A precision welding method for connecting multiple wires with micro-fine wires
By adopting funnel-shaped vias and extruded cavity surface technology in avionics systems, the stable connection between multiple strands of wires and micro filaments is achieved, solving the problem of insufficient edge bias and vibration fatigue performance of welding joints, and improving the welding joints Strength and stability, and precise control of joint diameter.
Patent Information
- Application Number
- CN202411059562.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-04
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-04
AI Technical Summary
The precision welding of micro filaments and multi-strand conductors in avionics systems has problems with insufficient edge bias, connection strength and vibration fatigue performance of welded joints, and it is difficult to accurately control the diameter of welded joints.
A precision welding method for connecting multi-stranded wires is adopted. By putting the segment to be welded of the multi-stranded wires into the funnel-shaped via of the graphite block, the micro-stranded wires are vertically inserted into the segment to be welded and placed in the graphite block. When heating on and on, powdered solder is added, and a specific shuttle structure is formed by using the extruded cavity surface of the inner wall of the via hole to achieve a stable connection between the multi-stranded wires and the fine wires.
The problem of micro-wire biasing toward the edge of the welded joint is solved, the connection strength and vibration fatigue performance of the welded joint are improved, and the diameter of the welded joint is easy to control, forming a stable "catch" structure to enhance the connection strength and stability.
Smart Images

Figure CN118720308B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of micro-connection of components of an avionics system, and in particular relates to a precision welding method for connecting multiple strands of wires with micro-filaments. Background Art
[0002] The sensor components in avionics systems involve welding connections of fine wires to multiple strands of wire (multiple strands usually refers to the number of strands being no less than fifteen). This is classified as a micro connection, which places very high demands on the welding quality of the joints, and the main connection method is resistance brazing.
[0003] In order to solve the problem of incomplete filling and poor performance of conventional resistance brazing joints, a precision resistance brazing method for multi-strand wires and micro-wires was developed in the early stage (Document 201710851557X). The multi-strand wires are placed on the brazing material, and the grooved graphite block is energized to melt the brazing material and infiltrate the gaps between the multi-strand wires to achieve connection between each wire. Then the micro-wire is placed on the brazing material, and the multi-strand wires infiltrated with the brazing material are placed on the micro-wire. The welding signal is input, and the brazing material melts to achieve brazing connection between the multi-strand wires and the micro-wire. The essence of this scheme is to connect the multi-strand wire with the first brazing material, and the micro-wire with the second brazing material respectively, and then connect the two together. However, this scheme still has some disadvantages, especially the micro-wire is seriously biased towards the edge of the welding joint (micro-connection joint), the connection strength and vibration fatigue performance of the welding joint need to be further optimized, and it is not convenient to accurately control the diameter of the welding joint within the allowable range. Summary of the invention
[0004] At least with respect to the technical problems mentioned in the background technology, the present invention aims to provide a precision welding method for connecting multiple wires with micro-filaments, which ingeniously solves the problem that the micro-filaments are seriously biased toward the edge of the welding joint.
[0005] The present invention adopts the following technical solution.
[0006] A precision welding method for connecting multiple strands of wires with micro-filaments, comprising the following steps:
[0007] Step 1, placing the second segment to be welded of the multi-strand wire into the via hole of the graphite block, with the upper end of the second segment to be welded facing upward; wherein the via hole is a funnel-shaped structure with a thick top and a thin bottom, and the second segment to be welded is a divergent structure adapted to the via hole;
[0008] Step 2, insert the first segment to be welded of the micro-wire vertically downward into the middle of the second segment to be welded, and maintain this posture;
[0009] Step 3, adding powdered solder and flux into the via hole;
[0010] Step 4, heating the graphite block by means of a welding power source, so that the solder in the via hole melts and fills the gap, and after cooling, the multi-strand wires are connected by soldering to the micro-filaments.
[0011] As a preferred embodiment, the aperture of the positioning hole below the via is not larger than the minimum diameter of the via, and the limit position of the downward flow of liquid solder is the junction between the second segment to be welded and the insulation layer of the multi-strand wire (i.e. the lower end of the insulation layer peeling area, i.e. the exposed root position of the wire).
[0012] As a preferred solution, the graphite block is formed by splicing two graphite pieces, one of which is connected to the positive pole of the power supply, and the other is connected to the negative pole of the power supply.
[0013] As a preferred solution, the upper end of the positioning hole is located at the junction of the insulating layer.
[0014] Furthermore, the positioning hole is a through hole provided on the insulating support block, and a cooling water flow channel is provided on the insulating support block. With such a solution, the end position of the connecting joint can be accurately controlled.
[0015] As a preferred solution, when the diameter of the fine wire is 0.2-0.5 mm, the maximum diameter of the second segment to be welded in step 1 is 5 mm (ie, the maximum diameter of the divergent structure is 5 mm), and the maximum diameter of the connection joint after welding is 1 mm.
[0016] In order to facilitate the precise control of the welding joint diameter within the allowable range, during the process of electrically heating the graphite block, the second segment to be welded of the multi-strand wire and the first segment to be welded of the micro-wire are controlled to move downward synchronously to achieve the contraction of the second segment to be welded and control the maximum diameter of the connecting joint within 2 mm.
[0017] As a preferred solution, the segment of the micro-wire to be welded is in a spiral, columnar or flat shape.
[0018] As a preferred solution, the speed at which the second segment to be welded and the micro-wire move downward synchronously is controlled to be 1~2mm / s.
[0019] Beneficial effect: The solution of the present invention not only cleverly solves the problem of the micro-wire seriously deviating to the edge of the welding joint, but also solves the problem that the wires of the multi-strand conductors are prone to bunching and cold welding defects, and realizes the stable connection of the first segment of the micro-wire to be welded in the middle area of the second welding segment, which greatly improves the connection strength and vibration fatigue performance of the welding joint, and facilitates the precise control of the diameter of the welding joint within the allowable range; in the welding joint formed by the solution of the present invention, the wires of the multi-strand conductor cover the micro-wire in a "grasping" manner, and cooperate with the solder filling part to form a specific shuttle structure, which effectively ensures the stability and connection strength of the welding joint. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Schematic diagram of the second segment to be welded of the multi-strand wire in Example 1 (divergent structure);
[0021] Figure 2 This is a schematic diagram of the state of the micro-filament connected to the multi-strand wire before welding in Example 1;
[0022] Figure 3 This is a schematic diagram of the state of the micro-filament connected to multiple strands of wires after welding in Example 1. DETAILED DESCRIPTION
[0023] The technical solution of the present invention is described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1
[0024] A precision welding method for connecting a plurality of wires with a micro-fine wire is used to connect a nickel wire and a silver wire, wherein the overall diameter of the nickel wire is about 0.6 mm, the diameter of a single wire is about 20 μm, the diameter of the silver wire is about 0.1 mm, and the segment 11 to be welded of the micro-fine wire is columnar, and the steps include:
[0025] Pre-welding pretreatment: The end segments of the multi-strand wires are stripped to expose the single strands of the multi-strand wires, thereby obtaining the second segment 12 to be welded (the area where the wires are exposed), and then the second segment 12 to be welded is spread out to form a Figure 1 The divergent structure shown; then the multi-strand wire segment 12 to be welded and the micro-wire segment 11 to be welded are chemically cleaned and dried for standby use; the chemical cleaning process of the pre-treatment is prior art and will not be described in detail here;
[0026] The graphite block 1 used in this embodiment is formed by splicing two graphite pieces, one of which is connected to the positive pole of the power supply, and the other is connected to the negative pole of the power supply, and the lower end of the graphite piece is close to the insulating support block 7; wherein, the positioning hole 5 is a through hole arranged on the insulating support block, and a cooling water flow channel 8 is arranged on the insulating support block 7, and the cooling water flow channel 8 is externally connected to the circulating water system; the via hole 3 is a funnel-shaped structure with a thick top and a thin bottom, and the radial cross section of the via hole 3 is circular, and the aperture of the positioning hole 5 below the via hole 3 is not greater than the minimum diameter of the via hole 3; without considering the error, the aperture of the positioning hole 5 in this example is equal to the minimum diameter of the via hole 3 and equal to the outer diameter of the insulation layer of the multi-strand conductor 4;
[0027] Step 1, place the second segment 12 to be welded of the multi-strand wire 4 into the through hole 3 of the graphite block 1, with the upper end of the second segment 12 to be welded facing upward, and fix the graphite block 1 to prevent the size of the through hole 3 from changing; wherein the second segment 12 to be welded is a divergent structure adapted to the through hole 3, and the state at this time is as follows Figure 2 As shown; the second section 12 to be welded where the multi-strand wire 4 is placed should meet the requirement that the upper end of the positioning hole 5 is located at the junction of the insulation layer (i.e., the lower end of the insulation layer peeling area, i.e., the exposed wire root), so that the limit position of the liquid solder flowing downward can be the junction of the insulation layer, thereby facilitating the precise control of the end position of the connection joint;
[0028] Step 2, keep the second segment 12 to be welded of the multi-strand wire 4 fixed (mainly to prevent the second segment 12 to be welded from moving downward in this step), insert the first segment 11 to be welded of the micro-wire vertically downward into the middle of the second segment 12 to be welded, and maintain this posture. The state at this time is as follows Figure 2 As shown;
[0029] Step 3, add powdered solder and flux into the via 3, the state at this time is as follows Figure 2 As shown, the figure number 9 represents the added powdered solder and flux, and the added solder and flux will fill some gaps in the via hole 3;
[0030] Step 4, the graphite block is electrically heated by a welding power source, so that the solder in the via hole 3 melts and fills the gap, and after cooling, the multi-strand wire and the micro-filament are brazed and connected, and the obtained connection joint 10 is as shown in FIG. Figure 3 As shown (the actual upper end of the connecting joint 10 is not pointed, but is shaped like an elliptical head, but is generally similar to a shuttle body);
[0031] In this step, during the process of heating the graphite block 1 by electricity, the second segment 12 to be welded of the multi-strand wire 4 and the first segment 11 to be welded of the fine wire are controlled to move downward synchronously (specifically, the multi-strand wire 4 can be pulled down and the second segment 12 to be welded of the fine wire can be moved downward at the same time) to achieve the folding of the second segment 12 to be welded and control the maximum diameter of the connection joint within 2 mm. The force applied to the second segment 12 to be welded during the folding process is as follows: Figure 3 As shown by the middle arrow, the molten solder can be squeezed to adhere to the segment 1 to be welded 11 and fully immersed in the gap of the segment 2 to be welded 12 itself; wherein, the speed of the synchronous downward movement of the segment 2 to be welded 12 and the micro-wire is controlled to be 1mm / s.
[0032] In this embodiment, the via hole of a specific shape, the second segment to be welded 12 and each step are very critical. A mode that is essentially different from the traditional resistance brazing "positive and negative electrodes press down the segment to be welded" is adopted. During the power-on heating process, the segment to be welded is used to actively extrude the cavity surface (the inner wall of the via hole 3) to shape the connection joint. In this process, the molten solder is squeezed into the wire gaps of the multi-strand conductor itself for filling, and on the other hand, it moves up relative to the micro-filament and adheres to the micro-filament, thereby forming a specific shuttle structure. Due to the use of the divergent structure of the second segment to be welded 12, the first segment to be welded 11 of the micro-filament can be smoothly and quickly aligned with the center of the second segment to be welded 12 and inserted axially, so that the wire of the second segment to be welded 12 is surrounded by the periphery of the first segment to be welded 11. As the solder is filled and formed, the wire of the multi-strand conductor is finally covered with the micro-filament in a "grasping" manner. Example 2
[0033] A precision welding method for connecting multiple strands of wires with a micro-wire, referring to Example 1, which differs from Example 1 in that: a segment 11 to be welded of the micro-wire is spiral-shaped; when the diameter of the micro-wire is 0.2-0.5 mm, the maximum diameter of the segment 2 12 to be welded in step 1 is 5 mm, and the maximum diameter of the connection joint after welding is controlled to be 1 mm.
[0034] The scheme in the embodiment not only cleverly solves the problem of the micro-wire seriously deviating to the edge of the welding joint, but also solves the problem of the wires of the multi-strand conductor being prone to bunching and cold welding defects, and achieves the stable connection of the first segment of the micro-wire to be welded in the middle area of the second welding segment, greatly improving the connection strength and vibration fatigue performance of the welding joint (compared with the connection joint implemented by the existing precision resistance brazing method of multi-strand conductors and micro-wires), and also facilitates the precise control of the welding joint diameter within the allowable range; in the welding joint formed by adopting this scheme, the wires of the multi-strand conductor cover the micro-wire in a "grasping" manner, and cooperate with the solder filling part to form a specific shuttle structure, which effectively ensures the stability and connection strength of the welding joint.
Claims
1. A precision welding method for connecting multiple wires with micro-filaments, characterized in that the steps include: Step 1, placing the second segment (12) to be welded of the multi-strand wire (4) into the through hole (3) of the graphite block (1), with the upper end of the second segment (12) to be welded facing upward; wherein the through hole (3) is a funnel-shaped structure that is thick at the top and thin at the bottom, and the second segment (12) to be welded is a divergent structure that is adapted to the through hole (3); Step 2, insert the first segment to be welded (11) of the micro-wire vertically downward into the middle of the second segment to be welded (12), and maintain this posture; Step 3, adding powdered solder and flux into the via hole (3); Step 4, heating the graphite block (1) by applying electricity through a welding power supply, so that the solder in the via hole (3) melts and fills the gap, and after cooling, the multi-strand wire and the micro-filament are brazed together; The aperture of the positioning hole (5) below the through hole (3) is not larger than the minimum diameter of the through hole (3); the limit position of the downward flow of the liquid solder is the junction position of the insulating layer of the second segment to be welded (12) and the multi-strand conductor (4); the upper end of the positioning hole (5) is located at the junction position of the insulating layer; the graphite block (1) is formed by splicing two graphite pieces, one of which is connected to the positive pole of the power supply and the other is connected to the negative pole of the power supply; the positioning hole (5) is a through hole provided on the insulating support block (7), and a cooling water flow channel (8) is provided on the insulating support block (7); When the diameter of the micro-filament is 0.2-0.5 mm, the maximum diameter of the second segment to be welded (12) in step 1 is 5 mm, and the maximum diameter of the connection joint after welding is 1 mm; During the process of heating the graphite block with electricity, the second segment to be welded (12) of the multi-strand wire (4) and the first segment to be welded (11) of the micro-wire are controlled to move downward synchronously to achieve the retraction of the second segment to be welded (12). The speed of the synchronous downward movement of the second segment to be welded (12) and the micro-wire is controlled to be 1~2mm / s.
2. The precision welding method for connecting multiple wires with micro-filaments according to claim 1, characterized in that: The segment to be welded (11) of the micro-wire is in the shape of a spiral or a column.