Narrow-gap GTAW rotating electric arc welding process for thick plate high-strength steel
By adopting multi-layer single-pass GTAW rotating arc welding process in narrow gap welding of high-strength steel thick plates, using high-purity argon gas and changing the welding arc rotation direction layer by layer, the problem of unfused side walls is solved, and the welding efficiency and quality, ensuring the high performance of welded joints.
Patent Information
- Application Number
- CN202411023070.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-01
AI Technical Summary
High-strength steel is prone to sidewall unfusion defects during narrow-gap welding of thick plates, resulting in low welding efficiency.
The multi-layer single-pass GTAW rotating arc welding process is adopted. By presetting anti-deformation and using high-purity argon gas for bottoming, filling and cover welding, the welding arc rotation direction is changed layer by layer, and the inter-layer temperature is controlled to ensure the quality of the weld. Fusion evenly.
It effectively solves the problem of unfused side walls of narrow gap welding of thick plates, improves welding efficiency, and ensures efficient welding quality of high-strength steel thick plates. The mechanical properties of the welded joints are close to those of the base material.
Smart Images

Figure CN118720345A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a narrow gap GTAW rotary arc welding process for thick plate high-strength steel, belonging to the technical field of welding processes. Background Art
[0002] High-strength steel has the advantages of high strength and good comprehensive mechanical properties. High-strength steel components are widely used in marine engineering and shipbuilding industries. With the development of the national marine and shipbuilding industries, further requirements have been put forward for the efficient and stable production of high-strength steel welded components.
[0003] TIG has the advantages of low equipment cost, stable welding, high weld quality, and easy automated welding. TIG welding of high-strength steel is most widely used. Since high-strength steel is a material that is easily magnetized, a multi-layer and multi-pass welding process is usually adopted. Due to the influence of magnetism, it is easy to have the defect of unfused side walls of thick plate narrow gap welding. For this reason, the present invention is proposed. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a narrow gap GTAW rotary arc welding process for thick plate high-strength steel, which realizes a multi-layer single-pass welding process, effectively solves the defect of unfused side walls of narrow gap welding of thick plates, and greatly improves welding efficiency.
[0005] The technical solution of the present invention is as follows:
[0006] A narrow gap GTAW rotary arc welding process for thick plate high-strength steel, the steps are as follows:
[0007] S1: Beveling of workpiece;
[0008] S2: Remove oil and oxide scale from the workpiece surface before welding;
[0009] S3: preset anti-deformation;
[0010] S4: welding gun centering, weld tracking zero calibration;
[0011] S5: Tongbei protection gas;
[0012] S6: Use high-purity argon for base coating and set welding parameters;
[0013] S7: Change the rotation direction of the welding arc;
[0014] S8: Use high-purity argon for filling and set welding parameters;
[0015] S9: Use high-purity argon for capping and set welding parameters.
[0016] Preferably, according to the present invention, in step S3, a reverse deformation of 3 to 6° is prefabricated on a workbench.
[0017] Preferably, according to the present invention, in step S5, the gas introduced is pure argon, the purity of the argon is ≥99.99%, and the back protection gas flow rate is 5-15 L / min.
[0018] According to the preferred embodiment of the present invention, in step S6, the welding parameters are: high-strength steel Welding wire, welding current 200 ~ 300A, welding speed 0.5 ~ 5mm / min, wire feeding speed 0 ~ 10mm / s, welding arc rotation direction is clockwise, rotation speed 0 ~ 500r / min, control interlayer temperature, cooling after welding, the interlayer temperature does not exceed 120 ℃.
[0019] Preferably, according to the present invention, in step S7, the rotation direction of the rotating arc is changed to counterclockwise.
[0020] According to the preferred embodiment of the present invention, in step S8, the welding parameters are: high-strength steel is selected Welding wire, welding current 200 ~ 300A, welding speed 0.5 ~ 5mm / min, wire feeding speed 0 ~ 25mm / s, rotation speed 0 ~ 500r / min, control the interlayer temperature, cooling after welding, the interlayer temperature does not exceed 120℃, and change the rotation direction of the welding arc layer by layer.
[0021] Preferably, according to the present invention, in step S8, the filling is stopped when the weld height is 1 to 3 mm lower than the base material thickness.
[0022] According to the preferred embodiment of the present invention, in step S9, the welding parameters are: high-strength steel is selected Welding wire, welding current 200 ~ 300A, welding speed 0.5 ~ 5mm / min, wire feeding speed 0 ~ 30mm / s, change the rotation direction of the welding arc, rotation speed 0 ~ 500r / min.
[0023] The beneficial effects of the present invention are:
[0024] The present invention provides a thick plate high-strength steel narrow gap GTAW rotary arc welding process, which realizes a multi-layer single-pass welding process, effectively solves the defect of unfused side walls of thick plate narrow gap welding, greatly improves welding efficiency, and ensures efficient welding of high-strength steel thick plates. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a front view schematic diagram of the welding arc rotation and swing of the present invention;
[0026] Figure 2 It is a top view schematic diagram of the welding arc rotation and swing of the present invention;
[0027] Figure 3 A schematic diagram of welding penetration of the present invention;
[0028] Figure 4 This is a macroscopic morphology diagram of the filler layer weld of an embodiment of the present invention;
[0029] Figure 5 This is a front macroscopic morphology diagram of a weld according to an embodiment of the present invention;
[0030] Figure 6 This is a macroscopic morphology of the back side of the weld according to an embodiment of the present invention;
[0031] Figure 7 A macroscopic metallographic image of a weld cross section according to an embodiment of the present invention;
[0032] Figure 8 A comparison diagram of a welded joint before and after stretching according to an embodiment of the present invention;
[0033] Fig. 9 This is a bar graph of the -50°C impact toughness of the weld delamination of an embodiment of the present invention. DETAILED DESCRIPTION
[0034] The present invention will be further described below by way of embodiments in conjunction with the accompanying drawings, but is not limited thereto.
[0035] Embodiment 1:
[0036] A narrow gap GTAW rotary arc welding process for thick plate high-strength steel, the steps are as follows:
[0037] S1: The workpiece is grooved, and the groove structure is as follows Figure 1 As shown, the groove form is a U-shaped groove, the blunt edge is 2mm, and the gap on the upper edge of the groove is 12mm;
[0038] S2: Remove oil and oxide scale from the workpiece surface before welding;
[0039] S3: Preset anti-deformation, prefabricate 3-6° anti-deformation on the workbench;
[0040] S4: welding gun centering, weld tracking zero calibration;
[0041] S5: back protection gas, the gas introduced is pure argon, the purity of argon is ≥99.99%, and the back protection gas flow rate is 5-15L / min;
[0042] S6: Use high-purity argon for base coating, set welding parameters, and select high-strength steel Welding wire, welding current 200 ~ 300A, welding speed 0.5 ~ 5mm / min, wire feeding speed 0 ~ 10mm / s, welding arc rotation direction is clockwise, rotation speed 0 ~ 500r / min, control interlayer temperature, post-weld cooling, interlayer temperature does not exceed 120℃;
[0043] S7: Change the rotation direction of the welding arc, the rotation direction of the rotating arc is changed to counterclockwise;
[0044] S8: Use high-purity argon for filling, set welding parameters, and select high-strength steel Welding wire, welding current 200-300A, welding speed 0.5-5mm / min, wire feeding speed 0-25mm / s, rotation speed 0-500r / min, control interlayer temperature, post-weld cooling, interlayer temperature not exceeding 120℃, change the rotation direction of the welding arc layer by layer, stop filling when the weld height is 1-3mm lower than the parent material thickness;
[0045] The rotation direction of the welding arc is divided into clockwise and counterclockwise. The side with the same welding direction as the tungsten electrode rotation direction is called the forward side, and the side with the opposite welding direction as the tungsten electrode rotation direction is called the backward side. The rotating arc will drive the molten pool to flow, and the molten pool will tend to the backward side. In order to make the weld biased evenly, the welding arc rotation direction needs to be changed after each welding. Figure 3 As shown, h b is the sidewall melting depth on the retreating side, h f H is the sidewall melting depth on the advancing side, b To deepen the bottom melt and make the weld uniform.
[0046] S9: Use high-purity argon for capping, set welding parameters, and select high-strength steel Welding wire, welding current 200 ~ 300A, welding speed 0.5 ~ 5mm / min, wire feeding speed 0 ~ 30mm / s, change the rotation direction of the welding arc, rotation speed 0 ~ 500r / min.
[0047] After narrow gap GTAW rotary arc welding of 47 mm thick high-strength steel using the above welding process, the filler layer weld is formed as follows: Figure 4 As shown, the weld is beautifully formed, without spatter or undercut defects, and the fish scale pattern is fine and uniform.
[0048] The weld seams on the front and back sides are metallic in color, beautifully formed, and free of undercut defects, such as Figure 5 and Figure 6 As shown in the figure, under the macroscopic microscope, there is no side wall non-fusion phenomenon in each layer, and the side wall fusion is good, such as Figure 7 As shown in the figure, the mechanical properties of the welded joint were tested. The average tensile strength of the base material was 893.13 MPa, and the average tensile strength of the welded joint was 895.25 MPa. The mechanical properties of the welded joint were close to those of the base material. The Charpy impact energy at -50℃ reached 276.34 J / cm 2 The tensile properties and -50℃ Charpy impact properties of the welded joints are as follows: Fig. 9 As shown, the impact energy of each layer is close and the strength of the welded joint is qualified.
[0049] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A narrow gap GTAW rotary arc welding process for thick plate high strength steel, characterized in that: Here are the steps: S1: Beveling of workpiece; S2: Remove oil and oxide scale from the workpiece surface before welding; S3: preset anti-deformation; S4: welding gun centering, weld tracking zero calibration; S5: Tongbei protection gas; S6: Use argon for primer and set welding parameters; S7: Change the rotation direction of the welding arc; S8: Use high-purity argon for filling and set welding parameters; S9: Use high-purity argon for capping and set welding parameters.
2. The thick plate high strength steel narrow gap GTAW rotary arc welding process as claimed in claim 1, characterized in that: In step S3, a reverse deformation of 3 to 6 degrees is prefabricated on a workbench.
3. The thick plate high strength steel narrow gap GTAW rotary arc welding process as claimed in claim 2, characterized in that: In step S5, the gas introduced is pure argon gas, the purity of argon gas is ≥99.99%, and the back protection gas flow rate is 5-15 L / min.
4. The thick plate high strength steel narrow gap GTAW rotary arc welding process as claimed in claim 3, characterized in that: In step S6, the welding parameters are: high-strength steel Welding wire, welding current 200 ~ 300A, welding speed 0.5 ~ 5mm / min, wire feeding speed 0 ~ 10mm / s, welding arc rotation direction is clockwise, rotation speed 0 ~ 500r / min, control interlayer temperature, cooling after welding, the interlayer temperature does not exceed 120 ℃.
5. The thick plate high strength steel narrow gap GTAW rotary arc welding process as claimed in claim 4, characterized in that: In step S7, the rotation direction of the rotating arc is changed to counterclockwise.
6. The thick plate high strength steel narrow gap GTAW rotary arc welding process as claimed in claim 5, characterized in that: In step S8, the welding parameters are: high-strength steel Welding wire, welding current 200 ~ 300A, welding speed 0.5 ~ 5mm / min, wire feeding speed 0 ~ 25mm / s, rotation speed 0 ~ 500r / min, control the interlayer temperature, cooling after welding, the interlayer temperature does not exceed 120℃, and change the rotation direction of the welding arc layer by layer.
7. The narrow gap GTAW rotary arc welding process for thick plate high strength steel as claimed in claim 6, characterized in that: In step S8, the filling is stopped when the weld height is 1 to 3 mm lower than the base material thickness.
8. The thick plate high strength steel narrow gap GTAW rotary arc welding process as claimed in claim 7, characterized in that: In step S9, the welding parameters are: high-strength steel Welding wire, welding current 200 ~ 300A, welding speed 0.5 ~ 5mm / min, wire feeding speed 0 ~ 30mm / s, change the rotation direction of the welding arc, rotation speed 0 ~ 500r / min.
Citation Information
Patent Citations
Moderate and high strength large-thickness component electromagnetic controlling narrow gap or ultra-narrow gap pulse efflux molten electrode gas-shield welding method and equipment
CN101143401A
Welding method for arc-rocking narrow-gap one-side welding with back formation
CN104002028A
GTAW welding system and method suitable for ultra-narrow gap
CN110977109A
Welding method for extremely thick steel plate
JP2007313524A