Nickel-based alloy coiled plate continuous annealing and pickling line welding method

By using argon-oxygen mixture and specific welding wire in nickel-based alloy welding, combined with automatic and manual welding technology, the difficulty and cracking problems of nickel-based alloy welding have been solved, and the continuous and stable production of nickel-based alloys and the expansion of thickness specifications have been achieved, reducing the crack risk and costs.

CN118720347APending Publication Date: 2024-10-01GANSU JIU STEEL GRP HONGXING IRON & STEEL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411213708.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Nickel-based alloys are difficult to weld in the production of stainless steel continuous annealing and pickling lines. They cannot be completely fused and are prone to cracks, leading to serious accidents such as belt breakage in the production line.

Method used

Using argon-oxygen mixed gas shielded welding, ER309L-Si welding wire and E309L-Si welding rod, through a combination of automatic welding machine and manual welding, the welding parameters and shielding gas flow are adjusted to form an I-shaped groove and perform the welding on the back of the weld. Hand fillet welding to ensure complete fusion and reduce risk of cracking.

Benefits of technology

It achieves continuous and stable production of nickel-based alloys, expands the range of thickness specifications, reduces crack sensitivity and welding wire procurement costs, and avoids strip breakage problems caused by weld quality issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
Patent Text Reader

Abstract

The invention discloses a continuous annealing and pickling line welding method for a nickel-based alloy coiled plate. The method comprises the following steps: (1) adjusting the flow of protective gas; (2) welding wire selection; (3) preparing a groove; (4) performing front welding by an automatic welding machine; (5) cutting a crescent on a welding seam; and (6) manually welding the back of the weld joint. According to the method, when a stainless steel continuous annealing and pickling line is utilized, during welding of N06625 and other nickel-based alloy rolled plates, a single-face welding and double-face forming automatic welding machine is selected, back forming depends on copper beam forcible forming, on the basis, small parameters are adopted for welding one pass on the front face through welding wires, and then welding is conducted for one pass on the back face through welding wires; and then filling the incomplete fusion part of the back surface by adopting manual shielded metal arc welding overhead welding, and finally realizing complete fusion of the N06625 and reducing the crack sensitivity by adopting a small-current rapid welding process for manual shielded metal arc welding. The welding wire and the welding rod used in the method are both made of common 309L-Si stainless steel, and the fusion depth is increased by adjusting the position of a welding torch, so that a welding joint can be solidified in an FA mode, and cracks are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nickel-based alloy welding, in particular to a nickel-based alloy coil continuous annealing and pickling line welding method. Background Art

[0002] N06625 nickel-based alloy is a solid solution strengthened alloy developed by adding Mo and Nb as the main strengthening elements to Ni-Cr alloy. It has good mechanical properties and corrosion resistance, and is an important raw material for aviation, aerospace, nuclear energy, petroleum and chemical industries. The production of N06625 coils generally uses the same equipment as the production of stainless steel coils, that is, it is produced using a stainless steel annealing and pickling line. The high temperature strength and rolling load of this type of steel during hot rolling are significantly higher than those of stainless steel products. At present, the maximum specification that can be hot-rolled for wide-width products (≥1030mm) is 7.5~8.5mm, and thinner specifications will exceed the rolling load. N06625 nickel-based alloy has the characteristics of high crack sensitivity and shallow melting depth during welding, which makes welding difficult. The subsequent hot annealing and pickling line production needs to weld the N06625 alloy coils with welding wire to ensure continuous production, but the on-site welding equipment is generally a MAG automatic welding machine, the groove is an I-shaped groove after double precision shearing, and there is no manual processing V-shaped groove condition, and the welding thickness is generally between 3.0 and 6.0 mm. Therefore, it is very difficult to use existing equipment to ensure that thick N06625 is completely fused without cracks. Summary of the invention

[0003] Based on the above, in order to solve the technical problems that the existing nickel-based alloys are extremely difficult to weld during the production of stainless steel continuous annealing and pickling lines, cannot be completely fused, and cracks will occur, resulting in vicious production accidents such as broken belts on the production line, the purpose of the present invention is to provide a nickel-based alloy coil continuous annealing and pickling line welding method to achieve continuous and stable production of nickel-based alloys in stainless steel hot annealing and pickling lines.

[0004] To achieve its purpose, the present invention adopts the following technical solution: A nickel-based alloy coil continuous annealing pickling line welding method, comprising the following steps: Step 1: Prepare protective gas and adjust flow rate Use argon-oxygen mixed gas as shielding gas to protect the weld; Step 2: Welding wire selection The welding wire is ER309L-Si, with a diameter of 1.2 mm; Step 3: Bevel preparation The nickel-based alloy coil to be welded is sheared into an I-type groove using a shearing device; Step 4: Automatic welding machine front welding The thickness of the nickel-based alloy coil is 7.5~8.5mm, and the welding parameters are controlled as follows: weld gap 2.0~2.2mm, welding voltage 26~28V, welding current 290~310A, wire feeding speed 15~16m / min, welding speed 0.5~0.6m / min, torch height 17~18mm; Step 5: Cut the crescent of the weld Cut crescents at the arc starting and arc ending parts of the weld; Step 6: Manual welding on the back of the weld At the weld inspection position, manual arc welding is used to fill the back of the weld. The welding rod is E309L-Si. Diameter 4.0mm.

[0005] As a further preferred embodiment of the technical solution of the present invention, the nickel-based alloy is N06625 nickel-based alloy; preferably, it is a wide and thick specification N06625 nickel-based alloy with a width of ≥1030 mm and a thickness of 7.5-8.5 mm.

[0006] Furthermore, in step 1, the argon-oxygen mixed gas is Ar and O with a volume fraction of 3-5%. 2 The protective gas should be appropriately increased in active gas O 2 The content (3~5%) can reduce the surface tension of liquid metal, improve the fluidity of the molten pool metal, and help increase the weld penetration.

[0007] Furthermore, in step 1, the flow rate of the argon-oxygen mixed gas is 15-20 L / min. Since the thickness of the base material is relatively thick (7.5-8.5 mm), appropriately increasing the flow rate of the protective gas can effectively prevent oxidation and stabilize the arc.

[0008] Furthermore, in step four, the automatic welding machine is a single-sided welding and double-sided forming welding machine.

[0009] Furthermore, in step six, the welding parameters of the manual arc welding overhead welding are: welding voltage 28~30V, welding current 140~160A, and welding speed 0.2~0.4m / min.

[0010] The present invention takes into account the characteristics of shallow penetration and high crack sensitivity of N06625 nickel-based alloy during welding, and the problem of serious production accidents such as cracking of the weld of wide and thick products during production in the thermal annealing and pickling line, and proposes a new welding method. Compared with the traditional method, the following beneficial effects are achieved: 1. The traditional thermal annealing and pickling line welding machine is a MAG automatic butt welding machine. The thickness of the welded stainless steel is generally between 3.0 and 6.0 mm. To achieve the welding of the wide and thick specification N06625 nickel-based alloy with a width of ≥1030 mm and a thickness of 7.5 to 8.5 mm, large welding parameters are required. However, the high nickel content and poor fluidity of the molten steel in N06625 lead to shallow weld depth. To achieve complete fusion, larger welding parameters are required, which may exceed the capacity limit of the welding machine equipment. The N06625 welding crack sensitivity is high, and large welding parameters will significantly increase the crack tendency. Generally, welding specifications recommend the use of small parameters for welding. The thermal annealing and pickling line welding machine of the present invention adopts a single-sided welding and double-sided forming automatic welding machine, and the back forming is forced to form by the copper beam. On this basis, a small parameter is first used to weld one pass on the front side, and the back side adopts manual arc welding to fill the unfused part on the back side. The manual arc welding adopts a small current fast welding process, and finally achieves complete fusion of N06625 and reduces crack sensitivity.

[0011] 2. The filling material of the welding method of the present invention adopts ordinary 309L-Si stainless steel welding wire and welding rod. By adjusting the position of the welding torch to increase the penetration depth, the weld joint can be solidified in FA mode to avoid the generation of cracks. Compared with the existing nickel-based alloy welding wire, the liquid molten pool has better fluidity and deeper penetration, and can also reduce the purchase cost of the welding wire.

[0012] 3. The welding method of the present invention can expand the thickness specification range of stainless steel and nickel-based alloys produced by the thermal annealing and pickling line, avoiding the problem of broken strips caused by weld quality problems during thermal annealing and pickling production of thick stainless steel and nickel-based alloys. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is the macroscopic morphology of the welded joint when welding N06625 using the traditional welding method; Figure 2 This is the macroscopic morphology of the welded joint when N06625 is welded by the welding method of the present invention. DETAILED DESCRIPTION

[0014] The present invention is further described below by means of specific embodiments in conjunction with the accompanying drawings, but the present invention is not limited in any form.

[0015] The present invention takes N06625 as an example to explain the detailed description of the welding method of the continuous annealing and pickling line of the nickel-based alloy coil. The automatic welding machine used is the RCM 250-65 DC argon arc welding machine of GUILD Company.

[0016] Example 1 Welding method of continuous annealing and pickling line for N06625 alloy coil with thickness of 7.5mm: Step 1: Prepare protective gas and adjust flow rate Using Ar+3%O 2 To protect the weld, the protective gas flow rate is 15L / min; Step 2: Welding wire selection The welding wire is ER309L-Si, with a diameter of 1.2 mm; Step 3: Bevel preparation The N06625 alloy coil to be welded is sheared into an I-type groove using a shearing device; Step 4: Automatic welding machine front welding The welding parameters were controlled as follows: weld gap 2.0 mm, welding voltage 26 V, welding current 290 A, wire feeding speed 16 m / min, welding speed 0.6 m / min, torch height 18 mm; Step 5: Cut the crescent of the weld Cut crescents at the arc starting and arc ending parts of the weld; Step 6: Manual welding on the back of the weld At the weld inspection position, manual arc welding is used for filler welding on the back of the weld. The welding rod is E309L-Si with a diameter of 4.0 mm. The welding parameters are controlled as follows: welding voltage 28 V, welding current 140 A, and welding speed 0.4 m / min.

[0017] After the welded nickel-based alloy coil passes through various bending rollers from the entrance to the exit of the annealing and pickling line, the weld remains intact, ensuring stable production.

[0018] Example 2 Welding method of continuous annealing and pickling line for N06625 alloy coil with thickness of 8.5mm: Step 1: Prepare protective gas and adjust flow rate Using Ar+4%O 2 Protect the weld with a protective gas flow rate of 20L / min; Step 2: Welding wire selection The welding wire is ER309L-Si, with a diameter of 1.2 mm; Step 3: Bevel preparation The N06625 alloy coil to be welded is sheared into an I-type groove using a shearing device; Step 4: Automatic welding machine front welding The welding parameters were controlled as follows: weld gap 2.2 mm, welding voltage 28 V, welding current 310 A, wire feeding speed 15 m / min, welding speed 0.5 m / min, torch height 17 mm; Step 5: Cut the crescent of the weld Cut crescents at the arc starting and arc ending parts of the weld; Step 6: Manual welding on the back of the weld At the weld inspection position, manual arc welding was used to fill the back of the weld. The welding rod was E309L-Si with a diameter of 4.0 mm. The welding parameters were controlled as follows: welding voltage 30 V, welding current 160 A, and welding speed 0.2 m / min. The final macroscopic morphology of the weld joint is as follows: Figure 1 As shown, compared with the traditional welding method when welding N06625, the macroscopic morphology of the welded joint ( Figure 2 , the weld root is not fully penetrated), the weld joint is completely fused and there are no solidification cracks.

[0019] After the welded nickel-based alloy coil passes through various bending rollers from the entrance to the exit of the annealing and pickling line, the weld remains intact, ensuring stable production.

[0020] Example 3 Welding method of continuous annealing and pickling line for N06625 alloy coil with thickness of 8.0mm: Step 1: Prepare protective gas and adjust flow rate Using Ar+5%O 2 To protect the weld, the protective gas flow rate is 18L / min; Step 2: Welding wire selection The welding wire is ER309L-Si, with a diameter of 1.2 mm; Step 3: Bevel preparation The N06625 alloy coil to be welded is sheared into an I-type groove using a shearing device; Step 4: Automatic welding machine front welding The welding parameters were controlled as follows: weld gap 2.1 mm, welding voltage 27 V, welding current 300 A, wire feeding speed 15.5 m / min, welding speed 0.55 m / min, and torch height 17.5 mm; Step 5: Cut the crescent of the weld Cut crescents at the arc starting and arc ending parts of the weld; Step 6: Manual welding on the back of the weld At the weld inspection position, manual arc welding is used for filler welding on the back of the weld. The welding rod is E309L-Si with a diameter of 4.0 mm. The welding parameters are controlled as follows: welding voltage 29 V, welding current 150 A, and welding speed 0.3 m / min.

[0021] After the welded nickel-based alloy coil passes through various bending rollers from the entrance to the exit of the annealing and pickling line, the weld remains intact, ensuring stable production.

Claims

1. A welding method for a nickel-based alloy coil continuous annealing and pickling line, It is characterized in that The following steps are involved: Step 1: Prepare protective gas and adjust flow rate Use argon-oxygen mixed gas as shielding gas to protect the weld; Step 2: Welding wire selection The welding wire is ER309L-Si, with a diameter of 1.2 mm; Step 3: Bevel preparation The nickel-based alloy coil to be welded is sheared into an I-type groove using a shearing device; Step 4: Automatic welding machine front welding The thickness of the nickel-based alloy coil is 7.5~8.5mm, and the welding parameters are controlled as follows: weld gap 2.0~2.2mm, welding voltage 26~28V, welding current 290~310A, wire feeding speed 15~16m / min, welding speed 0.5~0.6m / min, torch height 17~18mm; Step 5: Cut the crescent of the weld Cut crescents at the arc starting and arc ending parts of the weld; Step 6: Manual welding on the back of the weld At the weld inspection position, manual arc welding is used to fill the back of the weld. The welding rod is E309L-Si. Diameter 4.0mm.

2. A nickel-based alloy coil continuous annealing pickling line welding method as claimed in claim 1, It is characterized in that The nickel-based alloy is N06625 nickel-based alloy.

3. A nickel-based alloy coil continuous annealing pickling line welding method as claimed in claim 2, It is characterized in that The nickel-based alloy has a width of ≥1030 mm and a thickness of 7.5-8.5 mm.

4. A nickel-based alloy coil continuous annealing pickling line welding method as claimed in claim 3, It is characterized in that In step 1, the argon-oxygen mixed gas is Ar and O with a volume fraction of 3-5%. 2 mixture.

5. A nickel-based alloy coil continuous annealing pickling line welding method as described in any one of claims 1 to 4, It is characterized in that In step 1, the flow rate of the argon-oxygen mixed gas is 15-20 L / min.

6. A nickel-based alloy coil continuous annealing pickling line welding method as claimed in any one of claims 5, It is characterized in that In step 4, the automatic welding machine is a single-sided welding and double-sided forming welding machine.

7. A nickel-based alloy coil continuous annealing pickling line welding method as claimed in claim 6, It is characterized in that In step six, the welding parameters of the manual arc welding overhead welding are: welding voltage 28~30V, welding current 140~160A, and welding speed 0.2~0.4m / min.

Citation Information

Cited By

  • Dissimilar metal welding method applied to nickel-copper alloy and stainless steel