A ceramic plate imitating natural materials and preparation method thereof

By using modified aluminum silicate fibers and additives, the compressive strength and breaking modulus of ceramic sheets are improved, and the problems of easy breakage and high water absorption of ceramic sheets are solved, and its mechanical properties and durability are enhanced.

CN118702476BActive Publication Date: 2024-11-01GUANGZHOU MEGA BUILDING MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411178656.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-01
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The existing ceramic plates have uneven density, low strength, easy to break, and may fall off or crack under external forces or humid environments after installation, affecting the appearance and safety of the building.

Method used

Modified aluminum silicate fibers and modified additives are prepared by chemical reactions and copolymerization to enhance the compressive strength and breakage modulus of ceramic plates, and a mesh structure is formed by modifying additives to improve the density and permeability of the plates. ability.

Benefits of technology

The compressive strength and breaking modulus of ceramic plates are improved, the water absorption rate is reduced, the mechanical properties and durability of the plates are enhanced, and the quality problems in external forces and humid environments are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the field of building ceramics, and discloses a ceramic plate imitating natural materials and a preparation method thereof. The ceramic plate imitating natural materials comprises the following components in parts by weight: 40-60 parts of ceramic waste, 8-15 parts of blast furnace slag, 10-20 parts of wollastonite, 5-10 parts of modified aluminum silicate fiber, 4-8 parts of modified additives, 5-15 parts of water glass, 10-15 parts of potassium feldspar, 1-5 parts of expansion agent, and 1-3 parts of foaming agent; the modified aluminum silicate fiber is prepared by grafting carboxylated kaolin with aluminum silicate fiber through γ-aminopropyltriethoxysilane by chemical reaction; the modified additive is prepared by copolymerizing modified nano titanium dioxide, modified graphene oxide, styrene and hydroxyethyl methacrylate under the action of an initiator azobisisobutyronitrile. The invention provides the ceramic plate with higher compressive strength and rupture modulus by adding the modified aluminum silicate fiber and the modified additive, is not easy to break, and has low water absorption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building ceramics, and in particular relates to a ceramic plate imitating natural materials and a preparation method thereof. Background Art

[0002] As people's living standards improve, their aesthetics become more personalized in the selection of decoration and finishing materials, and they pay more attention to style and taste. There is also an increasing demand for the application of finishing materials such as walls, floors, curtain walls, furniture, cabinets, countertops, etc. in modern decoration. The existing finishing materials mainly include natural stone and artificial quartz. Among them, artificial quartz refers to a plate formed by vibrating and pressing resin, quartz, and colorant and curing at 100~200℃. Because it contains resin materials, it has low hardness, poor acid and alkali resistance, and is not resistant to high temperatures. Natural stone has relatively high hardness, good high temperature resistance, and rich color, but natural stone resources are extremely limited.

[0003] In recent years, ceramic panels imitating natural materials have been gradually applied to the field of decoration. They have excellent acid and alkali resistance, high temperature resistance and other advantages, and have extremely broad application prospects. However, the existing ceramic panels have uneven density and low strength. The panels are easy to break during processing or transportation, which brings inconvenience to construction. In addition, after installation, ceramic panels will cause serious quality problems such as falling off and cracking under the action of external forces such as vibration, impact, and extrusion, as well as in a humid environment. This not only affects the appearance of the building, but also poses certain hidden dangers to the safety of building decoration. Summary of the invention

[0004] In order to solve the deficiencies mentioned in the above background technology, the purpose of the present invention is to provide a ceramic plate imitating natural materials and a preparation method thereof. By adding modified aluminum silicate fiber and modified additives, the ceramic plate is given higher compressive strength and rupture modulus, is not easy to break, and has low water absorption.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A ceramic plate imitating natural materials, comprising the following components by weight: 40-60 parts of ceramic waste, 8-15 parts of blast furnace slag, 10-20 parts of wollastonite, 5-10 parts of modified aluminum silicate fiber, 4-8 parts of modified additives, 5-15 parts of water glass, 10-15 parts of potassium feldspar, 1-5 parts of expansion agent, and 1-3 parts of foaming agent;

[0007] The modified aluminum silicate fiber is prepared by grafting carboxylated kaolin with aluminum silicate fiber through γ-aminopropyltriethoxysilane by chemical reaction; the modified additive is prepared by copolymerizing modified nano titanium dioxide, modified graphene oxide, styrene and hydroxyethyl methacrylate under the action of initiator azobisisobutyronitrile.

[0008] Preferably, the ceramic waste is composed of the following by mass percentage: SiO2: 66~68%, Al2O3: 15~17%, MgO: 3.5~5.5%, CaO: 1.5~2%, Na2O: 2.5~3.5%, K2O: 2~3%, Fe2O3: 0.8~1.1% and the remainder impurities.

[0009] Preferably, the ceramic waste and blast furnace slag have a mesh size of 300 to 500 meshes.

[0010] Preferably, the preparation method of the modified aluminum silicate fiber comprises the following steps:

[0011] A. Take γ-aminopropyltriethoxysilane and succinic anhydride in N, N-dimethylformamide, stir at 70-85°C for 3-4 hours to obtain a mixed solution, ultrasonically disperse kaolin in N, N-dimethylformamide, then add deionized water and mix, add to the mixed solution, stir at 40-50°C for 2-4 hours, centrifuge, wash and dry after the reaction is completed to prepare carboxylated kaolin;

[0012] B. Soak the aluminum silicate fiber in a hydrochloric acid solution for 5-6 hours to remove surface impurities, then soak it in a sodium hydroxide solution and place it at 75-85° C. for 10-12 hours to prepare pretreated aluminum silicate fiber;

[0013] C. Take carboxylated kaolin and disperse it in N,N-dimethylformamide by ultrasonic. Add dicyclohexylcarbodiimide, γ-aminopropyltriethoxysilane and pretreated aluminum silicate fiber. Stir at 55-70°C for 4-7h. After the reaction is completed, centrifuge and dry to prepare modified aluminum silicate fiber.

[0014] Preferably, in step C, the mass ratio of carboxylated kaolin, γ-aminopropyltriethoxysilane and pretreated aluminum silicate fiber is 1-2.5:2.4-5:4-6.

[0015] Preferably, the preparation method of the modified additive comprises the following steps:

[0016] (1) Ultrasonic dispersion of nano-titanium dioxide in a mixed solution of ethanol and deionized water, dropwise addition of glacial acetic acid to adjust the pH value of the system to 4-6, heating to 70-85°C, adding γ-methacryloxypropyltrimethoxysilane to react for 8-12 hours, and filtering, washing and drying after the reaction to obtain modified nano-titanium dioxide;

[0017] (2) ultrasonically dispersing graphene oxide in deionized water to obtain a dispersion, dissolving p-phenylenediamine in deionized water and adding it to the dispersion, ultrasonically mixing and reacting at 40-55°C for 20-24 hours, filtering, washing and drying after the reaction to obtain amino graphene oxide, and then placing amino graphene oxide and glycidyl methacrylate in a reactor, reacting at 90-110°C for 2-3 hours to prepare modified graphene oxide;

[0018] (3) In a nitrogen atmosphere, anhydrous ethanol, modified nano-titanium dioxide, modified graphene oxide, styrene and hydroxyethyl methacrylate are placed in a reactor and stirred to mix evenly at room temperature. Then, azobisisobutyronitrile is added and the temperature is raised to 70-80°C for reaction for 6-8 hours. After the reaction is completed, the mixture is cooled to room temperature, and the modified additive is prepared by rotary evaporation, precipitation and drying.

[0019] Preferably, in step (3), the mass ratio of modified nano titanium dioxide, modified graphene oxide, styrene and hydroxyethyl methacrylate is 3.2-3.6:6-8:1-1.2:1.2-1.4.

[0020] Preferably, the method for preparing the ceramic plate imitating natural materials comprises the following steps:

[0021] S1, adding parts by weight of ceramic waste, blast furnace slag, wollastonite, expansion agent, foaming agent, water glass, and potassium feldspar to a ball mill, and wet-milling for 10 to 18 hours to obtain a premix;

[0022] S2, taking the premix, the modified aluminum silicate fiber and the modified additive into a mixer and mixing them evenly to obtain a mixture;

[0023] S3, transporting the mixed material to the aging warehouse for aging treatment for 8-12 hours to obtain aged material, the aging treatment temperature is 35-45°C, and the aging humidity is 30-50%;

[0024] S4, transferring the aged material into a blank mold, and extruding it at 80-90 MPa to obtain a formed blank;

[0025] S5. The formed blank is cured, demolded, sintered at 1100-1200°C for 1-3h, cooled to room temperature, and edge-ground to obtain a ceramic plate imitating natural materials.

[0026] Beneficial effects of the present invention:

[0027] The ceramic plate for preparing the imitation natural material of the present invention is prepared by mixing ceramic waste, blast furnace slag, wollastonite, modified aluminum silicate fiber, modified additive, water glass, potassium feldspar, expansion agent and foaming agent according to certain weight parts. The present invention uses γ-aminopropyl triethoxysilane and succinic anhydride to modify kaolin, so that carboxyl groups are grafted on the surface of kaolin, and γ-aminopropyl triethoxysilane is used as a bridging agent, and the amino group at one end of the γ-aminopropyl triethoxysilane and the carboxyl group on the surface of kaolin undergo amidation reaction, and the silanol group at the other end of the γ-aminopropyl triethoxysilane undergoes condensation reaction with the hydroxyl group on the surface of the pretreated aluminum silicate fiber, so that the kaolin is grafted on the surface of the aluminum silicate fiber through the silane coupling agent, the roughness of the surface of the aluminum silicate fiber is increased, thereby increasing the mechanical bite force and chemical bonding force between the aluminum silicate fiber and the matrix, and reducing the porosity of the plate, slowing down the penetration of water, and at the same time, the addition of the modified aluminum silicate fiber can give the plate excellent compressive strength and rupture modulus. In addition, the present invention uses γ-methacryloxypropyltrimethoxysilane to treat nano titanium dioxide, and at the same time, graphene oxide and p-phenylenediamine are grafted and then further grafted with glycidyl methacrylate, thereby introducing double bond structures on the surfaces of nano titanium dioxide and graphene oxide as bridges for polymerization with styrene and hydroxyethyl methacrylate, thereby preparing a modified additive. The molecular chains in the modified additive are intertwined to form a network structure, connecting the components together, improving the compactness of the board, and improving the anti-seepage ability. In addition, the modified additive is added to the board to effectively fill the internal pores of the matrix, improve the compactness of the board, reduce the later stress accumulation, and thus enhance the mechanical properties and durability of the board. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1 A method for preparing modified aluminum silicate fiber comprises the following steps:

[0030] A. Take 2g of γ-aminopropyltriethoxysilane and 1g of succinic anhydride in 50mL of N,N-dimethylformamide, stir at 85°C for 3h to obtain a mixed solution, take 3g of kaolin and ultrasonically disperse it in 100mL of N,N-dimethylformamide, then add 5mL of deionized water and mix, add to the mixed solution, stir at 45°C for 3h, centrifuge, wash and dry after the reaction is completed to prepare carboxylated kaolin;

[0031] B. Take 5g of aluminum silicate fiber and soak it in 0.1mol / L hydrochloric acid solution for 6h to remove surface impurities, then soak it in 1mol / L sodium hydroxide solution and place it at 80°C for 12h to prepare pretreated aluminum silicate fiber;

[0032] C. Take 2g of carboxylated kaolin and ultrasonically disperse it in 100mL of N,N-dimethylformamide, add 0.3g of dicyclohexylcarbodiimide, 3.2g of γ-aminopropyltriethoxysilane and 5g of pretreated aluminum silicate fiber, stir at 60°C for 5h, and after the reaction is completed, centrifuge and dry to prepare modified aluminum silicate fiber.

[0033] Example 2 A method for preparing a modified additive comprises the following steps:

[0034] (1) 2 g of nano-titanium dioxide was ultrasonically dispersed in a mixed solution of 34 mL of ethanol and 6 mL of deionized water, glacial acetic acid was added dropwise to adjust the pH value of the system to 5, the temperature was raised to 75 °C, γ-methacryloxypropyltrimethoxysilane was added and reacted for 12 h. After the reaction was completed, the modified nano-titanium dioxide was obtained by filtering, washing and drying;

[0035] (2) 0.8 g of graphene oxide was ultrasonically dispersed in 100 mL of deionized water to obtain a dispersion, 1.2 g of p-phenylenediamine was dissolved in 100 mL of deionized water and added to the dispersion, ultrasonically mixed and reacted at 45° C. for 24 h. After the reaction was completed, the mixture was filtered, washed and dried to obtain amino-modified graphene oxide. Then 1 g of amino-modified graphene oxide and 1.42 g of glycidyl methacrylate were placed in a reactor and reacted at 105° C. for 2 h to prepare modified graphene oxide.

[0036] (3) In a nitrogen atmosphere, 120 mL of anhydrous ethanol, 3.3 g of modified nano-titanium dioxide, 6.5 g of modified graphene oxide, 1 g of styrene and 1.3 g of hydroxyethyl methacrylate were placed in a reactor and stirred to mix evenly at room temperature. Then, 0.4 g of azobisisobutyronitrile was added and the mixture was heated to 80 °C and reacted for 7 h. After the reaction was completed, the mixture was cooled to room temperature and subjected to rotary evaporation, precipitation and drying to obtain a modified additive.

[0037] Example 3 A ceramic plate imitating natural materials, including 42 parts of ceramic waste, 8 parts of blast furnace slag, 10 parts of wollastonite, 5 parts of modified aluminum silicate fiber prepared in Example 1, 4 parts of modified additive prepared in Example 2, 7 parts of water glass, 10 parts of potassium feldspar, 1 part of calcium oxide expansion agent, and 1 part of hydrogen peroxide foaming agent.

[0038] The method for preparing the ceramic plate imitating natural materials comprises the following steps:

[0039] S1, adding parts by weight of ceramic waste, blast furnace slag, wollastonite, expansion agent, foaming agent, water glass, and potassium feldspar to a ball mill, and wet-milling for 16 hours to obtain a premix;

[0040] S2, taking the premix, the modified aluminum silicate fiber and the modified additive into a mixer and mixing them evenly to obtain a mixture;

[0041] S3, transporting the mixed material to an aging warehouse for aging treatment for 12 hours to obtain an aged material, the aging treatment temperature is 40°C, and the aging humidity is 35%;

[0042] S4, transferring the aged material into a green body mold, and extruding it at 85 MPa to obtain a formed green body;

[0043] S5. The formed blank is cured, demolded, sintered at 1100° C. for 1 hour, cooled to room temperature, and edge-ground to obtain a ceramic plate imitating natural materials.

[0044] Example 4 A ceramic plate imitating natural materials, including 55 parts of ceramic waste, 12 parts of blast furnace slag, 15 parts of wollastonite, 8 parts of modified aluminum silicate fiber prepared in Example 1, 6 parts of modified additive prepared in Example 2, 10 parts of water glass, 12 parts of potassium feldspar, 3 parts of calcium oxide expansion agent, and 2 parts of hydrogen peroxide foaming agent.

[0045] The preparation method of the above-mentioned ceramic plate imitating natural materials is the same as that of Example 3.

[0046] Example 5 A ceramic plate imitating natural materials, including 60 parts of ceramic waste, 15 parts of blast furnace slag, 18 parts of wollastonite, 10 parts of modified aluminum silicate fiber prepared in Example 1, 8 parts of modified additive prepared in Example 2, 14 parts of water glass, 15 parts of potassium feldspar, 5 parts of calcium oxide expansion agent, and 3 parts of hydrogen peroxide foaming agent.

[0047] The preparation method of the above-mentioned ceramic plate imitating natural materials is the same as that of Example 3.

[0048] Comparative Example 1 A ceramic plate imitating natural materials includes 60 parts of ceramic waste, 15 parts of blast furnace slag, 18 parts of wollastonite, 10 parts of aluminum silicate fiber, 8 parts of the modified additive prepared in Example 2, 14 parts of water glass, 15 parts of potassium feldspar, 5 parts of calcium oxide expansion agent, and 3 parts of hydrogen peroxide foaming agent.

[0049] The preparation method of the above-mentioned ceramic plate imitating natural materials is the same as that of Example 3.

[0050] Comparative Example 2 A ceramic plate imitating natural materials includes 60 parts of ceramic waste, 15 parts of blast furnace slag, 18 parts of wollastonite, 10 parts of modified aluminum silicate fiber prepared in Example 1, 14 parts of water glass, 15 parts of potassium feldspar, 5 parts of calcium oxide expansion agent, and 3 parts of hydrogen peroxide foaming agent.

[0051] The preparation method of the above-mentioned ceramic plate imitating natural materials is the same as that of Example 3.

[0052] Performance Testing

[0053] The ceramic plates prepared in Examples 3-5 and Comparative Examples 1-2 were subjected to performance tests: the compressive strength was tested using a universal testing machine, the sample size was 100mm×100mm×40mm, and the loading speed was 0.5mm / min; the modulus of rupture was tested with reference to GB / T 3810.4-2016; the water absorption was tested with reference to GB / T 3810.3-2016, and the data results are shown in Table 1.

[0054] Table 1 Test results of sample performance

[0055]

[0056] It can be seen from the data in Table 1 that the ceramic plates prepared in Examples 3-5 of the present invention have higher compressive strength and rupture modulus than those in Comparative Examples 1-2, and have lower water absorption. In Comparative Example 1, the aluminum silicate fiber was not modified, and in Comparative Example 2, no modifying additive was added. The compressive strength and rupture modulus of the ceramic plates prepared in Comparative Examples 1-2 were significantly lower than those in Examples 1-2.

[0057] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0058] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A ceramic plate imitating natural materials, It is characterized in that The invention comprises the following components in parts by weight: 40-60 parts of ceramic waste, 8-15 parts of blast furnace slag, 10-20 parts of wollastonite, 5-10 parts of modified aluminum silicate fiber, 4-8 parts of modified additive, 5-15 parts of water glass, 10-15 parts of potassium feldspar, 1-5 parts of expansion agent, and 1-3 parts of foaming agent; The modified aluminum silicate fiber is prepared by grafting carboxylated kaolin with aluminum silicate fiber through γ-aminopropyltriethoxysilane by chemical reaction; the modified additive is prepared by copolymerizing modified nano titanium dioxide, modified graphene oxide, styrene and hydroxyethyl methacrylate under the action of initiator azobisisobutyronitrile; The preparation method of the modified aluminum silicate fiber comprises the following steps: A. Take γ-aminopropyltriethoxysilane and succinic anhydride in N, N-dimethylformamide, stir at 70-85°C for 3-4 hours to obtain a mixed solution, ultrasonically disperse kaolin in N, N-dimethylformamide, then add deionized water and mix, add to the mixed solution, stir at 40-50°C for 2-4 hours, centrifuge, wash and dry after the reaction is completed to prepare carboxylated kaolin; B. Soak the aluminum silicate fiber in a hydrochloric acid solution for 5-6 hours to remove surface impurities, then soak it in a sodium hydroxide solution and place it at 75-85° C. for 10-12 hours to prepare pretreated aluminum silicate fiber; C. Ultrasonic dispersion of carboxylated kaolin in N,N-dimethylformamide, addition of dicyclohexylcarbodiimide, γ-aminopropyltriethoxysilane and pretreated aluminum silicate fiber, stirring at 55-70°C for 4-7h, centrifugation and drying after the reaction is completed, to prepare modified aluminum silicate fiber; In the step C, the mass ratio of carboxylated kaolin, γ-aminopropyltriethoxysilane and pretreated aluminum silicate fiber is 1-2.5:2.4-5:4-6; The preparation method of the modified additive comprises the following steps: (1) Ultrasonic dispersion of nano-titanium dioxide in a mixed solution of ethanol and deionized water, dropwise addition of glacial acetic acid to adjust the pH value of the system to 4-6, heating to 70-85°C, adding γ-methacryloxypropyltrimethoxysilane to react for 8-12 hours, and filtering, washing and drying after the reaction to obtain modified nano-titanium dioxide; (2) ultrasonically dispersing graphene oxide in deionized water to obtain a dispersion, dissolving p-phenylenediamine in deionized water and adding it to the dispersion, ultrasonically mixing and reacting at 40-55°C for 20-24 hours, filtering, washing and drying after the reaction to obtain amino graphene oxide, and then placing amino graphene oxide and glycidyl methacrylate in a reactor, reacting at 90-110°C for 2-3 hours to prepare modified graphene oxide; (3) In a nitrogen atmosphere, anhydrous ethanol, modified nano-titanium dioxide, modified graphene oxide, styrene and hydroxyethyl methacrylate are placed in a reactor, stirred and mixed evenly at room temperature, and then azobisisobutyronitrile is added, and the temperature is raised to 70-80°C for reaction for 6-8 hours. After the reaction is completed, the mixture is cooled to room temperature, and the modified additive is prepared by rotary evaporation, precipitation and drying. In the step (3), the mass ratio of modified nano titanium dioxide, modified graphene oxide, styrene and hydroxyethyl methacrylate is 3.2-3.6:6-8:1-1.2:1.2-1.

4.

2. The ceramic plate imitating natural materials according to claim 1, It is characterized in that The ceramic waste is composed of the following by mass percentage: SiO 2 :66~68%,Al 2 O 3 : 15~17%, MgO: 3.5~5.5%, CaO: 1.5~2%, Na 2 O: 2.5~3.5%, K 2 O: 2~3%, Fe 2 O 3 : 0.8~1.1% and the remainder of impurities.

3. The ceramic plate imitating natural materials according to claim 1, It is characterized in that The mesh size of the ceramic waste and blast furnace slag is 300-500 meshes.

4. The ceramic plate imitating natural materials according to any one of claims 1 to 3, It is characterized in that The method for preparing the ceramic plate imitating natural materials comprises the following steps: S1, adding parts by weight of ceramic waste, blast furnace slag, wollastonite, expansion agent, foaming agent, water glass, and potassium feldspar to a ball mill, and wet-milling for 10 to 18 hours to obtain a premix; S2, taking the premix, the modified aluminum silicate fiber and the modified additive into a mixer and mixing them evenly to obtain a mixture; S3, transporting the mixed material to an aging warehouse for aging treatment for 8-12 hours to obtain aged material, the aging treatment temperature is 35-45°C, and the aging humidity is 30-50%; S4, transferring the aged material to a blank mold, and extruding it at 80-90 MPa to obtain a formed blank; S5. The formed blank is cured, demolded, sintered at 1100-1200°C for 1-3h, cooled to room temperature, and edge-ground to obtain a ceramic plate imitating natural materials.