A hot-melt membrane for building waterproofing roll and its production process

By formulating a polypropylene hot-melt film and using polymeric modified components and water-blocking modified components to improve the density and mechanical properties, the problem of air and water permeability of the polypropylene film during high-temperature baking has been solved, and the effective use of asphalt waterproofing membranes has been achieved. Waterproof and extended lifespan.

CN118702995BActive Publication Date: 2024-10-29CANGZHOU ZHAOYANG PAPER PLASTIC PACKAGING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411188414.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-10-29
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The polypropylene film is prone to hot melt volatilization during high-temperature baking, causing the asphalt waterproofing membrane to be air-permeable and water-permeable during storage, affecting the waterproofing effect.

Method used

The polypropylene hot-melt film production process is used to form a high-density hot-melt film by formulating polypropylene, compatibilizer, polymeric modified ingredients, water-blocking modified ingredients, antioxidants and lubricants to increase the cross-linking density and strengthen the Mechanical properties to achieve air and water blocking effect.

Benefits of technology

Significantly reduces oxygen and moisture transmittance, extends the service life of asphalt waterproof membrane, and provides good waterproofing effect under high temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118702995B_ABST
    Figure CN118702995B_ABST
Patent Text Reader

Abstract

The invention relates to the field of material technology, and discloses a hot-melt film for building waterproof coiled materials and a production process thereof. The hot-melt film is made of polypropylene as a main raw material, supplemented with additives such as a compatibilizer, a polymeric modified component, and a water-blocking modified component, and is prepared through a mixing and extrusion process. The polymeric modified component has a branched structure and contains a large amount of secondary amino groups, which can interact with the compatibilizer during subsequent processing, thereby converting a polypropylene matrix from a linear structure to a branched structure, greatly improving the crosslinking density of the polypropylene hot-melt film, reducing the porosity, and thus reducing the permeability of oxygen, water, etc. The addition of the water-blocking modified component can generate a super-hydrophobic structure on the surface of the hot-melt film, preventing the attachment of water vapor, and avoiding the penetration phenomenon caused by the long-term attachment of water vapor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of materials, and in particular to a hot-melt film for building waterproofing coiled materials and a production process thereof. Background Art

[0002] In the field of modern construction, waterproofing is one of the key links to ensure the integrity of the building structure and extend its service life. In this project, asphalt waterproofing membrane has good water resistance, weather resistance, crack resistance and certain flexibility. It can effectively resist the erosion of rainwater, groundwater and other liquid media, and protect the building structure from damage. At the same time, it has good construction performance and economy, and has become one of the indispensable materials in waterproofing projects. However, asphalt-based waterproofing membranes are easily corroded by moisture, oxygen, etc. during storage, causing organic matter to seep out, resulting in a weakened waterproofing effect. At present, it is generally achieved by attaching a thin film material during the preparation process of the asphalt waterproofing membrane to form a protective film on the surface of the asphalt waterproofing membrane, which can prevent the asphalt waterproofing membrane from direct contact with moisture in the air.

[0003] Asphalt waterproofing membranes need to be baked at high temperatures during construction, research has found that polypropylene films are easy to melt and volatilize during high-temperature baking, leaving less residue, which can make asphalt waterproofing membranes fit the building better. Therefore, using polypropylene films as protective films for asphalt waterproofing membranes is more advantageous in practical applications. However, polypropylene has a linear structure, so the film density is relatively low and there is still air permeability, which actually still has an adverse effect on the long-term storage of asphalt waterproofing membranes. Therefore, it is urgent to increase the density of polypropylene film materials to prevent the penetration of moisture and oxygen.

[0004] Based on this, the present invention provides a polypropylene hot-melt film material, which can be directly used as a protective film for asphalt waterproofing membranes and has a good gas and oxygen barrier effect. Summary of the invention

[0005] In order to solve the problems mentioned in the background technology, the purpose of the present invention is to provide a hot-melt membrane for building waterproofing membrane and a production process thereof.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A production process of a hot-melt film for building waterproofing membrane, wherein the hot-melt film is made of the following raw materials in parts by weight:

[0008] Polypropylene 75-82 parts;

[0009] Compatibilizer 10-16 parts;

[0010] 2-3.5 parts of polymeric modified component;

[0011] 3-5 parts of water-blocking modified component;

[0012] Antioxidant 0.5-1 part;

[0013] 1-2 parts of lubricant;

[0014] The production process comprises the following steps:

[0015] Step 1: Material mixing

[0016] Weigh polypropylene, compatibilizer, polymer-type modified component, water-blocking modified component, antioxidant, and lubricant according to weight proportions, and then put them into a mixer, control the speed to 1000-2000 r / min, and stir and mix at a temperature of 100-120° C. for 30-40 minutes to prepare a mixture;

[0017] Step 2: Extrusion

[0018] The mixed material is fed into the extruder, the processing temperature is controlled at 215-230°C, and the masterbatch is formed through the melt extrusion process. The screw temperature is controlled at 200-240°C and the cold roller temperature is controlled at 20-40°C to form a cast film, and then the hot melt film is obtained through cooling and shaping treatment.

[0019] As a further embodiment of the present invention, the preparation method of the compatibilizer is as follows:

[0020] SBS and toluene are stirred and mixed, and after they are completely dissolved, a homogeneous liquid is formed, and nitrogen is introduced for protection. Then, isocyanoethyl methacrylate and dibenzoyl peroxide are added to the homogeneous liquid, and then the temperature is controlled to 80-90° C., maintained for 6-9 hours, and then the temperature is lowered and discharged to prepare a compatibilizer.

[0021] As a further embodiment of the present invention, the method for preparing the polymeric modified component comprises the following steps:

[0022] Step S1, 1,3-adamantanediol and N,N-dimethylformamide are mixed, stirred to dissolve, and then epichlorohydrin and a phase transfer catalyst are added. After the addition is completed, the temperature is raised to 70-80° C., and the mixture is stirred for 1-3 hours at the same temperature. The temperature is then lowered to 60-65° C., and a sodium hydroxide solution is added. After the addition is completed, the mixture is stirred for 2-4 hours, and the heating is stopped. The mixture is discharged to obtain a bridged body;

[0023] Step S2, adding the bridge body to toluene, mechanically stirring until completely dissolved, and then adding the branching agent. After the addition is complete, nitrogen is introduced to expel the air, and then the temperature is gradually increased to 60-70°C. After continuous stirring for 6-9 hours, the heating is stopped, the nitrogen is removed, and the material is discharged to obtain the polymer modified component.

[0024] As a further embodiment of the present invention, in step S1, the phase transfer catalyst is at least one of tetrabutylammonium bromide, tetrabutylammonium hydrogen sulfate or tetrabutylammonium chloride.

[0025] As a further embodiment of the present invention, in step S1, the molar ratio of 1,3-adamantanediol to epichlorohydrin is 1:2.

[0026] As a further embodiment of the present invention, in step S2, the branching agent is tris(2-aminoethyl)amine.

[0027] In the above technical scheme, 1,3-adamantanediol can react with epichlorohydrin under the action of a phase transfer catalyst and sodium hydroxide, and an adamantane derivative containing two equivalents of epoxy groups, i.e., a bridge body, is obtained by controlling the dosage ratio of 1,3-adamantanediol and epichlorohydrin. Then, the epoxy groups contained in the bridge body structure can undergo continuous ring-opening reactions with a branching agent, thereby forming a polymeric substance with a branched structure, i.e., a polymeric modified component.

[0028] As a further solution of the present invention, the preparation method of the water-blocking modified component is as follows:

[0029] Step S11, mixing the terminal hydroxyl silicone oil with dimethyl sulfoxide, stirring to form a mixed solution, then adding iminodiacetic acid and p-toluenesulfonic acid, gradually heating to 90-100° C., stirring at this temperature for 8-12 hours, evaporating under reduced pressure to remove the solvent, discharging the material, and preparing a silicone oil derivative;

[0030] Step S12, adding the silicone oil derivative to tetrahydrofuran, stirring and mixing, then adding tert-butyl halide, stirring at 60-65° C. for 3-6 hours, then evaporating to remove the solvent, cooling and discharging the material, and thus preparing the water-blocking modified component.

[0031] As a further embodiment of the present invention, in step S11, the number average molecular weight of the terminal hydroxyl silicone oil is 5000.

[0032] As a further embodiment of the present invention, in step S12, the halogenated tert-butane is 1-bromo-3,3-dimethylbutane.

[0033] In the above technical scheme, p-toluenesulfonic acid is first used as a catalyst to cause continuous condensation of the terminal hydroxyl group of the terminal hydroxyl silicone oil with iminodiacetic acid to form a silicone oil derivative having an alternating structure of silicone oil-iminodiacetic ester connected by an ester bond. Then, 1-bromo-3,3-dimethylbutane is used to replace the imino group in the silicone oil derivative to form a silicone oil derivative having a strong hydrophobic structure such as silicone oil and tert-butyl in the structure, that is, a water-blocking modified component.

[0034] As a further embodiment of the present invention, the antioxidant is at least one of antioxidant 1010, antioxidant 168 or antioxidant 1076; the lubricant is at least one of stearic acid, zinc stearate or calcium stearate.

[0035] A hot-melt membrane for building waterproofing coiled material is produced by adopting the above production process.

[0036] Beneficial effects of the present invention:

[0037] (1) The polymeric modified component prepared by the present invention has a branched structure and contains a large number of secondary amino groups. It can interact with the compatibilizer during the subsequent processing, thereby converting the polypropylene matrix from a linear structure to a branched structure, which can greatly increase the crosslinking density of the polypropylene hot melt film, reduce the porosity, and thus reduce the permeability of oxygen, water, etc. In addition, since the polymeric modified component also contains a large number of rigid heterocyclic rings of adamantane, these rigid heterocyclic structures are incorporated into the crosslinked network of polypropylene, and thus can effectively enhance the mechanical properties of the polypropylene hot melt film.

[0038] (2) The present invention prepares a water-blocking modified component as an additive and mixes it with a polypropylene matrix. The water-blocking modified component uses a large amount of silicone oil and tert-butyl and other strong hydrophobic structures contained in the component to produce a super-hydrophobic structure on the surface of the polypropylene hot-melt film, thereby preventing the attachment of water vapor and avoiding the penetration phenomenon caused by long-term attachment of water vapor. Therefore, the water-blocking modified component can cooperate with the polymer-type modified component to achieve excellent air and water barrier effects, thereby effectively extending the life of the asphalt waterproof membrane.

[0039] (3) The polypropylene hot-melt film prepared in the present invention can melt and volatilize under high temperature conditions during the construction of the asphalt waterproofing membrane, so that the asphalt can be tightly attached to the wall after melting, so that the asphalt waterproofing membrane can achieve a good waterproofing effect.

[0040] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0042] Figure 1 This is the infrared test image of the polymer modified component;

[0043] Figure 2 This is the infrared analysis test diagram of the water-blocking modified component. DETAILED DESCRIPTION

[0044] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1

[0045] A hot-melt membrane for building waterproofing membrane is made of the following raw materials in parts by weight:

[0046] Polypropylene 75 parts;

[0047] 10 parts of compatibilizer;

[0048] 2 parts of polymeric modified component;

[0049] 3 parts of water-blocking modified component;

[0050] Antioxidant 1010 0.5 parts;

[0051] Lubricant: 1 part of stearic acid;

[0052] The production process of the hot melt film comprises the following steps:

[0053] Step 1: Material mixing

[0054] Polypropylene, compatibilizer, polymer-type modified component, water-blocking modified component, antioxidant 1010, and lubricant stearic acid were weighed according to weight proportions, and then put into a mixer, the speed was controlled to be 1500 r / min, and the mixture was stirred and mixed at a temperature of 100° C. for 30 minutes to prepare a mixture;

[0055] Step 2: Extrusion

[0056] The mixed material is fed into the extruder, the processing temperature is controlled at 220°C, and the masterbatch is formed through the melt extrusion process. The screw temperature is controlled at 210°C and the cold roller temperature is controlled at 30°C for cast film formation. After cooling and shaping treatment, the hot melt film can be obtained. Example 2

[0057] A hot-melt membrane for building waterproofing membrane is made of the following raw materials in parts by weight:

[0058] Polypropylene 80 parts;

[0059] 15 parts of compatibilizer;

[0060] 3 parts of polymeric modified component;

[0061] 4 parts of water-blocking modified component;

[0062] Antioxidant 168 0.8 parts;

[0063] Lubricant calcium stearate 1.5 parts;

[0064] The production process of the hot melt film comprises the following steps:

[0065] Step 1: Material mixing

[0066] Polypropylene, compatibilizer, polymer-type modified component, water-blocking modified component, antioxidant 168, and lubricant calcium stearate were weighed according to weight parts, and then put into a mixer, the speed was controlled to 1500r / min, and the mixture was stirred and mixed at a temperature of 110°C for 40 minutes to prepare a mixture;

[0067] Step 2: Extrusion

[0068] The mixed material is fed into the extruder, the processing temperature is controlled at 220°C, and the masterbatch is formed through the melt extrusion process. The screw temperature is controlled at 220°C and the cold roller temperature is controlled at 30°C for film casting. After cooling and shaping, the hot melt film can be obtained. Example 3

[0069] A hot-melt membrane for building waterproofing membrane is made of the following raw materials in parts by weight:

[0070] Polypropylene 82 parts;

[0071] 16 parts of compatibilizer;

[0072] 3.5 parts of polymeric modified component;

[0073] 5 parts of water-blocking modified component;

[0074] Antioxidant 1076 1 part;

[0075] Lubricant: 2 parts zinc stearate;

[0076] The production process of the hot melt film comprises the following steps:

[0077] Step 1: Material mixing

[0078] Polypropylene, compatibilizer, polymer-type modified component, water-blocking modified component, antioxidant 1076, and lubricant zinc stearate were weighed according to weight proportions, and then put into a mixer, the speed was controlled to be 2000 r / min, and the mixture was stirred and mixed at a temperature of 120° C. for 40 minutes to prepare a mixture;

[0079] Step 2: Extrusion

[0080] The mixed material is fed into the extruder, the processing temperature is controlled at 230°C, and the masterbatch is formed through the melt extrusion process. The screw temperature is controlled at 240°C and the cold roller temperature is controlled at 20°C for film casting. After cooling and shaping, the hot melt film can be obtained.

[0081] Comparative Example 1

[0082] A hot-melt membrane for building waterproofing membrane is made of the following raw materials in parts by weight:

[0083] Polypropylene 80 parts;

[0084] 15 parts of compatibilizer;

[0085] 3 parts of polymeric modified component;

[0086] Antioxidant 168 0.8 parts;

[0087] Lubricant calcium stearate 1.5 parts;

[0088] The production process of the hot melt film comprises the following steps:

[0089] Step 1: Material mixing

[0090] Polypropylene, compatibilizer, polymer-modified component, antioxidant 168, and lubricant calcium stearate were weighed according to weight proportions, and then put into a mixer, the speed was controlled to be 1500 r / min, and the mixture was stirred and mixed at a temperature of 110° C. for 40 minutes to prepare a mixture;

[0091] Step 2: Extrusion

[0092] The mixed material is fed into the extruder, the processing temperature is controlled at 220°C, and the masterbatch is formed through the melt extrusion process. The screw temperature is controlled at 220°C and the cold roller temperature is controlled at 30°C for film casting. After cooling and shaping, the hot melt film can be obtained.

[0093] Comparative Example 2

[0094] A hot-melt membrane for building waterproofing membrane is made of the following raw materials in parts by weight:

[0095] Polypropylene 80 parts;

[0096] 15 parts of compatibilizer;

[0097] 4 parts of water-blocking modified component;

[0098] Antioxidant 168 0.8 parts;

[0099] Lubricant calcium stearate 1.5 parts;

[0100] The production process of the hot melt film comprises the following steps:

[0101] Step 1: Material mixing

[0102] Polypropylene, compatibilizer, water-blocking modification component, antioxidant 168, and lubricant calcium stearate were weighed according to weight proportions, and then put into a mixer, the speed was controlled to be 1500 r / min, and the mixture was stirred and mixed at a temperature of 110° C. for 40 minutes to prepare a mixture;

[0103] Step 2: Extrusion

[0104] The mixed material is fed into the extruder, the processing temperature is controlled at 220°C, and the masterbatch is formed through the melt extrusion process. The screw temperature is controlled at 220°C and the cold roller temperature is controlled at 30°C for film casting. After cooling and shaping, the hot melt film can be obtained.

[0105] The compatibilizers in the above examples and comparative examples were prepared by the following method:

[0106] 15 g of SBS and toluene were stirred and mixed, and after they were completely dissolved, a homogeneous liquid was formed. Nitrogen was introduced for protection, and then 1.5 g of isocyanoethyl methacrylate and 0.1 g of dibenzoyl peroxide were added to the homogeneous liquid. The temperature was then controlled to 90° C. and maintained for 8 hours. The material was then cooled and discharged to prepare a compatibilizer.

[0107] The polymeric modified components in the above examples and comparative examples were prepared by the following method:

[0108] Step S1, 0.6 g of 1,3-adamantanediol and N,N-dimethylformamide were mixed, stirred to dissolve, and then 0.66 g of epichlorohydrin and 0.1 g of tetrabutylammonium bromide were added. After the addition was completed, the temperature was raised to 75° C., and the mixture was stirred for 2 h. Then, the temperature was lowered to 65° C., 2 mL of 15% sodium hydroxide solution was added, and after the addition was completed, the mixture was stirred for 3 h. The heating was stopped, and the material was discharged to obtain a bridged body.

[0109] Step S2, add 0.5g of the bridge body to toluene, stir mechanically until it is completely dissolved, then add 0.15g of tri(2-aminoethyl)amine, pass nitrogen after the addition to exhaust the air, then gradually increase the temperature to 65°C, continue stirring for 8h, stop heating, remove nitrogen, and discharge the material to obtain a polymer modified component.

[0110] Figure 1 This is the infrared test image of the polymer modified component, where 3486cm -1 The absorption peak at 3289 cm is the characteristic absorption peak of NH of secondary amino group. -1 The absorption peak at 1320 cm is the characteristic absorption peak of hydroxyl group. -1 The absorption peak at 1079cm is the characteristic absorption peak of CN.-1 The absorption peak that appears at is the CO characteristic absorption peak of the ether bond.

[0111] The water-blocking modified components in the above examples and comparative examples were prepared by the following method:

[0112] Step S11, 3.5 g of terminal hydroxyl silicone oil with a number average molecular weight of 5000 is mixed with dimethyl sulfoxide, and stirred to form a mixed solution, and then 0.1 g of iminodiacetic acid and 0.05 g of p-toluenesulfonic acid are added. After the addition, the temperature is gradually raised to 100° C., and stirring is maintained at this temperature for 9 hours. The solvent is evaporated under reduced pressure, and the material is discharged to prepare a silicone oil derivative;

[0113] Step S12, add 2.6g of silicone oil derivative to tetrahydrofuran, stir and mix, then add 0.2g of 1-bromo-3,3-dimethylbutane, stir at 65°C for 4h, then evaporate to remove the solvent, cool and discharge, and the water-blocking modified component can be prepared.

[0114] Figure 2 This is the infrared analysis test chart of the water-blocking modified component, where 2800-3000cm -1 The absorption peak at 1751 cm is the characteristic absorption peak of CH of methyl and methylene. -1 The absorption peak at 1062 cm is the characteristic absorption peak of C=O of ester group. -1 The absorption peak that appears at is the Si-O characteristic absorption peak.

[0115] Test Case

[0116] The hot melt films in Examples 1 to 3 and Comparative Examples 1 to 2 were made into test samples of corresponding specifications, and the thickness was controlled to be 30 μm;

[0117] According to the standard GB / T 1037-2021, the water vapor transmission rate test is carried out; according to the standard GB / T 1038-2000, the oxygen transmission rate test is carried out;

[0118] Water contact angle test was performed using TC-A3 automatic contact angle meter;

[0119] According to the standard GB / T 1040.3-2006, tensile properties test was carried out;

[0120] The test results are recorded in Table 1:

[0121] Table 1 - Performance test results

[0122]

[0123] According to the test data, the hot melt film produced by adding polymeric modified ingredients and water-blocking modified ingredients has obviously better air and water barrier effects, and the surface water contact angle is greater than 150°, which shows super hydrophobicity. Therefore, it can prevent the slow penetration caused by water vapor adhesion, and the mechanical properties are also excellent. On the contrary, the hot melt film obtained by removing the water-blocking modified ingredients has a significant decrease in water barrier effect, and the hot melt film obtained by removing the polymeric modified ingredients has a greatly reduced air and water barrier effect, and the mechanical properties also have a significant decrease.

[0124] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the scope defined by the concept of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A production process for hot melt membrane for building waterproofing membrane, characterized in that: The hot melt film is made of the following raw materials in parts by weight: Polypropylene 75-82 parts; Compatibilizer 10-16 parts; 2-3.5 parts of polymeric modified component; 3-5 parts of water-blocking modified component; Antioxidant 0.5-1 part; 1-2 parts of lubricant; The production process comprises the following steps: Step 1: Material mixing Weigh polypropylene, compatibilizer, polymer-type modified component, water-blocking modified component, antioxidant, and lubricant according to weight proportions, and then put them into a mixer, control the speed to 1000-2000 r / min, and stir and mix at a temperature of 100-120° C. for 30-40 minutes to prepare a mixture; Step 2: Extrusion The mixed material is fed into the extruder, the processing temperature is controlled at 215-230°C, a master batch is formed through a melt extrusion process, the screw temperature is controlled at 200-240°C, the cold roller temperature is controlled at 20-40°C, a film is cast, and then a hot melt film is obtained through cooling and shaping. The preparation method of the compatibilizer is as follows: SBS and toluene are stirred and mixed, and after they are completely dissolved, a homogeneous liquid material is formed, and nitrogen is introduced for protection. Then, isocyanoethyl methacrylate and dibenzoyl peroxide are added to the homogeneous liquid material, and then the temperature is controlled to 80-90° C., maintained for 6-9 hours, and then the temperature is lowered and discharged to prepare a compatibilizer; The preparation method of the polymeric modified component comprises the following steps: Step S1, 1,3-adamantanediol and N,N-dimethylformamide are mixed, stirred to dissolve, and then epichlorohydrin and a phase transfer catalyst are added. After the addition is completed, the temperature is raised to 70-80° C., and the mixture is stirred for 1-3 hours at the same temperature. The temperature is then lowered to 60-65° C., and a sodium hydroxide solution is added. After the addition is completed, the mixture is stirred for 2-4 hours, and the heating is stopped. The mixture is discharged to obtain a bridged body; Step S2, adding the bridge body to toluene, mechanically stirring until completely dissolved, then adding the branching agent, introducing nitrogen after the addition to expel the air, then gradually raising the temperature to 60-70°C, stirring continuously for 6-9 hours, stopping heating, removing nitrogen, discharging, and obtaining a polymer modified component; The phase transfer catalyst is at least one of tetrabutylammonium bromide, tetrabutylammonium hydrogen sulfate or tetrabutylammonium chloride; The branching agent is tris(2-aminoethyl)amine; The preparation method of the water-blocking modified component is as follows: Step S11, mixing the terminal hydroxyl silicone oil with dimethyl sulfoxide, stirring to form a mixed solution, then adding iminodiacetic acid and p-toluenesulfonic acid, gradually heating to 90-100° C., stirring at this temperature for 8-12 hours, evaporating under reduced pressure to remove the solvent, discharging the material, and preparing a silicone oil derivative; Step S12, adding the silicone oil derivative to tetrahydrofuran, stirring and mixing, then adding tert-butyl halide, stirring at 60-65° C. for 3-6 hours, then evaporating to remove the solvent, cooling and discharging the material, and thus preparing the water-blocking modified component.

2. A production process for hot melt membrane for building waterproofing membrane according to claim 1, characterized in that: In step S1, the molar ratio of 1,3-adamantanediol to epichlorohydrin is 1:

2.

3. The production process of a hot melt membrane for building waterproofing membrane according to claim 1, characterized in that: In step S11, the number average molecular weight of the hydroxy-terminated silicone oil is 5,000.

4. The production process of a hot melt membrane for building waterproofing membrane according to claim 1, characterized in that: In step S12, the tert-butyl halide is 1-bromo-3,3-dimethylbutane.

5. A hot melt membrane for building waterproofing membrane, characterized in that: The method is prepared by the production process as claimed in claim 1.

Citation Information

Patent Citations

  • Self-emulsifying cleaning material as well as preparation method and application thereof

    CN115710538A

  • Adamantane derivative, method for producing the same and resin composition containing adamantane derivative

    JP2011219451A