts bentonite; 1 part ammonium persulfate; 1 part sodium bisulfite; and 5 parts phenylenediamine. The polyaryletherketone has a number-average molecular weight of 40,000 and a particle size of 40 μm; the polyaryletherketone is polyetheretherketone. The bentonite is sodium bentonite with a particle size of 25 μm. The phenylenediamine is 3,5-dinitro-1,2-phenylenediamine.

[0076] The preparation method of the above-mentioned temperature-resistant and salt-resistant fluid loss reducer for drilling fluid comprises the following steps:

[0077] (1) Dissolve 2-acrylamide-2-methylpropanesulfonic acid in water according to the mass ratio, control the system temperature at 18°C, adjust the pH to 7, then add acrylamide and vinyl pyrrolidone, adjust the pH to 9, add octadecyltrimethylammonium chloride to the system, then introduce nitrogen, and raise the temperature to 56°C. The nitrogen introduction time is 12 minutes; NaOH is used to adjust the pH value;

[0078] (2) Keeping the temperature of step (1) unchanged, add phenylenediamine, ammonium persulfate and sodium bisulfite to the reaction system according to the mass ratio, and continue the reaction at 56°C for 1.5 hours to obtain a gel-like product;

[0079] (3) The gel product was dissolved in water, heated to 73°C, and then hydrolyzed polyacrylonitrile-ammonium salt and polyaryletherketone were added according to the mass ratio. The reaction was continued for 1.5 hours. Bentonite was added with stirring and the reaction was continued for 4 hours. After the reaction was completed, the product was washed, dried, and crushed to obtain a temperature-resistant and salt-resistant fluid loss reducer for drilling fluid.

[0080] Comparative Example 1

[0081] The difference from Example 1 is that polyaryletherketone was not added.

[0082] Comparative Example 2

[0083] The difference from Example 1 is that vinyl pyrrolidone and phenylenediamine were not added.

[0084] Comparative Example 3

[0085] The difference from Example 1 is that bentonite and hydrolyzed polyacrylonitrile-ammonium salt are not added.

[0086] Comparative Example 4

[0087] The difference from Example 1 is that the pH is not adjusted in step (1).

[0088] Comparative Example 5

[0089] The difference from Example 1 is that in step (3), bentonite, hydrolyzed polyacrylonitrile-ammonium salt and polyaryletherketone are added together into the gel product for reaction.

[0090] Application Example 1

[0091] The application method of the temperature-resistant and salt-resistant fluid loss reducer for drilling fluid comprises the following steps:

[0092] a. Bentonite and sodium carbonate were successively added to water and stirred for 7h, and allowed to stand for 22h to obtain a pre-hydrated base slurry;

[0093] b. The fluid loss additive obtained in Example 1, polyethylene glycol, sulfonated phenolic resin, tartaric acid, polyacrylamide, and barite powder were sequentially added to the prehydrated base slurry, and the pH value of the system was adjusted to 9 with NaOH to obtain a drilling fluid.

[0094] In the above application method, the weight parts of each raw material are: 6 parts of bentonite; 0.5 parts of sodium carbonate; 100 parts of water; 3 parts of fluid loss reducer; 4 parts of polyethylene glycol; 6 parts of sulfonated phenolic resin; 0.2 parts of tartaric acid; 0.2 parts of polyacrylamide; and 53 parts of barite powder.

[0095] Application Example 2

[0096] The application method of the temperature-resistant and salt-resistant fluid loss reducer for drilling fluid comprises the following steps:

[0097] a. The bentonite and sodium carbonate were successively added to water and stirred for 8h, and allowed to stand for 24h to obtain a pre-hydrated base slurry;

[0098] b. The fluid loss additive obtained in Example 2, polyethylene glycol, sulfonated phenolic resin, tartaric acid, polyacrylamide, and barite powder were sequentially added to the prehydrated base slurry, and the pH value of the system was adjusted to 10 with NaOH to obtain a drilling fluid.

[0099] In the above application method, the weight parts of each raw material are: 5 parts of bentonite; 0.3 parts of sodium carbonate; 95 parts of water; 2 parts of fluid loss reducer; 3 parts of polyethylene glycol; 5 parts of sulfonated phenolic resin; 0.1 parts of tartaric acid; 0.1 parts of polyacrylamide; and 50 parts of barite powder.

[0100] Application Example 3

[0101] The application method of the temperature-resistant and salt-resistant fluid loss reducer for drilling fluid comprises the following steps:

[0102] a. Bentonite and sodium carbonate were added to water and stirred for 6h, and allowed to stand for 20h to obtain a pre-hydrated base slurry;

[0103] b. The fluid loss reducer obtained in Example 3, polyethylene glycol, sulfonated phenolic resin, tartaric acid, polyacrylamide, and barite powder were sequentially added to the prehydrated base slurry, and the pH value of the system was adjusted to 9 with NaOH to obtain a drilling fluid.

[0104] In the above application method, the weight parts of each raw material are: 8 parts of bentonite; 0.8 parts of sodium carbonate; 103 parts of water; 5 parts of fluid loss reducer; 5 parts of polyethylene glycol; 6 parts of sulfonated phenolic resin; 0.2 parts of tartaric acid; 0.2 parts of polyacrylamide; and 55 parts of barite powder.

[0105] Application Example 4

[0106] The difference from Application Example 1 is that the fluid loss reducer is the fluid loss reducer obtained in Example 4.

[0107] Application Example 5

[0108] The difference from Application Example 1 is that the fluid loss reducer is the fluid loss reducer obtained in Example 5.

[0109] Application Example 6

[0110] The difference from Application Example 1 is that the fluid loss reducer is the fluid loss reducer obtained in Example 6.

[0111] Application Example 7

[0112] The difference from Application Example 1 is that the fluid loss reducer is the fluid loss reducer obtained in Example 7.

[0113] Application Example 8

[0114] The difference from Application Example 1 is that the fluid loss reducer is the fluid loss reducer obtained in Example 8.

[0115] Comparative Application Example 1

[0116] The difference from Application Example 1 is that the fluid loss reducer is the fluid loss reducer obtained in Comparative Example 1.

[0117] Application Comparative Example 2

[0118] The difference from Application Example 1 is that the fluid loss reducer is the fluid loss reducer obtained in Comparative Example 2.

[0119] Application Comparative Example 3

[0120] The difference from Application Example 1 is that the fluid loss reducer is the fluid loss reducer obtained in Comparative Example 3.

[0121] Comparative Application Example 4

[0122] The difference from Application Example 1 is that the fluid loss reducer is the fluid loss reducer obtained in Comparative Example 4.

[0123] Application Comparative Example 5

[0124] The difference from Application Example 1 is that the fluid loss reducer is the fluid loss reducer obtained in Comparative Example 5.

[0125] Application Comparative Example 6

[0126] The difference from Application Example 1 is that sulfonated asphalt is used as the coating inhibitor.

[0127] With reference to GB16783.1-2014 "Field Testing of Drilling Fluids in the Petroleum and Natural Gas Industry Part 1: Water-Based Drilling Fluids", the performance of Application Examples 1-8 and Application Comparative Examples 1-6 were evaluated.

[0128] The core plugging rate test method is as follows: take 400mL drilling fluid, add 36wt% NaCl, stir at 5000rpm for 25min, put it into an aging tank, put it into a roller furnace, roll it at a constant temperature of 245℃ for 16h, take it out and cool it to room temperature, and then stir it at 5000rpm for 20min. The core plugging rate is tested as follows: on the core flow test instrument, use the drilling fluid contamination holder to measure the initial forward standard brine permeability K1 of the rock sample. Then remove the core contamination holder and connect it to the drilling fluid high temperature and high pressure dynamic comprehensive tester. Use the above drilling fluid to positively plug the rock sample. The drilling fluid temperature is 85℃, the pressure difference is 3.5MPa, the confining pressure is 5MPa, and the shear rate is 150s. -1 After 30 minutes of damage, the core contamination holder was removed and connected to the core flow tester to measure the core forward standard brine permeability K2. The core plugging rate is:

[0129] .

[0130] The test data of Application Examples 1-8 are shown in Table 1.

[0131] The test data of Comparative Examples 1-6 are shown in Table 2.

[0132] Table 1 Test data of application examples 1-8

[0133]

[0134] Table 2 Test data of comparative examples 1-6

[0135]

[0136] Data analysis of the application examples and comparative examples shows that the fluid loss reducer prepared by the present invention can withstand an operating environment of 245°C and 36% NaCl concentration, and the core plugging rate can reach 97.8%. A comparison of the data of application example 1, application comparative example 1, and application comparative example 6 shows that polyaryletherketone plays a vital role in the formation of the overall network structure. At the same time, the polyaryletherketone film layer acts as a physical barrier to prevent water and solid particles in the drilling fluid from filtering through the well wall into the formation. This barrier effect helps reduce the amount of drilling fluid loss, protect the well wall stability, and prevent formation damage. It can also form a dense protective film on the surface of the amide-coated inhibitor, improving the overall performance of the drilling fluid. A comparison of the data of application example 1, application comparative example 2, and application comparative example 3 shows that vinylpyrrolidone and phenylenediamine play a very important role in the polymerization of the polymer chain skeleton structure; bentonite and hydrolyzed polyacrylonitrile-ammonium salt stabilize the functional groups, improving the overall performance of the fluid loss reducer.

Claims

1. A temperature-resistant and salt-resistant fluid loss reducer for drilling fluid, characterized in that: The invention is composed of the following raw materials in parts by weight: 20-30 parts of acrylamide; 10-15 parts of vinyl pyrrolidone; 3-5 parts of hydrolyzed polyacrylonitrile-ammonium salt; 4-6 parts of polyaryletherketone; 5-7 parts of octadecyltrimethylammonium chloride; 40-50 parts of 2-acrylamide-2-methylpropanesulfonic acid; 15-20 parts of bentonite; 1-3 parts of ammonium persulfate; 1-3 parts of sodium bisulfite; 5-8 parts of phenylenediamine; The polyaryletherketone has a number average molecular weight of 30,000-50,000 and a particle size of 30-45 μm; the polyaryletherketone is one of polyetheretherketone or polyetherketoneketone; The phenylenediamine is 3,5-dinitro-1,2-phenylenediamine; The preparation method of the temperature-resistant and salt-resistant fluid loss reducer for drilling fluid comprises the following steps: (1) Dissolve 2-acrylamide-2-methylpropanesulfonic acid in water according to the mass ratio, control the system temperature at 15-18°C, adjust the pH to 6-7, then add acrylamide and vinyl pyrrolidone, adjust the pH to 7-9, add octadecyltrimethylammonium chloride to the system, then introduce nitrogen and raise the temperature to 54-56°C; (2) Keeping the temperature of step (1) unchanged, add phenylenediamine, ammonium persulfate and sodium bisulfite to the reaction system according to the mass ratio, and continue to react at 54-56° C. for 1-1.5 hours to obtain a gel product; (3) Dissolve the gel product in water, heat it to 70-73°C, add hydrolyzed polyacrylonitrile-ammonium salt and polyaryletherketone according to the mass ratio, react for 1-1.5 hours, add bentonite with stirring, and continue to react for 2-4 hours. After the reaction is completed, wash, dry and crush the product to obtain a temperature-resistant and salt-resistant fluid loss reducer for drilling fluid.

2. The temperature-resistant and salt-resistant fluid loss reducer for drilling fluid according to claim 1, characterized in that: The bentonite is sodium-based bentonite with a particle size of 25-45 μm.

3. The temperature-resistant and salt-resistant fluid loss reducer for drilling fluid according to claim 1, characterized in that: In the step (1), the nitrogen is introduced for 10-12 minutes; and the pH value is adjusted using NaOH.

4. The temperature-resistant and salt-resistant fluid loss reducer for drilling fluid according to claim 1, characterized in that: The step (2) further comprises washing, precipitating and filtering the gel product; the washing is performed with acetone for a washing time of 0.5-1 h.

5. A method for applying the temperature-resistant and salt-resistant fluid loss reducer for drilling fluid according to any one of claims 1 to 4, characterized in that: The following steps are involved: a. Add bentonite and sodium carbonate to water and stir for 6-8h, let stand for 20-24h to obtain a pre-hydrated base slurry; b. Add the temperature-resistant and salt-resistant fluid loss reducer, polyethylene glycol, sulfonated phenolic resin, tartaric acid, coating inhibitor and barite powder to the prehydrated base slurry in sequence, and adjust the pH value of the system to 9-10 with NaOH to obtain the drilling fluid.

6. The application method of the temperature-resistant and salt-resistant fluid loss reducer for drilling fluid according to claim 5, characterized in that: The weight proportions of the raw materials in step a and step b are as follows: 5-8 parts of bentonite; 0.3-0.8 parts of sodium carbonate; 95-103 parts of water; 2-5 parts of temperature-resistant and salt-resistant fluid loss reducer for drilling fluid; 3-5 parts of polyethylene glycol; 5-6 parts of sulfonated phenolic resin; 0.1-0.2 parts of tartaric acid; 0.1-0.2 parts of coating inhibitor; 50-55 parts of barite powder.

7. The application method of the temperature-resistant and salt-resistant fluid loss reducer for drilling fluid according to claim 5, characterized in that: The coating inhibitor is a coating inhibitor containing an amide group.

Citation Information

Patent Citations

  • High-temperature-resistant salt-resistant copolymer-type water-based drilling fluid loss reducing agent as well as preparation method and application thereof

    CN110437361A

  • Preparation method of environment-friendly ultrahigh-temperature-resistant filtrate reducer for water-based drilling fluid

    CN111875758A

  • High-temperature-resistant salt-resistant polymer filtrate reducer used in water-based drilling fluid and preparation method thereof

    CN104388061A

  • Fluids and methods for treating hydrocarbon-bearing formations

    CN107771203A