Preparation method of powder high temperature alloy ring
Through the preparation method of powder high-temperature alloy ring parts, the cooling rate range is optimized by using thermal isostatic pressure and solid solution treatment, which solves the problems of low material utilization and insufficient mechanical properties in the existing process, and realizes the efficient preparation of ring parts and Performance improvement.
Patent Information
- Application Number
- CN202411216506.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-02
AI Technical Summary
The existing manufacturing process of high-temperature alloy ring parts has problems such as low material utilization, high cost and insufficient mechanical properties, especially in terms of tensile yield strength and composite durability at high temperatures.
The preparation method of powder high-temperature alloy ring parts is adopted, through thermal isostatic pressure treatment and solid solution treatment, combined with machining, the assembly method and cover structure of the ring blank are adjusted, and the cooling rate range is optimized to improve material utilization and mechanical properties.
The process flow is simplified, the cost is reduced, and the material utilization is improved significantly, and the structure uniformity and mechanical properties of the annular parts are significantly improved, especially the tensile yield strength and composite durability at 650°C and 750°C.
Smart Images

Figure CN118720143B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of powder metallurgy, and in particular to a method for preparing a powder high-temperature alloy ring part. Background Art
[0002] With the development of high thrust-to-weight ratio aircraft engines, the operating temperature and performance requirements for key hot end components of the engine, such as turbine disks, are becoming increasingly higher. The manufacturing process of ring parts mainly includes two methods: traditional vacuum melting + forging deformation process, hot isostatic pressing + rolling ring parts. The first method is to prepare large-sized ingots into ring parts of final size through multiple processes such as upsetting, punching, stamping, heat treatment and machining. The process has the following main shortcomings: (1) The large-size ingot cast by the master alloy will cause serious segregation of the ingot, coarse and uneven structure, which will make it difficult to open the ingot and forge deformation, and this defect will be inherited to the final ring structure, resulting in isotropic differences in the performance of the ring; (2) The process of preparing the ring includes multiple upsetting and punching processes, which will cause material loss and low material utilization; (3) In order to ensure the forming size of the delivered ring, it is necessary to go through at least 2 upsetting and rolling processes to obtain a fine grain structure, and the ring blank will be repeatedly heated, kept warm, unloaded and rolled. The preparation process is complicated and the cost is high. Although the second method has the advantage of a short process compared to the first method, it still has shortcomings: (1) The mechanical properties of the ring still have problems such as low tensile yield strength margin at 650℃ and easy fracture of the composite endurance at 750℃; (2) The utilization rate of powder materials and production costs still need to be further optimized.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a powder high-temperature alloy ring part, which has a short process flow, high material utilization rate, low cost, and at the same time, the mechanical properties of the prepared ring part are significantly improved.
[0005] In order to achieve the above-mentioned object of the present invention, the present invention provides a method for preparing a powder high-temperature alloy ring, comprising the following steps:
[0006] S1. The high temperature alloy powder is loaded into the annular casing structure and hot isostatic pressing is performed to obtain a ring blank;
[0007] S2. The ring blank is subjected to solution treatment and aging treatment, and then machined to obtain the finished ring part;
[0008] The ring blank is a superposition of X ring parts before machining in the axial direction, where X is selected from an integer ≥ 1; the center hole of the annular sleeve is vacant or has an iron core in the gap;
[0009] The assembly method is adjusted so that the characteristic cooling rate value of the ring blank during the cooling process of the solution treatment is within the optimized characteristic cooling rate value range; the assembly method includes: the selection of X and the setting method of the center hole of the annular sleeve;
[0010] The acquisition of the characteristic cooling rate value includes: using Deform software to perform numerical simulation of S1 and S2 in a corresponding assembly mode, selecting at least one part of the ring blank as a test point, obtaining the cooling rate of the test point at different temperatures during the furnace cooling process of the solution treatment, and drawing a curve with the cooling rate as the ordinate and the temperature as the abscissa. The value of the ordinate corresponding to the highest point of the curve is the characteristic cooling rate value;
[0011] The acquisition of the optimized characteristic cooling rate value range includes: selecting at least one parameter from the tensile strength and yield strength of the ring part, and determining a preset target value; establishing a functional relationship between the selected parameter and the characteristic cooling rate value, and acquiring the optimized characteristic cooling rate value range that makes the selected parameter meet the preset target value according to the functional relationship.
[0012] In a specific embodiment of the present invention, a plurality of test points are arranged in the ring blank according to the value of X and the radial dimension of the ring blank.
[0013] In a specific embodiment of the present invention, in obtaining the characteristic cooling rate value, at least two or more test points are selected to calculate the characteristic cooling rate values respectively; and the assembly method is adjusted so that the characteristic cooling rate values of more than 80% of the test points are within the optimized characteristic cooling rate value range.
[0014] In a specific embodiment of the present invention, it also includes: a machining treatment method for the annular sleeve before the solid solution treatment; the machining treatment method for the annular sleeve before the solid solution treatment includes any one of the following methods:
[0015] (1) Do not remove the cover (i.e., full cover);
[0016] (2) Machining to remove all the sleeves (i.e. no sleeves);
[0017] (3) Machining to remove the sleeve at the center hole of the annular sleeve (i.e., the sleeve has no inner skin);
[0018] (4) Machining to remove the center hole of the annular sleeve and the sleeve on the upper and lower end surfaces (i.e., leaving the outer skin of the sleeve).
[0019] In a specific embodiment of the present invention, the machining treatment method is adjusted so that the characteristic cooling rate value of the ring blank during the cooling process after the solution treatment is within the second optimized characteristic cooling rate value range or partially lower than the second optimized characteristic cooling rate range;
[0020] The acquisition of the second optimized characteristic cooling rate value range includes: selecting an existing ring-shaped product of the same type as the ring-shaped alloy, simulating the ring-shaped product according to the actual preparation process, selecting at least 3 test points in the ring-shaped product, and obtaining the characteristic cooling rate values of each test point during the solution treatment, so that the maximum value and the minimum value of the obtained characteristic cooling rate values of the ring-shaped product constitute the second optimized characteristic cooling rate range.
[0021] In a specific embodiment of the present invention, when adjusting the machining treatment method, the characteristic cooling rate values of more than 80% of the test points of the ring blank are within the second optimized characteristic cooling rate value range.
[0022] In a specific embodiment of the present invention, the preparation of the high-temperature alloy powder includes: preparing a master alloy rod by vacuum horizontal continuous casting technology, then preparing powder by plasma rotating electrode method, and screening and selecting powder with a particle size range of 50 to 150 μm.
[0023] In a specific embodiment of the present invention, the annular member includes at least one of a sealing disk, a baffle ring, a front baffle plate and a rear baffle plate.
[0024] Another aspect of the present invention provides a method for preparing a powder high-temperature alloy ring, comprising the following steps:
[0025] (a) High-temperature alloy powder is loaded into an annular casing structure and subjected to hot isostatic pressing to obtain a ring blank;
[0026] (b) subjecting the ring blank to a solution treatment and an aging treatment, and then machining to obtain the finished ring part;
[0027] The ring blank is a superposition of X ring parts before machining in the axial direction, where X is an integer between 4 and 8; the center hole of the ring sleeve is vacant;
[0028] Before the solution treatment, the ring blank is machined to remove the sheath at the center hole of the annular sheath.
[0029] In a specific embodiment of the present invention, the high temperature alloy powder includes at least one of FGH4091, FGH4095, FGH4096, FGH4097, FGH4098 and FGH4099.
[0030] In a specific embodiment of the present invention, in the annular sheath structure, the outer diameter of the sheath is 1.07×D~1.1×D, the inner diameter of the sheath is 0.95×d~0.98×d, the height of the sheath is 1.29×H×X~1.34×H×X, and the thickness of the sheath is 5~10mm; wherein D, d, and H are respectively the outer diameter, inner diameter, and height of the finished annular component, and X is the number of corresponding annular components in the stacked body. Furthermore, the material of the annular sheath structure is low carbon steel or stainless steel.
[0031] In a specific embodiment of the present invention, during the hot isostatic pressing treatment, the temperature is 1160-1210°C, the pressure is ≥120MPa, and the heat preservation and pressure holding time is ≥2h. Furthermore, during the hot isostatic pressing treatment, after heat preservation and pressure holding, the heat preservation and pressure holding are followed by furnace cooling.
[0032] In a specific embodiment of the present invention, in step (b), the machining includes: removing the upper and lower end surfaces of the annular sleeve and the outer cylindrical sleeve, and then machining and cutting according to the size of the delivered annular part.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] (1) In the preparation method of the present invention, the packaging and assembly method of the ring-shaped part is changed, and the powder high-temperature alloy ring blank is directly obtained by hot isostatic pressing to obtain a near-net shape, and then heat treatment and machining are performed to obtain the finished ring-shaped part. Compared with the existing preparation process, the present invention has the advantages of shorter preparation process, lower cost, and higher material utilization rate;
[0035] (2) The preparation method of the present invention can produce ring-shaped parts with good uniformity of structure and good mechanical properties by changing the packaging and assembly method of the ring-shaped parts and cooperating with the heat treatment process. The ring-shaped parts have high tensile yield strength at 650°C and 750°C, and stable composite endurance performance at 750°C without notch sensitivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0037] Figure 1 A schematic diagram of various packaging assembly methods provided by an embodiment of the present invention;
[0038] Figure 2 Schematic diagram of four machining treatment methods for the annular sleeve before solution treatment provided in embodiments of the present invention;
[0039] Figure 3 A simplified diagram of the process flow for preparing a powder high-temperature alloy ring member provided in an embodiment of the present invention;
[0040] Figure 4 The morphology of the high-temperature alloy powder provided in the embodiment of the present invention; (a) and (b) correspond to different magnifications respectively;
[0041] Figure 5 The relationship between temperature and time during the cooling process of the solution heat treatment corresponding to the various packaging assembly methods provided in the embodiment of the present invention; Figure 1 The assembly methods of (Ⅰ) to (Ⅳ);
[0042] Figure 6 A graph showing the relationship between the cooling rate and the temperature at different test points during the cooling process of the solution heat treatment corresponding to the various packaging assembly methods provided in the embodiments of the present invention;
[0043] Figure 7 A relationship diagram between characteristic cooling rate and room temperature tensile strength of a qualified product provided by an embodiment of the present invention;
[0044] Figure 8 The relationship between temperature and time during the cooling process of the solution heat treatment corresponding to the four machining treatment methods of the annular sleeve before the solution treatment provided in the embodiment of the present invention; Figure 2 Machining methods (Ⅰ) to (Ⅳ) in the above;
[0045] Fig. 9 A graph showing the relationship between the cooling rate and the temperature at different test points during the out-of-furnace cooling process of the solution heat treatment corresponding to the four machining treatment methods for the annular sheath before the solution treatment provided in the embodiments of the present invention; (a) to (c) respectively correspond to the test points near the center hole, the middle and the edge of the axial center of the different machining methods, (d) to (f) respectively correspond to the test points near the center hole, the middle and the edge of the axial middle of the different machining methods, and (h) to (j) respectively correspond to the test points near the center hole, the middle and the edge of the axial top of the different machining methods;
[0046] Fig.10 The alloy grain structure of the ring-shaped part prepared in Example 1 of the present invention;
[0047] Fig.11 The alloy grain structure of the ring member prepared in Comparative Example 1 of the present invention;
[0048] Fig.12 The precipitated phase structure of the ring-shaped part prepared in Example 1 of the present invention;
[0049] Fig.13 This is the precipitation phase structure of the ring-shaped part prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0050] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0051] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0052] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0053] In one aspect, the present invention provides a method for preparing a powder high-temperature alloy ring, comprising the following steps:
[0054] S1. The high temperature alloy powder is loaded into the annular casing structure and hot isostatic pressing is performed to obtain a ring blank;
[0055] S2. The ring blank is subjected to solution treatment and aging treatment, and then machined to obtain a finished ring part;
[0056] The ring blank is a superposition of X ring parts before machining in the axial direction, where X is selected from an integer ≥ 1; the center hole of the ring sleeve is vacant or has an iron core in the gap;
[0057] The assembly method is adjusted so that the characteristic cooling rate value of the ring blank during the cooling process of the solution treatment furnace is within the optimized characteristic cooling rate value range; the assembly method includes: the selection of X and the setting method of the center hole of the annular sleeve;
[0058] The acquisition of the characteristic cooling rate value includes: using Deform software to perform numerical simulation of S1 and S2 under the corresponding assembly mode, selecting at least one part of the ring blank as a test point, obtaining the cooling rate of the test point at different temperatures during the furnace cooling process of the solution treatment, and drawing a curve with the cooling rate as the ordinate and the temperature as the abscissa. The value of the ordinate corresponding to the highest point of the curve is the characteristic cooling rate value;
[0059] The acquisition of the optimized characteristic cooling rate value range includes: selecting at least one parameter from the tensile strength and yield strength of the ring part, and determining a preset target value; establishing a functional relationship between the selected parameter and the characteristic cooling rate value, and acquiring the optimized characteristic cooling rate value range that makes the selected parameter meet the preset target value according to the functional relationship.
[0060] The present invention uses Deform software to simulate and calculate the cooling rates of different parts during the solution treatment process under different assembly methods, and obtains corresponding characteristic cooling rate values; by adjusting the assembly method, the characteristic cooling rate value is within the optimized characteristic cooling rate value range. The actual preparation of the ring part under such an assembly method can not only improve the material utilization rate and reduce the cost, but also ensure the uniformity of the organization and the consistency of the performance of the ring part, and at the same time improve the mechanical properties of the ring part.
[0061] The present invention changes the packaging and assembly method of the ring parts, and can directly adopt the above steps to obtain the ring parts, thereby avoiding the multi-fire forging deformation process in the traditional ring part manufacturing process and the rolling process of the existing hot isostatic pressing to prepare the ring parts, simplifying the process flow, improving material utilization, and the organizational properties and mechanical properties of the obtained ring parts are better.
[0062] When numerical simulations of S1 and S2 are performed under the selected assembly method, the corresponding numerical simulation models are constructed with the actual preparation parameters of the annular parts.
[0063] In actual operation, X ring parts can be combined to use one package, and X can be an integer such as 1, 2, ... 5, ... 10, ... 15, ... In addition, in order to further reduce the amount of powder and save costs, the number of ring parts X used in combination with one package can be further optimized according to the number of delivered ring parts N, such as X = N / n, n is an integer ≥ 1, n ≤ N, that is, N ring parts are equally divided into n identical ring packages, which can not only reduce the amount of powder and improve processing efficiency, but also ensure the consistency of the ring parts.
[0064] The present invention takes the number of delivered annular parts N=6 as an example, and explains the annular package assembly method as follows. In actual operation, the number of delivered annular parts N is 6. In other cases, the design principle is the same and will not be repeated here.
[0065] When N=6, the package can be used as follows Figure 1 The assembly method shown, but not limited to this, the first (I) is "two-in-one", every 2 ring parts are combined into a sleeve; the first (II) is "three-in-one", every 3 ring parts are combined into a sleeve; the first (III) is a "six-in-one" sleeve without core, every 6 ring parts are combined into a sleeve. The center hole of the annular sleeve can be left empty, that is, no object is placed. It is also possible to fit the iron core in the gap of the center hole of the annular sleeve, that is, place an iron core object in the center hole, that is, the first (IV) is a "six-in-one" sleeve plus core. The assembly methods of the first (I) and the second (II) can also choose the method of leaving the center hole empty or fitting with an iron core in the gap according to the characteristic cooling rate value. The corresponding specific assembly method of fitting with an iron core in the gap is not shown in the figure.
[0066] In a specific embodiment of the present invention, a plurality of test points are set in the ring blank according to the value of X and the radial dimension of the ring blank.
[0067] In a specific embodiment of the present invention, in obtaining the characteristic cooling rate value, at least two or more test points are selected to calculate the characteristic cooling rate values respectively; and the assembly method is adjusted so that the characteristic cooling rate values of more than 80% of the test points are within the optimized characteristic cooling rate value range. For example, when the number of test points is a, the characteristic cooling rate values corresponding to more than 80% of the test points, i.e., ≥80%×a test points, are within the optimized characteristic cooling rate value range.
[0068] In a specific embodiment of the present invention, when X is an even number, in obtaining the characteristic cooling rate value, n×X / 2 test points are selected to calculate the characteristic cooling rate value respectively, and n is an integer ≥1; when X is an odd number, in obtaining the characteristic cooling rate value, n×(X+1) / 2 test points are selected to calculate the characteristic cooling rate value respectively, and n is an integer ≥1.
[0069] In actual operation, the center point of each ring part in the ring blank can be selected as the test point, and n×X / 2 or (X+1) / 2 ring parts can be selected continuously from top to bottom or from bottom to top. Figure 3 As an example of several assembly methods, the selection of specific test points can be as follows Figure 3 As shown in, but not limited to.
[0070] In a specific embodiment of the present invention, in the numerical simulation performed by selecting X and the arrangement of the center hole of the annular sleeve, the annular sleeve is not removed before the solution treatment, and if there is a matching iron core, the iron core is removed.
[0071] The method for obtaining the optimized characteristic cooling rate value range may specifically include: selecting at least 3 ring-shaped products with qualified comprehensive performance of the same known alloy type and the same preparation process, wherein a qualified ring-shaped product refers to a product whose tensile strength and yield strength meet the customer's preset target values; testing its room temperature or high temperature tensile strength, or room temperature or high temperature yield strength, and then simulating it according to its actual preparation process to obtain the characteristic cooling rate value of its corresponding test point during the cooling process of the solution treatment furnace.
[0072] Among them, the same preparation process refers to the same master alloy smelting process, powder making process, hot isostatic pressing process, and heat treatment process; during the hot isostatic pressing process, the sleeve specifications correspond to the sleeve specifications of a single annular part, that is, in the annular sleeve structure, the sleeve outer diameter is 1.07×D~1.1×D, the sleeve inner diameter is 0.95×d~0.98×d, the sleeve height is 1.29×H~1.34×H, and the sleeve thickness is 5~10mm.
[0073] Among them, the shape of the selected existing ring-shaped product is similar to the shape of the target ring-shaped product of the present invention, and the outer diameter, inner diameter and height of the selected ring-shaped product are D', d', and H', respectively, satisfying: D'≥1.2D, d'≤0.6d, H'≥1.5H, such as D' can be 1.2D~1.5D, d' can be 0.25d~0.6d, and H' can be 1.5H~4H.
[0074] In actual operation, in obtaining the optimized characteristic cooling rate value range, the test points are the same as the test points selected for obtaining the characteristic cooling rate values. The assembly method is adjusted so that during the cooling process of the ring blank out of the furnace after solution treatment, the characteristic cooling rate values of more than 80% of the test points are within the corresponding optimized characteristic cooling rate value range.
[0075] The characteristic cooling rate values obtained by numerical simulation of S1 and S2 by the Deform software of the present invention under different assembly modes are compared with the optimized characteristic cooling rate value range, and an assembly mode that can make the characteristic cooling rate value of the ring blank during the solution treatment furnace cooling process within the optimized characteristic cooling rate value range is selected, that is, X is selected and the setting method of the center hole of the annular sleeve is selected.
[0076] In a specific embodiment of the present invention, it also includes: a machining treatment method for the annular sleeve before the solution treatment; the machining treatment method for the annular sleeve before the solution treatment includes any one of the following methods:
[0077] (1) Do not remove the cover (i.e., full cover);
[0078] (2) Machining to remove all the sleeves (i.e. no sleeves);
[0079] (3) Machining to remove the sleeve at the center hole of the annular sleeve (i.e., the sleeve has no inner skin);
[0080] (4) Machining to remove the center hole of the annular sleeve and the sleeve on the upper and lower end surfaces (i.e., leaving the outer skin of the sleeve).
[0081] Figure 2 Schematic diagram of four machining treatment methods for the annular sleeve before solution treatment provided by the embodiment of the present invention. By adjusting the machining treatment method for the annular sleeve before solution treatment, the heat treatment state of the ring blank during solution treatment is further adjusted, and the performance of the ring blank is further optimized.
[0082] In a specific embodiment of the present invention, the machining treatment method is adjusted so that the characteristic cooling rate value of the ring blank during the cooling process of the solution treatment is within the second optimized characteristic cooling rate value range or partially lower than the second optimized characteristic cooling rate range;
[0083] The acquisition of the second optimized characteristic cooling rate value range includes: selecting an existing ring-shaped product of the same alloy type as the ring-shaped product, simulating the ring-shaped product according to the actual preparation process, selecting at least 3 test points in the ring-shaped product, and obtaining the characteristic cooling rate values of each test point during the solution treatment, so that the maximum value and the minimum value of the characteristic cooling rate values of the ring-shaped product constitute the second optimized characteristic cooling rate range.
[0084] When obtaining the second optimized characteristic cooling rate value range, the selected existing ring-shaped product is similar in shape to the target ring-shaped product of the present invention, and the outer diameter, inner diameter and height of the selected ring-shaped product are D'', d'' and H'' respectively, satisfying: D''≥0.85D, d''≤0.9d, H''≥2.5×X×H, such as D'' can be 0.85D~D, d'' can be 0.75d~0.9d, and H'' can be 2.5×X×H~3.5×X×H.
[0085] In a specific embodiment of the present invention, when adjusting the machining treatment method, the characteristic cooling rate values of more than 80% of the test points of the ring blank are within the second optimized characteristic cooling rate value range.
[0086] In actual operation, the characteristic cooling rate values corresponding to each test point of different machining treatment methods are obtained respectively, and the characteristic cooling rate values are compared with the second optimized characteristic cooling rate value range to ensure that the characteristic cooling rate values of more than 80% of the test points are within the second optimized characteristic cooling rate range. When there is a test point where the characteristic cooling rate value is not within the second optimized characteristic cooling rate range, it is preferred to select the case where the characteristic cooling rate value corresponding to the test point is lower than the second optimized characteristic cooling rate range. Among them, since the calculated characteristic cooling rate value and the optimized characteristic cooling rate range both correspond to negative values, the lower than here means that the absolute value of the characteristic cooling rate value is less than the absolute value of the values at both ends of the optimized characteristic cooling rate range.
[0087] In a specific embodiment of the present invention, the arrangement of X and the center hole of the annular sleeve is first selected, and then the machining treatment method of the annular sleeve before solution treatment is selected.
[0088] In a specific embodiment of the present invention, in the dimension design of the annular sheath structure, MSC.MARC software is used in combination with CAD drawing software, and numerical simulation software is used to calculate the shrinkage deformation of the sheath during hot isostatic pressing to obtain the sheath dimensions.
[0089] Among them, the calculation of the shrinkage deformation of the sheath during hot isostatic pressing by numerical simulation software includes: obtaining the parameters of the high-temperature alloy powder and the sheath material, inputting the annular sheath structure, the sheath material parameters and the high-temperature alloy powder parameters into the software, and auxiliary thermodynamic software JMat.Pro is used to calculate the thermophysical parameters of the high-temperature alloy powder and the sheath material, and obtain the material parameters of the high-temperature alloy powder and the sheath (Poisson's ratio, Young's modulus, thermal expansion coefficient, specific heat solution, thermal conductivity, etc.) with temperature. In addition, it is also necessary to combine the test results of the tensile test of the powder high-temperature alloy material at different temperatures, such as the yield stress parameter value, as a reference for simulating the stress deformation degree of each part of the sheath under the action of high-temperature three-dimensional pressure during hot isostatic pressing. Then select the calculation model parameters in the MSC.Marc software, and continuously optimize the iterative calculation results according to the actual size of the sheath after deformation after hot isostatic pressing of similar alloy products, so as to obtain the shrinkage deformation data of the sheath. In the optimal iterative calculation, the goal is to select the sheath size that is closest to the size of the final delivery product blank, so as to reduce the amount of powder in the sheath and reduce production costs. This method is to predict the shrinkage of the turbine disk jacket by simulating it, thereby providing a basis for determining the size of the turbine disk.
[0090] In a specific embodiment of the present invention, the preparation of high temperature alloy powder includes: preparing master alloy rods by vacuum horizontal continuous casting technology, then preparing powder by plasma rotating electrode method, and screening and selecting powder with a particle size range of 50 to 150 μm.
[0091] In a specific embodiment of the present invention, the annular member includes at least one of a sealing disk, a baffle ring, a front baffle plate and a rear baffle plate.
[0092] The present invention takes a sealing disk made of FGH4097 high-temperature alloy (specification dimensions: outer diameter 380-400mm, inner diameter 270-290mm, height 21-23mm) and its corresponding sealing disk made of existing specification GH4079 high-temperature alloy (specification dimensions are the same as those of the FGH4097 alloy sealing disk) as examples to illustrate the preparation method of FGH4097 high-temperature alloy ring parts.
[0093] Figure 3A simplified process flow chart of the preparation process of a powder high-temperature alloy ring member provided in an embodiment of the present invention is as follows: Figure 3 As shown, the method for preparing the powder high temperature alloy ring of this embodiment includes the following steps:
[0094] (1) The master alloy bars are prepared by vacuum horizontal continuous casting (VHCC) technology;
[0095] (2) Powder making using plasma rotating electrode method (PREP);
[0096] (3) Direct hot isostatic pressing to prepare ring blanks by near-net forming;
[0097] (4) machining the ring blank obtained in step (3) before heat treatment;
[0098] (5) Heat treatment, including solution treatment and aging treatment;
[0099] (6) The delivered ring parts are obtained by machining.
[0100] In step (1), the master alloy bar is prepared by vacuum horizontal continuous casting (VHCC) technology, and the master alloy bar meets the requirements of GB / T 38941-2020 "High-temperature alloy bar for plasma rotary electrode atomization powder making". The master alloy bar is a round bar, the bar diameter can be 30-100 mm, and the bar length can be determined according to the powder making process requirements. The surface quality requirements of the bar need to be bright after machining and grinding, and there are no visible black spots, slag, cracks and secondary shrinkage defects at both ends and the outer circumference, no oil stains in the center hole, and the surface roughness Ra should not be greater than 1.6μm. In addition, the master alloy bar can also be melted by vacuum induction melting plus vacuum arc remelting, vacuum induction melting plus electroslag remelting, or vacuum induction melting plus vacuum arc remelting plus electroslag remelting. The present invention does not elaborate on the specific operation of preparing the master alloy rod by the VHCC technology, and adopts the existing vacuum horizontal continuous casting (VHCC) technology to prepare the master alloy rod.
[0101] In step (2), PREP is used to prepare high-temperature alloy spherical powder, and the obtained powder meets the requirements of GB / T 38815-2020 "Plasma Rotating Electrode Atomized High-temperature Alloy Powder". The number of non-metallic inclusions in each 1.0 kg of alloy powder is not more than 20, and the size of non-metallic inclusions is not more than 150 μm. The O content in the powder is ≤70ppm, and the N content is ≤50ppm. In the preparation method of the powder high-temperature alloy ring of the present invention, the powder is directly subjected to hot isostatic pressing near-net forming by a certain packaging assembly method, and the heat treatment process is combined to help improve the uniformity of the structure; the present invention has wider requirements for the particle size of the powder used for hot isostatic pressing, and the powder that meets the following requirements: the powder particle size range is 50 to 150 μm, and the particle size D50 in the laser particle size distribution is 80 to 90 μm. The mechanical properties of the powder high-temperature alloy ring prepared by the present invention using the powder that meets the above particle size requirements all meet the indicators. Under the condition of meeting the performance index, the powder with a wider particle size range can be selected to improve the powder utilization rate and greatly reduce the production cost. The specific operation of the PREP process for preparing the high-temperature alloy spherical powder is not described in detail in the present invention, and the existing conventional PREP process can be used; the powder is screened and electrostatically removed to select the powder with a particle size range of 50 to 150 μm, and the particle size D50 in the laser particle size distribution is 80 to 90 μm. Figure 4 Shown is a morphology of FGH4097 high temperature alloy powder prepared by PREP according to an embodiment of the present invention.
[0102] In step (3), the preparation of the ring blank by hot isostatic pressing near net forming includes: powder degassing, sleeve installation, sealing welding, hot isostatic pressing, etc. Taking the number of delivered ring parts N=6 as an example, according to Figure 1 The Deform software is used to perform numerical simulation of S1 and S2 under the corresponding assembly mode. Figure 1 The test points of the ring blank are selected as shown, and the relationship between temperature and time of each test point during the cooling process of the solution heat treatment is obtained as shown in the figure Figure 5 As shown. The slope of each point on the curve obtained from the temperature and time relationship diagram is the cooling rate. Then draw a curve with the cooling rate as the ordinate and the temperature as the abscissa. The value of the ordinate corresponding to the highest point of the curve is the characteristic cooling rate. Figure 1 The test points of the ring blank are selected as shown in the figure, and the relationship between the cooling rate and the temperature of each test point during the cooling process of the solution heat treatment is obtained as shown in the figure Figure 6 Table 1 shows the characteristic cooling rate values of different parts of the FGH4097 sealing disk.
[0103] Table 1 Characteristic cooling rate values of FGH4097 sealing disk
[0104]
[0105] According to the method for obtaining the optimized characteristic cooling rate value range, the room temperature tensile strength of other existing known qualified products prepared by the same alloy grade FGH4097 alloy according to the same process (such as taking product 1, product 2 and product 3 as examples, but not limited to this, the size of product 1 can be: outer diameter 510-535mm, inner diameter 100-113mm, height 48-58mm; the size of product 2 can be: outer diameter 508-525mm, inner diameter 80-90mm, height 66-76mm; the size of product 3 can be: outer diameter 500-510mm, inner diameter 140-150mm, height 40-50mm) is used as the corresponding control parameter, and 3 test points are selected along the radial direction of each product, which are named near the center hole, center, and edge respectively along the center hole to the edge, and the characteristic cooling rate of each test point of each product and the room temperature tensile strength relationship diagram are obtained, such as Figure 7 As shown, series 1 to series 9 correspond to the test results of each test point of products 1 to 3, as shown in Table 2. The room temperature tensile strength of the FGH4097 high temperature alloy sealing disk obtained meets the preset target value and the corresponding optimized characteristic cooling rate value range is -0.73 to -1.62℃ / s.
[0106] Table 2 Characteristic cooling rate values of products 1 to 3
[0107]
[0108] and Figure 6 Compared with Table 1, it can be seen that for the "two-in-one" method, the cooling rate is too fast, and for the "six-in-one plus core" method, the cooling rate is too slow. The characteristic cooling rate values of these two methods (the judgment method here is: among the cooling rate test points selected from different parts of each package structure, the characteristic cooling rate values of more than 80% of the test points need to be within the optimized characteristic cooling rate value range) are not within the optimized characteristic cooling rate value range. The cooling rate of the center part of the "six-in-one" method is slower, close to the lower limit of the characteristic cooling rate range, and the cooling rate of the "three-in-one" method is within the characteristic cooling rate range, but the characteristic cooling rate is biased towards the upper limit. The "six-in-one" method is preferred, that is, the ring blank is a superposition of 6 ring parts before machining in the axial direction.
[0109] Select other qualified products of different specifications made by the same alloy grade FGH4097 alloy and the same preparation process, such as product 4, whose package structure and size are similar to the "six-in-one" laminate. Specifically, the size of product 4 can be: outer diameter 345-355mm, inner diameter 230-235mm, height 375-387mm, but not limited to this. Perform heat treatment cooling rate simulation on product 4 to obtain different parts of product 4 (9 test points, the position of the test points is referenced Figure 2) The characteristic cooling rate value during the cooling process of the solution treatment. Table 3 shows the characteristic cooling rate values of different test points of product 4. According to the test results of Table 3, the second optimized characteristic cooling rate value range is -0.87~-2.78℃ / s. The purpose is to control the cooling rate of the sealing disk and other annular parts after solution heat treatment, and to further ensure the performance batch stability of different parts of the annular parts and the lack of 750℃ composite permanent notch sensitivity, etc., under the premise of meeting the technical indicators of the mechanical properties of the annular parts.
[0110] Table 3 Characteristic cooling rate values of product 4
[0111]
[0112] On the basis of choosing the "six-in-one" method, Figure 2 The Deform software is used to perform numerical simulation of S1 and S2 under the corresponding machining processing mode. Figure 2 The test points of the ring blank are selected as shown, and the relationship between temperature and time of each test point during the cooling process of the solution heat treatment is obtained as shown in the figure Figure 8 As shown. The slope of each point on the curve obtained from the temperature and time relationship diagram is the cooling rate. Then draw a curve with the cooling rate as the ordinate and the temperature as the abscissa. The value of the ordinate corresponding to the highest point of the curve is the characteristic cooling rate. Figure 2 The test points of the ring blank are selected as shown in the figure, and the relationship between the cooling rate and the temperature of each test point during the cooling process of the solution heat treatment is obtained as shown in the figure Fig. 9 And as shown in Table 4.
[0113] Table 4 Characteristic cooling rate values of different parts of the ring parts heat treated by the jacket without endothelial
[0114]
[0115] Will Fig. 9 Compared with the second optimized characteristic cooling rate range in Table 4, the influence of cooling rate on the performance of the ring (notch sensitivity and hardness) is comprehensively considered, and the final ring is selected Figure 2 The third type is the machining method of removing the sleeve at the center hole of the annular sleeve by machining (i.e. the sleeve has no inner skin).
[0116] Furthermore, for FGH4097 high-temperature alloy ring parts, MSC.MARC software combined with CAD drawing software is used to calculate the shrinkage deformation of the sleeve during hot isostatic pressing through numerical simulation software to obtain the sleeve size. In a specific embodiment of the present invention, in the annular sleeve structure, the outer diameter of the sleeve is 1.07×D~1.1×D, the inner diameter of the sleeve is 0.95×d~0.98×d, and the height of the sleeve is 1.29×H×X~1.34×H×X. It should be noted that the outer diameter, inner diameter and height dimensions of the sleeve in the present invention all refer to the internal dimensions of the sleeve, excluding the thickness of the sleeve itself, and the thickness of the sleeve is 5~10mm; wherein D, d, and H are the outer diameter, inner diameter and height of the finished ring part, respectively. Furthermore, the material of the annular sleeve structure is low carbon steel or stainless steel.
[0117] Based on this, another aspect of the present invention provides a method for preparing a powder high-temperature alloy ring, comprising the following steps:
[0118] (a) High-temperature alloy powder is loaded into an annular casing structure and subjected to hot isostatic pressing to obtain a ring blank;
[0119] (b) subjecting the ring blank to solution treatment and aging treatment, and then machining to obtain a finished ring part;
[0120] The ring blank is a superposition of X ring parts before machining in the axial direction, where X is an integer between 4 and 8; the center hole of the ring sleeve is vacant;
[0121] Before solution treatment, the ring blank is machined to remove the annular sleeve at the center hole.
[0122] In a specific embodiment of the present invention, the high temperature alloy powder includes at least one of FGH4091, FGH4095, FGH4096, FGH4097, FGH4098 and FGH4099.
[0123] In a specific embodiment of the present invention, in the annular sleeve structure, the sleeve outer diameter is 1.07×D~1.1×D, the sleeve inner diameter is 0.95×d~0.98×d, the sleeve height is 1.29×H×X~1.34×H×X, and the sleeve thickness is 5~10mm; wherein D, d, and H are the outer diameter, inner diameter, and height of the finished annular part, respectively. Further, the material of the annular sleeve structure is low carbon steel or stainless steel.
[0124] In a specific embodiment of the present invention, during the hot isostatic pressing treatment, the temperature is 1160-1210° C., the pressure is ≥120 MPa, the heat preservation and pressure holding time is ≥2 hours, and after the heat preservation and pressure holding, the furnace is cooled.
[0125] In a specific embodiment of the present invention, the solution treatment comprises: heat preservation treatment at 1110-1210° C. for 1-8 hours, followed by air cooling, salt quenching or oil quenching.
[0126] In a specific embodiment of the present invention, the aging system can be selected as primary aging, secondary aging or tertiary aging according to needs. For example, the aging treatment may include: heat preservation treatment at 850-920°C for 1-4 hours, followed by air cooling; heat preservation treatment at 700-760°C for 1-9 hours, followed by air cooling; heat preservation treatment at 640-710°C for 1-18 hours, followed by air cooling.
[0127] In a specific embodiment of the present invention, in step (b), machining includes: removing the upper and lower end surfaces of the annular sleeve and the outer cylindrical sleeve, and then machining and cutting according to the size of the delivered annular part.
[0128] The ring-shaped parts prepared by the preparation method of the present invention were subjected to ultrasonic nondestructive testing. The sound velocity of the ring-shaped parts was normal, and no single display signal exceeding the standard and abnormal bottom wave loss of the flat bottom hole with a diameter of 0.8 mm were found. Secondly, there were no defects such as microscopic holes and cracks visible to the naked eye on the surface of the ring-shaped parts, no coarse grains were found in the visual inspection, and the size and appearance inspection results of the ring-shaped parts met the design requirements.
[0129] The ring parts prepared by the present invention have better comprehensive performance than those manufactured by the traditional vacuum melting + forging deformation process and the hot isostatic pressing + rolling process. The present invention also solves the problems of low 650°C tensile yield strength margin and easy fracture of 750°C composite durability of the ring parts.
[0130] In addition, the greater advantages of the present invention are short process, low cost and high material utilization rate. Analyzing from the actual economic benefits created by the product, according to the weight of each ring blank delivered in the state of 10 to 13 kg, the market price of each ring blank is about 50,000 yuan, and the traditional vacuum melting + forging deformation process is used to manufacture the ring, and each 200 kg master alloy material is thrown, and about 3 to 5 qualified rings are produced. However, the powder high-temperature alloy ring prepared by the present invention produces 6 qualified rings for each 78 to 82 kg master alloy material, and the product qualification rate is 100%. According to the same master alloy material, the number of powder high-temperature alloy rings prepared by the present invention is about 3 to 5 times that of the traditional vacuum melting + forging deformation process. The main preparation processes used in the present invention, such as the vacuum horizontal continuous casting (VHCC) master alloy bar preparation process, the plasma rotating electrode atomization powder making process, the hot isostatic pressing process, etc., can achieve the goals of process controllability, reliable quality and cost reduction, and can meet the batch production needs of more types of rings for aircraft engines.
[0131] Example 1
[0132] This embodiment provides a method for preparing a FGH4097 powder high temperature alloy ring (with dimensions of inner ring diameter 260-300 mm, outer ring diameter 370-410 mm, and ring height 20-25 mm), comprising the following steps:
[0133] (1) FGH4097 master alloy rods were prepared by vacuum horizontal continuous casting (VHCC) technology, and then powdered by plasma rotating electrode method (PREP) to obtain FGH4097 powder with a powder size range of 50-150 μm and a particle size D50 of 80-90 μm in laser particle size distribution.
[0134] (2) The FGH4097 powder is loaded into a "six-in-one" annular structure package, and then the package is degassed, sealed and hot isostatically pressed, and then cooled with the furnace; wherein the hot isostatic pressing temperature is 1200±10℃, the pressure is ≥120MPa, the heat preservation and pressure holding time is 4h, and after heat preservation and pressure holding, it is cooled with the furnace. Among them, in the annular package structure, the outer diameter of the package is 436~446mm, the inner diameter of the package is 275~285mm, the height of the package is 178~185mm, and the thickness of the package is 5~10mm; wherein D, d, and H are the outer diameter, inner diameter, and height of the finished annular part, respectively. The material of the annular package structure is low carbon steel or stainless steel.
[0135] (3) Machining the ring blank obtained in step (2) to remove the sheath at the center hole. Then, solid solution treatment and three-stage aging treatment are performed; solid solution treatment includes: heat preservation treatment at 1110-1210℃ for 1-8h, air cooling or salt quenching or oil quenching; aging treatment includes: heat preservation treatment at 850-920℃ for 1-4h, air cooling; heat preservation treatment at 700-760℃ for 1-9h, air cooling; heat preservation treatment at 640-710℃ for 1-18h, air cooling. The aging system can be selected from primary aging, secondary aging or tertiary aging according to needs.
[0136] (4) The ring blank after heat treatment in step (3) is machined to remove the upper and lower end surfaces of the ring and the outer cylindrical sheath, and 6 rings are cut according to the dimensions of the delivery drawing.
[0137] Comparative Example 1
[0138] A GH4079 alloy ring (taking a sealing disk as an example) with the same specifications as in Example 1 but different composition is manufactured using a conventional vacuum melting + forging deformation process.
[0139] Experimental Example 1
[0140] Fig.10 and Fig.11 The alloy grain structures of the ring parts prepared in Example 1 of the present invention and Comparative Example 1 are shown respectively. Fig.10The grain structure of the FGH4097 alloy ring sampled after corrosion of the present invention shows that no obvious original grain boundary is found, the grain structure is relatively uniform, the average grain size is 39.84μm, and the grain size is 6.0-6.5. Fig.11 It can be seen that the grain structure of the alloy of Comparative Example 1 is coarser than that of Example 1, with an average grain size of 60.65 μm, a grain size of 4.5 to 5.0, and some irregular larger-sized carbides on the grain boundaries.
[0141] Fig.12 and Fig.13 The precipitation phase structures of the ring parts obtained in Example 1 and Comparative Example 1 of the present invention are the γ' precipitation phase structures obtained after electrolytic polishing and electrolytic corrosion of the samples taken from the respective ring parts. As can be seen from the figure, the primary γ' phase of the ring part of Example 1 is less residual and mainly distributed in the grain boundary in the form of irregular long strips, with an average size of about 1.30μm; the secondary γ' phase is more precipitated, mainly distributed in the crystal in the form of cubes, with an average size of about 0.48μm; the tertiary γ' phase is mainly in the form of small spheres and mainly distributed around the primary γ' phase and the secondary γ' phase, with an average size of about ≤70nm. The primary γ' phase of the ring part of Comparative Example 1 is almost completely dissolved, and the remaining ones are mainly in the form of small irregular long strips, with an average size of about 0.87μm; the secondary γ' phase is more precipitated, mainly distributed in the crystal in the form of spheres, with an average size of about 0.14μm; the tertiary γ' phase is in the form of small spheres, with an average size of about ≤50nm.
[0142] Experimental Example 2
[0143] The mechanical properties of the ring members of Example 1 and Comparative Example 1 of the present invention were tested, and the test results are shown in Tables 5 to 9. The numbers 1 to 3 of Example 1 correspond to the sample numbers of the first three ring members of the "six-in-one" sheath structure cut from top to bottom; the numbers 1 to 2 of Comparative Example 1 correspond to the sample numbers of the two selected comparative example ring members.
[0144] Table 5 Room temperature tensile properties
[0145]
[0146] Table 6 High temperature tensile properties at 650℃ and 750℃
[0147]
[0148] Table 7 Composite endurance properties of ring parts at 650℃ and 750℃
[0149]
[0150] Table 8 Impact energy and Brinell hardness at room temperature
[0151]
[0152] Table 9 650℃ low cycle fatigue
[0153]
[0154] From the above test results, it can be seen that the FGH4097 ring alloy prepared by the method of the present invention has fine and uniform grain structure, and has excellent room temperature tensile, high temperature tensile, high temperature endurance, room temperature impact, hardness and low cycle fatigue properties.
[0155] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a powder high temperature alloy ring, characterized in that: The steps include: S1. The high temperature alloy powder is loaded into the annular casing structure and hot isostatic pressing is performed to obtain a ring blank; S2. The ring blank is subjected to solution treatment and aging treatment, and then machined to obtain the finished ring part; The ring blank is a superposition of X ring parts before machining in the axial direction, where X is selected from an integer ≥ 1; the center hole of the annular sleeve is vacant or has an iron core in the gap; The assembly method is adjusted so that the characteristic cooling rate value of the ring blank during the cooling process of the solution treatment is within the optimized characteristic cooling rate value range; the assembly method includes: the selection of X and the setting method of the center hole of the annular sleeve; The acquisition of the characteristic cooling rate value includes: using Deform software to perform numerical simulation of S1 and S2 in a corresponding assembly mode, selecting at least one part of the ring blank as a test point, obtaining the cooling rate of the test point at different temperatures during the furnace cooling process of the solution treatment, and drawing a curve with the cooling rate as the ordinate and the temperature as the abscissa. The value of the ordinate corresponding to the highest point of the curve is the characteristic cooling rate value; The acquisition of the optimized characteristic cooling rate value range includes: selecting at least one parameter from the tensile strength and yield strength of the ring part, and determining a preset target value; establishing a functional relationship between the selected parameter and the characteristic cooling rate value, and acquiring the optimized characteristic cooling rate value range that makes the selected parameter meet the preset target value according to the functional relationship.
2. The method for preparing a powder high temperature alloy ring according to claim 1, characterized in that: A plurality of test points are arranged in the ring blank according to the value of X and the radial dimension of the ring blank.
3. The method for preparing a powder high temperature alloy ring according to claim 1, characterized in that: In obtaining the characteristic cooling rate value, at least two or more test points are selected to respectively calculate the characteristic cooling rate values; and the assembly method is adjusted so that the characteristic cooling rate values of more than 80% of the test points are within the optimized characteristic cooling rate value range.
4. The method for preparing a powder high temperature alloy ring according to claim 1, characterized in that: Also includes: The machining treatment method of the annular sleeve before the solution treatment; the machining treatment method of the annular sleeve before the solution treatment includes any one of the following methods: (1) Do not remove the cover; (2) Machining to remove all covers; (3) Machining to remove the sleeve at the center hole of the annular sleeve; (4) Machining to remove the center hole of the annular sleeve and the sleeves on the upper and lower end surfaces.
5. The method for preparing a powder high temperature alloy ring according to claim 4, characterized in that: Adjust the machining treatment method so that the characteristic cooling rate value of the ring blank during the cooling process of the solution treatment is within the second optimized characteristic cooling rate value range or partially lower than the second optimized characteristic cooling rate range; The acquisition of the second optimized characteristic cooling rate value range includes: selecting an existing ring-shaped product of the same type as the ring-shaped alloy, simulating the ring-shaped product according to the actual preparation process, selecting at least 3 test points in the ring-shaped product, and obtaining the characteristic cooling rate values of each test point during the solution treatment, so that the maximum value and the minimum value of the obtained characteristic cooling rate values of the ring-shaped product constitute the second optimized characteristic cooling rate range.
6. The method for preparing a powder high temperature alloy ring according to claim 5, characterized in that: When adjusting the machining treatment method, the characteristic cooling rate values of more than 80% of the test points of the ring blank are within the second optimized characteristic cooling rate value range.
7. The method for preparing a powder high temperature alloy ring according to claim 1, characterized in that: The preparation of the high temperature alloy powder comprises: preparing a master alloy rod by vacuum horizontal continuous casting technology, then preparing powder by plasma rotating electrode method, and screening and selecting powder with a particle size range of 50 to 150 μm; The annular member includes any one of a sealing disk, a baffle ring, a front baffle plate and a rear baffle plate.
8. The method for preparing a powder high temperature alloy ring according to claim 1, characterized in that: The ring blank is a superposition of X ring parts before machining in the axial direction, where X is an integer between 4 and 8; the center hole of the ring sleeve is vacant; Before the solution treatment, the ring blank is machined to remove the sheath at the center hole of the annular sheath; The high temperature alloy powder includes at least one of FGH4091, FGH4095, FGH4096, FGH4097, FGH4098 and FGH4099.
9. The method for preparing a powder high temperature alloy ring according to claim 8, characterized in that: In the annular sheath structure, the outer diameter of the sheath is 1.07×D to 1.1×D, the inner diameter of the sheath is 0.95×d to 0.98×d, the height of the sheath is 1.29×H×X to 1.34×H×X, and the thickness of the sheath is 5 to 10 mm; wherein D, d, and H are respectively the outer diameter, inner diameter, and height of the finished annular component, and X is the number of corresponding annular components in the stacked body; The material of the annular sleeve structure is low carbon steel or stainless steel.