Ceramic core soft core support self-adaptive preparation method based on additive and subtractive composite processing

Through the composite processing technology of additive and subtractive materials, combined with point laser inspection and CNC milling, the adaptive preparation of the soft core support of the hollow turbine blade ceramic core is realized, which solves the impact of the ceramic core profile error and clamping error on the wax wall thickness accuracy. Improved preparation efficiency and accuracy.

CN118720060AActive Publication Date: 2024-10-01NORTHWESTERN POLYTECHNICAL UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410969158.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-01
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The existing technology has problems with poor molding accuracy and dimensional control in the preparation of ceramic core soft core supports for hollow turbine blades. In particular, the fitting error has a greater impact under the variation of blade wall thickness and the complexity of the ceramic core profile, resulting in The accuracy of the wax wall thickness is difficult to guarantee.

Method used

An adaptive preparation method for soft core braces based on additive and subtractive materials is adopted. Through point laser detection, conformal printing and CNC milling processing, combined with a four-axis linkage system, automatic measurement and processing are achieved to achieve adaptive sticking of soft core braces. Well prepared with precision.

Benefits of technology

It achieves high-precision preparation of soft core supports for ceramic cores, ensures precise control of wax wall thickness, reduces the impact of clamping errors, improves preparation efficiency and molding accuracy, and controls the error range within 0.01mm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720060A_ABST
    Figure CN118720060A_ABST
Patent Text Reader

Abstract

The invention discloses a ceramic core soft core support self-adaptive preparation method based on additive and subtractive composite machining, and belongs to the technical field of precision casting of hollow turbine blades of aero-engines. The method comprises the steps of individual-state ceramic core profile detection and error analysis, individual-state ceramic core profile surface soft chaplet size self-adaptive calculation and fitting position calibration. A conformal printing process of the individual-state ceramic core molded surface soft core support; and a soft core support NC milling process, and soft core support forming precision and surface quality detection and evaluation. According to the method, aiming at the influence of manufacturing errors of the individual ceramic core molded surface on the wall thickness of the blade wax pattern, the thickness of the blade wax pattern is compensated by using the soft core supports with different sizes, so that the technical problems of poor forming precision and size control, fitting position deviation and the like in the preparation of the ceramic core molded surface soft core support by the existing method are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of precision casting of hollow turbine blades of aircraft engines, and specifically relates to an adaptive preparation method of a ceramic core soft core support based on composite processing of increasing and reducing materials. Background Art

[0002] Hollow turbine blades are one of the key core components of aircraft engines, and their wall thickness accuracy is a key technical indicator that determines the safety and stability of the blades in service. Due to the limitations of materials and structures, hollow turbine blades are mainly manufactured by non-residue investment casting. The specific process is generally as follows: first, the ceramic core reflecting the internal structure of the blade is placed in the wax mold, its position in the internal space of the mold cavity is adjusted, and the precision casting wax mold with the ceramic core is pressed; then, after shell making, dewaxing, sintering, casting, core removal and heat treatment, the precision casting blank of the turbine blade without residual is finally obtained. Under the premise of stable control of materials and processes, the wall thickness accuracy of the blade is mainly inherited from the wall thickness accuracy of the wax mold, and is guaranteed by the matching relationship between the ceramic core and the mold cavity surface. At present, the positioning of the ceramic core in the internal space of the mold cavity is mainly adjusted by attaching a soft core support. In view of the characteristics of variable wall thickness of the blade, the accuracy of the soft core support fitting position and the dimensional accuracy are particularly important for the adjustment of the spatial position of the ceramic core. Therefore, how to ensure the spatial position of the ceramic core inside the mold by accurately fitting soft core supports of different sizes and thicknesses, thereby controlling the wall thickness accuracy of the blade wax mold, is a key bottleneck problem that needs to be solved urgently.

[0003] At present, in the actual process of preparing the precision casting wax pattern of turbine blades, a hard core support made of resin material of equal thickness is manually attached to the surface of the ceramic core. However, considering the characteristics of variable wall thickness of the blade, the wall thickness difference between the leading and trailing edges of the ceramic core and the back of the blade basin is large. At the same time, combined with the manufacturing error of the ceramic core surface, the size of the soft core support also needs to be accurately adjusted; in addition, the current hard core support of equal thickness resin will cause the ceramic core surface to break during the wax pressing process due to the influence of dimensional accuracy and material, thus affecting the wall thickness deviation of the precision casting wax pattern and its preparation efficiency.

[0004] The prior art discloses a method for preparing a soft core support for a ceramic core of a turbine blade, and uses the FDM principle to realize the preparation of a soft core support for a ceramic core profile according to the physical properties of the wax material itself; there is also a disclosed method for processing a soft core support for a ceramic core of a turbine blade, and uses a three-coordinate method to perform CNC milling on the soft core support for the wax soft core support that is bonded to the ceramic core profile, thereby improving the consistency of the bonding points between the soft core support and the ceramic core. These two methods respectively achieve the consistency of the bonding points of the soft core support and the guarantee of dimensional accuracy. However, since the profile of the ceramic core itself is a complex free-form surface, the individual ceramic core profile error will also affect the wall thickness accuracy of the wax model, and it is necessary to compensate by changing the size of the soft core support, that is, the size of the individual ceramic core soft core support is different. In addition, since the wall thickness accuracy of the blade precision casting wax model is relatively high, the preparation of the soft core support by printing and milling in steps will affect the molding dimensional accuracy due to the clamping error. Therefore, in order to combine the individual ceramic core profile error and eliminate the influence of the clamping error on the dimensional accuracy of the soft core support, it is urgent to explore a new method for adaptive preparation of ceramic core soft core supports based on additive and subtractive composite processing. Summary of the invention

[0005] Technical issues to be solved:

[0006] In order to avoid the shortcomings of the prior art, the present invention provides an adaptive preparation method for a ceramic core soft core support based on composite processing of additive and subtractive materials. The method uses the theoretical ceramic core profile as the standard to obtain the manufacturing error of the individual ceramic core profile, and then determines the actual position of the soft core support, and determines the structure of the actual individual ceramic core profile soft core support in an adaptive manner; an integrated manufacturing system is used during preparation, and only one calibration is required to meet the automation requirements of complete measurement, printing, and processing. The present invention aims at the influence of the manufacturing error of the individual ceramic core profile on the wall thickness of the blade wax model, and uses soft core supports of different sizes to compensate for its thickness, thereby overcoming the technical problems of the existing methods in the preparation of ceramic core profile soft core supports in terms of poor molding accuracy and dimensional control.

[0007] The technical solution of the present invention is: an adaptive preparation method of a ceramic core soft core support based on additive and subtractive composite processing, and the specific steps are as follows:

[0008] Measure the actual ceramic core profile parameters and calibrate the soft core support position;

[0009] Determine the geometric shape of the soft core support in combination with the surface of the wax mold cavity;

[0010] A solid blank of a soft core support is prepared by conformal printing, wherein the free-form surface position of the soft core support that is attached to the ceramic core mold surface is obtained by decomposing a B-spline curve to obtain a printing path, a planar rectangular area located in the middle of the soft core support is printed by plane layering, and a free-form surface position attached to the cavity surface is obtained by decomposing a B-spline curve to obtain a printing path;

[0011] Measure the size of the soft core support solid blank to determine the machining allowance for material reduction;

[0012] Soft core support CNC milling processing;

[0013] Soft core support forming accuracy detection and evaluation.

[0014] A further technical solution of the present invention is: the method for calibrating the position of the soft core support is:

[0015] Based on the measured actual ceramic core profile parameters, a simulation model of the individual ceramic core profile is constructed;

[0016] Comparing the simulation model of the individual ceramic core profile with the theoretical ceramic core profile model to obtain the actual individual ceramic core profile manufacturing error;

[0017] Based on the obtained error value, the soft core support fitting point is re-determined on the simulation model of the actual ceramic core profile, thus completing the calibration of the soft core support position.

[0018] A further technical solution of the present invention is: the method for determining the geometric shape of the soft core support is:

[0019] Constructing a rectangular area at the determined soft core support position as the bottom surface of the soft core support, and discretizing the four sides of the rectangular area into point cloud data;

[0020] Calculate the normal direction of each point along its ceramic core surface and project it onto the cavity surface of the wax mold;

[0021] The projection points on the cavity surface are fitted into a spline curve, and the enveloping cavity surface is the upper surface of the soft core support;

[0022] The geometric shape of the soft core support is obtained by stretching the bottom surface of the soft core support to the upper surface of the soft core support.

[0023] A further technical solution of the present invention is: the additive method for preparing the soft core support solid blank is to use an FDM direct writing pneumatic extrusion nozzle with a nozzle diameter of 0.5 mm and printing process parameters: extrusion pressure of 0.015 MPa, heating temperature of 75°C, and moving trajectory speed of 15 mm / s.

[0024] A further technical solution of the present invention is: the method for determining the subtractive machining allowance of the soft core support solid blank is to perform size detection on the soft core support solid blank through point laser, and obtain the size deviation by comparing it with the theoretical soft core support size; when the actual size is larger than the theoretical size, determine the size of the CNC milling machining allowance; when the actual size is smaller than the theoretical size, perform size compensation on the soft core support solid blank.

[0025] A further technical solution of the present invention is: the CNC milling processing method of the soft core support is to determine the curved surface processing trajectory of the upper surface of the soft core support through a multi-axis linkage processing system, and then determine the processing trajectory of the side wall plane of the soft core support, connect the local processing trajectories, and obtain the CNC milling processing path of the soft core support; according to the determined processing path, drive the tool movement of the multi-axis linkage processing system, combined with three-dimensional measurement, to obtain the solid soft core support after fine processing.

[0026] A further technical solution of the present invention is: the multi-axis linkage machining system is a four-axis linkage CNC machining equipment, and the machining process parameters are: the electric spindle speed is 12000r / min; the feed speed is 3000mm / min; and the cooling method is air cooling.

[0027] A further technical solution of the present invention is: the soft core support forming accuracy detection and evaluation method is to use a point laser measuring instrument to detect the processed soft core support, so as to determine that its size meets the theoretical requirements and the error range is guaranteed to be within 0.01mm; then use a tool scanner to detect the actual wax pattern surface roughness, and at the same time detect the surface roughness of the soft core support, and compare the two to analyze the actual soft core support processing quality.

[0028] A device for preparing a ceramic core soft core support comprises a support column and a position calibration module, a measuring module, an additive manufacturing module and a milling processing module integrated thereon, wherein the support column is arranged on a workbench, and the ceramic core to be processed is installed on the workbench through a fixture and a rotating spindle turntable; the measuring module, the additive manufacturing module and the milling processing module respectively provide three workstations of measurement, additive manufacturing and milling processing, and realize the motion switching control of the three workstations through the control of a host computer; the surface of the ceramic core is measured by the measuring module, and the collected ceramic core surface point coordinate information is sent to the host computer, and the rotating spindle is controlled to perform adaptive adjustment on the position of the ceramic core according to the collected information; the soft core support blank is additively prepared by setting a position on the ceramic core surface by the additive manufacturing module; the soft core support blank prepared by additive processing is finely processed by the milling processing module; the three workstations of measurement, additive manufacturing and milling processing are positionally aligned by the position calibration module.

[0029] A further technical solution of the present invention is: the position calibration module includes a visual detection camera, which is used to calibrate the relative position relationship between the three workstations of measurement, additive manufacturing, and milling processing; the single pixel accuracy of the visual camera is 0.0038mm / pix, the detection field of view is: 19.4mm*19.4mm, and the working distance is 110mm;

[0030] The calibration method of the position calibration module is:

[0031] Lower the print head of the additive manufacturing module to the working position, and perform a "cross" wax print on the reference plane, which is marked as position A;

[0032] Reset the print head and lower the NC milling spindle of the milling processing module to the working position, and perform "cross" milling in the reference plane as position B;

[0033] Use the visual inspection camera to take pictures of the platform reference surface, calculate the XY direction deviation at the AB position, and perform coordinate calibration;

[0034] Move each workstation to the position of the tool setting probe and calibrate the Z-direction coordinates by touching the tool setting probe.

[0035] Beneficial Effects

[0036] The beneficial effect of the present invention is that the present invention provides an adaptive preparation method of a ceramic core soft core support based on additive and subtractive composite processing. The additive and subtractive manufacturing of the ceramic core soft core support is completed by mainly including three module manufacturing equipments of point laser detection, conformal printing of the ceramic core profile soft core support, and NC milling processing.

[0037] The method of the present invention first uses a point laser module to perform adaptive sampling on the actual individual ceramic core surface, and then obtains the individual ceramic core surface manufacturing error according to the reconstruction result of the individual ceramic core surface, so as to obtain the actual soft core support size, thereby avoiding the error caused by the use of a uniform thickness in the prior art; then, the ceramic core surface soft core support conformal printing module is used to realize the surface layering and path planning of the individual ceramic core surface soft core support, and the process parameters are optimized in combination with the material bonding performance and density of the conformal printing process, so as to obtain the ceramic core surface soft core support conformal manufacturing process parameters (nozzle size: 0.5mm; extrusion pressure: 0.015mpa; heating temperature is 75°C, and moving trajectory speed is 15mm / s). Through the parameter setting, the additive soft core support and the ceramic core surface can be completely fitted, thereby avoiding The position misalignment caused by poor fitting effect and the failure of position calibration were eliminated; then, the NC milling processing module was used to trim the size, shape and surface quality of the soft core support, and the milling processing parameters were optimized in combination with the physical properties of the soft core support material (processing method: four-axis linkage; spindle speed: 12000r / min; feed speed: 3000mm / min; cooling method: air cooling). The parameter design is combined with the additive wax, which can maintain the soft core support morphology during subtractive processing; finally, the point laser module is used to detect the forming size of the soft core support, and the adaptive preparation of the ceramic core surface soft core support is completed (the forming size accuracy error is controlled within 0.01mm, and the preparation time of a single ceramic core soft core support is controlled within 10min) to ensure the accuracy requirements of the prepared soft core support.

[0038] The present invention integrates three modules: a point laser detection module, an additive printing module, and an NC milling processing module, and implements the method using a four-axis additive and subtractive composite manufacturing equipment platform. The equipment platform structure includes a support column and a position calibration module, a measurement module, an additive manufacturing module, and a milling processing module integrated thereon. The support column is arranged on a workbench, and the ceramic core to be processed is installed on the workbench through a fixture and a rotating spindle turntable; the measurement module, the additive manufacturing module, and the milling processing module respectively provide three stations: measurement, additive manufacturing, and milling processing, and the motion switching control of the three stations is realized through the control of the host computer. Through the integrated design, the technical problems of the existing ceramic core profile soft core support preparation method in terms of poor molding accuracy and dimensional control are solved. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is a flow chart of the ceramic core profile soft core support adaptive increase and decrease material composite processing method of the present invention

[0040] Figure 2 It is a four-axis numerical control platform for composite processing of ceramic core profile soft core support adaptively increasing and reducing materials;

[0041] Figure 3 It is a schematic diagram of a method for calculating the forming dimensions of a soft core support on a ceramic core profile;

[0042] Figure 4 It is a schematic diagram of the layering of the soft core support curved surface of the ceramic core profile of the present invention;

[0043] Figure 5 It is a schematic diagram of the soft core support fitting position of the ceramic core profile of the present invention;

[0044] Explanation of the reference numerals: 1. A gantry support column made of marble; 2. A pneumatic print head assembly; 3. A CNC electric spindle; 4. A point laser rangefinder; 5. A visual inspection camera; 6. A rotating spindle (B-axis) turntable with a servo motor; 7. A ceramic core adaptive special tooling fixture. DETAILED DESCRIPTION

[0045] The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0046] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0047] In order to realize the adaptive additive and subtractive composite preparation of ceramic core surface soft core support, a ceramic core surface soft core support additive and subtractive composite preparation equipment platform is built in this example. Combined with the preparation method, the equipment platform mainly includes: a support column and a position calibration module integrated thereon, a measurement module, an additive manufacturing module, and a milling processing module. The support column is set on the workbench, and the ceramic core to be processed is installed on the workbench through a fixture and a rotating spindle turntable; the measurement module, the additive manufacturing module, and the milling processing module provide three stations of point laser detection, additive manufacturing, and milling processing respectively, and the motion switching control of the three stations is realized through the host computer control. The specific structure is as follows:

[0048] The device for preparing a ceramic core soft core support adopted in this embodiment includes a support column and a position calibration module, a measuring module, an additive manufacturing module, and a milling processing module integrated thereon. The support column is arranged on a workbench, and the ceramic core to be processed is installed on the workbench through a fixture and a rotating spindle turntable; the measuring module, the additive manufacturing module, and the milling processing module respectively provide three workstations of measurement, additive manufacturing, and milling processing, and the motion switching control of the three workstations is realized through the control of the host computer; the surface of the ceramic core is measured by the measuring module, and the collected coordinate information of the surface points of the ceramic core is sent to the host computer, and the rotating spindle is controlled to adaptively adjust the position of the ceramic core according to the collected information; the soft core support blank is additively prepared by setting a position on the surface of the ceramic core by the additive manufacturing module; the soft core support blank prepared by additive material is fine-processed by the milling processing module; the three workstations of measurement, additive manufacturing, and milling processing are positioned by the position calibration module.

[0049] Reference Figure 2 As shown, the support column 1 is a gantry structure, the spindle box is slidably connected to the crossbeam of the gantry through a horizontal slide rail, the position calibration module, the measurement module, the additive manufacturing module, and the milling processing module are all installed on the spindle box, the direction of movement of the spindle box along the horizontal slide rail is defined as the Y-axis, the direction of vertical movement is defined as the Z-axis, the central axis rotating around the Z-axis is defined as the C-axis, and the direction of horizontal movement of the workbench perpendicular to the Y-axis is defined as the X-axis, forming a four-axis CNC system of the composite processing platform; the four-axis CNC system is used to realize adaptive adjustment of the position and posture of the ceramic core.

[0050] Preferably, the position calibration module is a visual inspection camera 5, which is used to calibrate the relative position relationship between multiple stations. The single pixel accuracy of the visual camera is 0.0038mm / pix, the detection field of view is: 19.4mm*19.4mm, and the working distance is 110mm.

[0051] Preferably, the measuring module is a point laser detector 4, which is used to detect the position information of the sampling points on the ceramic core surface, and the measurement accuracy is ≤0.005mm. At the same time, the API library function is used for secondary development in the point laser detection process, and the actual soft core support increase and decrease material composite preparation process is combined for secondary development to ensure the position detection of the sampling points on the ceramic core surface and accurate data reading. At the same time, the actual soft core support bonding point position is calibrated on the surface of the ceramic core in an individual state.

[0052] Preferably, the additive manufacturing module is a pneumatic printing nozzle assembly 2, which mainly includes a PVC material barrel, an electronic regulating valve, a PEEK material insulation sleeve, a thermocouple, nozzles of different sizes and a high-precision "L"-shaped bracket connected to the platform module.

[0053] The electronic regulating valve can realize dynamic air pressure adjustment and temperature feedback through PLC development. The printing material for the soft core support is the wax material used for investment casting wax. It has small thermal diffusivity and shrinkage, and belongs to medium-temperature wax. It is granular at room temperature to achieve more sufficient heating and extrusion stability control. Preheating is required before use to ensure that the wax material is fully melted and reduce the internal bubbles in the molten state of the material to ensure the compactness of the soft core support.

[0054] Preferably, the milling processing module includes a CNC machining electric spindle 3, whose output torque is 0.6N·m, the maximum speed is 40000rpm, and the circular runout is ≤2um. A manual tool change method is adopted. Considering the wax material processing and cutting process, a two-tooth ball head high-speed steel milling cutter with different sizes is equipped.

[0055] Preferably, the rotating spindle (B-axis) turntable 6 with a servo motor, combined with the positioning method of the cone hole of the core head of the ceramic core profile and its own structural characteristics, can achieve high-precision preparation of the soft core support at the leading edge, trailing edge, blade basin and blade back of the ceramic core by rotating at different angles.

[0056] Preferably, the ceramic core adaptive special fixture 7 is designed with an adjustable knob fixture in combination with the structural characteristics of the individual ceramic core to ensure the adaptive and precise clamping of the individual ceramic core. Considering that the structure at the trailing edge is relatively weak, an adjustable side top rod is designed to provide auxiliary support to prevent vibration fracture during the process of adding or reducing materials.

[0057] Reference Figure 1 As shown, the specific steps of the ceramic core profile soft core support adaptive additive and subtractive composite processing method of the present invention are as follows:

[0058] Step 1: Detection of individual ceramic core profile errors and calculation of soft core support geometry;

[0059] In this example, the actual length of the ceramic core is 93 mm. The point laser measuring instrument is used to sample the sampling points on the actual ceramic core profile according to the planned measurement trajectory, and the actual ceramic core profile is reconstructed in three dimensions. Then, the rigid registration algorithm is used to calculate the deviation between the actual reconstructed ceramic core and the theoretical profile. Then, based on the empirical layout position of the ceramic core soft core support, the soft core support fitting point is calibrated on the individual reconstructed ceramic core profile, and then the soft core support size suitable for the individual ceramic core profile is recalculated.

[0060] Specifically, refer to Figure 5 As shown in the figure, the soft core support fitting points are distributed at the positions of the ceramic core sections II, V and VIII. According to the theoretical soft core support fitting points, the soft core support size for the actual ceramic core profile is calculated. Taking one of the soft core supports as an example, the actual size calculated is 2.89mm, and the theoretical size of the current point is 3.02mm; compared with the theoretical position, due to the manufacturing error of the ceramic core profile, the soft core support attachment thickness is thinner at this position. Finally, the actual position of the soft core support is calibrated and the position coordinates of the point are recorded.

[0061] Step 2, determine the geometric dimensions of the ceramic core profile soft core support;

[0062] Since the soft core support is a wax patch between the ceramic core surface and the wax mold cavity surface, the lower surface of the soft core support is the ceramic core surface, and the upper surface is the wax mold cavity surface. The projection planes of the soft core support fitting points on the upper and lower surfaces are both rectangles. With the current soft core support fitting point as the center, make a rectangle with a length of 5mm and a width of 4mm. Then the vertices of the rectangular area projected onto the ceramic core surface are recorded as: a, b, c, d; discretize the four sides of the rectangle into a point cloud, and calculate the projection of each point along the normal direction of its ceramic core surface to the cavity surface, forming new rectangular vertices recorded as: a', b', c', d'. Fit the projection points of the upper and lower surfaces into a spline curve, and the enclosed cavity surface is used as the upper surface of the soft core support. Thus, the hexahedron is obtained as the actual geometric shape of the soft core support, and the height of the center fitting point is the current soft core support size, such as Figure 3 shown.

[0063] Step 3, determine the soft core support material addition and subtraction composite preparation processing sequence;

[0064] According to the platform structure of the soft core support additive and subtractive material equipment, the ceramic core profile structure and the position of the soft core support, the soft core support blank is first prepared at the ceramic core blade basin, and then the actual soft core support size and milling allowance are determined by detection, and finally the soft core support is milled; then, the same additive and subtractive material processing and detection procedures are performed on the back of the ceramic core blade. Thus, the preparation of the entire ceramic core profile soft core support is completed.

[0065] Step 4: Common preparation of ceramic core surface soft core support blanks. Analyze the soft core support preparation materials, determine the printing process parameters and printing trajectory;

[0066] According to the size and geometric shape of the soft core support, the actual soft core support is firstly subjected to layered slicing. Since the lower surface of the soft core support is the ceramic core profile and the upper surface is the model cavity profile, both of which are free-form surfaces, this embodiment establishes a surface layering method.

[0067] First, the actual state of the ceramic core surface soft core support model is layered, and the soft core support is divided into two parts. The first part is the free surface position that fits the ceramic core surface, and the second part is the rectangular area of ​​the soft core support. Figure 4 The first part can be regarded as the differential of the NUBRS surface under the soft core support size, and its printing path can be decomposed into B-splines; the second part is the plane layering under the regular shape.

[0068] Then, wax filling is performed according to the layering results of the soft core support. The method adopted is the FDM direct writing pneumatic extrusion nozzle. Due to the influence of the material's own characteristics and the curvature of the ceramic core surface, the nozzle diameter is selected to be 0.5mm. Combined with the adhesion mechanism of the two materials during conformal printing, the soft core support preparation material is the same material as the investment casting wax model, which has smaller thermal diffusivity and shrinkage, and belongs to medium-temperature wax. The process parameters are: extrusion pressure is 0.015mpa; heating temperature is 75℃, and moving trajectory speed is 15mm / s. A reciprocating trajectory from outside to inside is used for soft core support printing trajectory planning. Since the ceramic core surface is a free-form surface, a four-axis linkage method is used for overall printing path planning.

[0069] Since the bottom of the soft core support is a free-form surface, a four-axis four-linkage method is used to plan the layered printing path of the soft core support surface. Assuming that the thickness of the soft core support at a certain point is 3mm, it is divided into 10 layers and a reciprocating trajectory from the outside to the inside is used to plan the printing trajectory of the soft core support.

[0070] Step 5: Detect the size of the soft core support blank;

[0071] Use a point laser measuring instrument to detect the upper surface of the soft core support blank, determine the actual fit point position size and compare it with the theoretical calculated value, and then determine the size of the milling allowance. When the actual size is larger than the theoretical size, determine the size of the CNC milling allowance; otherwise, perform size compensation on the existing soft core support.

[0072] Step 6: Milling of soft core support, determining processing parameters;

[0073] Since the upper surface of the soft core support fits the inside of the mold cavity (i.e., the mold cavity surface is a free-form surface), it is necessary to achieve surface processing through CNC milling. The soft core support uses wax material used for investment casting wax patterns, which has a small thermal diffusivity and shrinkage rate and belongs to medium-temperature wax; the amount of milling removal is determined based on the actual size results. The actual size of the soft core support is a rectangular block of 5mm×5mm×3mm.

[0074] A four-axis platform is used to mill the soft core support. According to the machine tool structure, the ceramic core soft core support is parallel to the Y axis, and the tool axis vector is the Z axis. A high-speed steel ball head milling cutter with a ball head radius of 4mm is selected. The tool handle is 75mm long. In order to facilitate chip removal, 2 teeth are selected.

[0075] Firstly, the CAM module in UG software is used to program the tool path trajectory of the four-axis linkage milling of the soft core support blank, and it is converted into Gcode instructions after post-processing. At the same time, the tool path simulation verification is performed using Vericut software, and finally it is transmitted to the ceramic core surface soft core support adaptive additive and subtractive composite processing platform. According to the actual soft core support machining allowance and material properties, a ball head tool made of high-speed steel with a tool head diameter of 4mm is selected. In order to facilitate chip removal, the tool teeth number is selected as 2. Set the electric spindle speed to 12000r / min; the feed speed to 300mm / min; the cooling method is air cooling. Thus, the CNC milling of the soft core support is completed.

[0076] Step 7: Soft core support molding size and surface quality inspection;

[0077] Recheck the soft core support after milling in the same way as in step 5 to make sure that its size meets the theoretical requirements and the error range is guaranteed to be within 0.01mm. If the size detection accuracy error does not exceed 0.01mm, it is considered that the soft core support processing meets the requirements; otherwise, perform secondary milling. Since the upper surface of the soft core support fits the cavity, its surface quality should be close to that of the blade wax model, so as to ensure that there will be no defects on the blade profile after casting.

[0078] At the same time, the tool scanner is used to detect the actual wax pattern surface roughness, and the surface roughness of the soft core support is also detected. The two are compared and analyzed to analyze the actual soft core support processing quality, thereby completing the adaptive preparation of the ceramic core soft core support.

[0079] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.

Claims

1. An adaptive preparation method for ceramic core soft core support based on additive and subtractive composite processing, Features Specific steps: Individual ceramic core surface inspection and error analysis; Combined with the wax mold cavity, calculate the actual geometric shape and size of the soft core support of the ceramic core surface; A solid blank of a soft core support is prepared by conformal printing, wherein the free-form surface position of the soft core support that is attached to the ceramic core mold surface is obtained by decomposing a B-spline curve to obtain a printing path, a planar rectangular area located in the middle of the soft core support is printed by plane layering, and a free-form surface position attached to the cavity surface is obtained by decomposing a B-spline curve to obtain a printing path; Measure the size of the soft core support solid blank to determine the machining allowance for material reduction; Soft core support CNC milling processing; Soft core support forming accuracy detection and evaluation.

2. According to claim 1, a method for adaptively preparing a ceramic core soft core support based on composite processing of additive and subtractive materials, Features: The method for calibrating the soft core support position is: Based on the measured actual ceramic core surface parameters, the three-dimensional model of the individual ceramic core surface is reconstructed; Performing model registration on the three-dimensional reconstructed model of the individual ceramic core profile and the theoretical ceramic core profile model to obtain the actual ceramic core profile manufacturing error; Based on the error analysis results of the individual ceramic core profile, the soft core support fitting points are re-determined on the simulation model of the actual ceramic core profile, thus completing the calibration of the soft core support position.

3. According to claim 1, a method for adaptively preparing a ceramic core soft core support based on composite processing of additive and subtractive materials, Features: The geometric shape and size calculation method of the soft core support is: Constructing a rectangular area at the determined soft core support position as a soft core support geometry, and discretizing four sides of the rectangular area into point cloud data; Calculate the normal direction of each point along its ceramic core surface and project it onto the cavity surface of the wax mold; The projection points on the cavity surface are fitted into a spline curve, and the enveloping cavity surface is the upper surface of the soft core support; The geometric shape of the soft core support is obtained by stretching the bottom surface of the soft core support to the upper surface of the soft core support.

4. According to claim 3, a method for adaptively preparing a ceramic core soft core support based on composite processing of additive and subtractive materials, Features: The additive method for preparing the soft core support solid blank is a conformal printing process, using an FDM direct writing pneumatic extrusion nozzle with a nozzle diameter of 0.5 mm and printing process parameters: extrusion pressure of 0.015 MPa, heating temperature of 75° C., and moving trajectory speed of 15 mm / s.

5. According to claim 1, a method for adaptively preparing a ceramic core soft core support based on composite processing of additive and subtractive materials, Features: The method for determining the subtractive machining allowance of the soft core support solid blank is to perform size detection on the soft core support solid blank by using a point laser, and compare it with the theoretical soft core support size to obtain the size deviation; when the actual size is larger than the theoretical size, determine the size of the CNC milling machining allowance; when the actual size is smaller than the theoretical size, perform size compensation on the soft core support solid blank.

6. According to claim 5, a method for adaptively preparing a ceramic core soft core support based on composite processing of additive and subtractive materials, Features: The CNC milling processing method for the soft core support is to determine the curved surface processing trajectory of the upper surface of the soft core support through a multi-axis linkage processing system, then determine the processing trajectory of the side wall plane of the soft core support, connect the local processing trajectories, and obtain the CNC milling processing path of the soft core support; according to the determined processing path, drive the tool movement of the multi-axis linkage processing system, combine with three-dimensional measurement, and obtain the solid soft core support after fine processing.

7. According to claim 6, a method for adaptively preparing a ceramic core soft core support based on composite processing of additive and subtractive materials, Features: The multi-axis linkage processing system is a four-axis linkage CNC processing equipment, and the processing parameters are: the electric spindle speed is 12000r / min; the feed speed is 3000mm / min; the cooling method is air cooling.

8. According to claim 1, a method for adaptively preparing a ceramic core soft core support based on composite processing of additive and subtractive materials, Features: The soft core support forming accuracy detection and evaluation method is to use a point laser measuring instrument to detect the processed soft core support to determine whether its size meets the theoretical requirements and the error range is guaranteed to be within 0.01mm; then use a tool scanner to detect the surface roughness of the soft core support on the ceramic core mold surface, and compare and analyze it with the roughness of the precision casting wax mold surface, and finally evaluate the actual soft core support processing surface quality.

9. A device for preparing a ceramic core soft core support, Features: A method for adaptively preparing a ceramic core soft core support based on additive and subtractive composite processing as described in any one of claims 1 to 8; comprising a support column and a position calibration module, a measuring module, an additive manufacturing module, and a milling processing module integrated thereon, wherein the support column is arranged on a workbench, and the ceramic core to be processed is installed on the workbench through a fixture and a rotating spindle turntable; the measuring module, the additive manufacturing module, and the milling processing module respectively provide three workstations of measurement, additive manufacturing, and milling processing, and the motion switching control of the three workstations is realized through the control of a host computer; the surface of the ceramic core is measured by the measuring module, and the collected coordinate information of the ceramic core surface points is sent to the host computer, and the rotating spindle is controlled to adaptively adjust the position of the ceramic core according to the collected information; the soft core support blank is additively prepared by setting a position on the surface of the ceramic core by the additive manufacturing module; the soft core support blank prepared by additive processing is fine-processed by the milling processing module; the three workstations of measurement, additive manufacturing, and milling processing are positioned by the position calibration module.

10. A device for preparing a ceramic core soft core support according to claim 9, Features: The position calibration module includes a visual inspection camera, which is used to calibrate the relative position relationship between the three workstations of measurement, additive manufacturing, and milling processing; the single pixel accuracy of the visual camera is 0.0038mm / pix, the detection field of view is: 19.4mm*19.4mm, and the working distance is 110mm; the calibration method of the position calibration module is: Lower the print head of the additive manufacturing module to the working position, and perform a "cross" wax print on the reference plane, which is recorded as position A; Reset the print head and lower the NC milling spindle of the milling processing module to the working position, and perform "cross" milling in the reference plane, which is recorded as position B; Use the visual inspection camera to take pictures of the platform reference surface, calculate the XY direction deviation at the AB position, and perform coordinate calibration; Move each workstation to the position of the tool setting probe and calibrate the Z-direction coordinates by touching the tool setting probe.

Citation Information

Patent Citations

  • Turbine blade ceramic core soft core support machining method

    CN106002112A

  • 3D printing method for soft ceramic core support of turbine blade

    CN106079433A

  • Hollow turbine blade precision casting wax pattern model reconstruction method under incomplete measurement data

    CN110851967A

  • Hollow turbine blade ceramic core soft core support positioning layout optimization method

    CN118627228A

  • Additive and subtractive composite machining platform for ceramic core soft core support of hollow turbine blade

    CN118720059A