Aluminum-plated silicon steel and preparation method thereof, and production process of pre-coated plated steel and thermal forming component

By designing a pre-plating layer of specific structures in aluminum-plating silicon thermoformed steel, combining an appropriate amount of Al-Si phase and Al-Si-Fe phase to form a double Al-rich intermetallic compound layer, aluminum plating in the prior art is solved The toughness and hydrogen embrittlement resistance of silicon thermoformed steel improve welding performance and corrosion resistance.

CN119061342AActive Publication Date: 2024-12-03VALIN ARCELORMITTAL AUTOMOTIVE STEEL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411220790.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-27
Publication Date
2024-12-03
Estimated Expiration
2044-05-27

AI Technical Summary

Technical Problem

While pursuing high strength, existing aluminum-plated silicon thermoformed steels are difficult to take into account both toughness and hydrogen embrittlement resistance, and the welding and corrosion resistance of thin coatings are insufficient.

Method used

Aluminum-coated silicon steel with specific structures, including steel substrate and pre-plating. The pre-plating layer consists of an intermediate layer and an aluminum-silicon plating layer. The aluminum-silicon plating layer contains an appropriate amount of Al-Si phase and Al-Si-Fe phase, and controls the dispersion of the plating layer. The index and the area and convexity of the aluminum flower form a double layer of Al-rich intermetallic compound, which improves the toughness and environmental tolerance of the coating.

Benefits of technology

It improves the coating toughness and hydrogen embrittlement resistance of thermoformed components, reduces crack sensitivity, and enhances corrosion resistance, ensuring high strength and good welding performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061342A_ABST
    Figure CN119061342A_ABST
Patent Text Reader

Abstract

The invention provides aluminum-plated silicon steel, a preparation method thereof, precoated plated steel and a production process of a thermal forming component. The aluminized silicon steel comprises a pre-plating layer arranged on a steel substrate. The pre-plating layer comprises a middle layer and an aluminum-silicon plating layer; the nominal thickness of the aluminum-silicon coating ranges from 10 micrometers to 33 micrometers. The aluminum-silicon coating contains an Al-Si phase with the proportion being 5%-40% and an Al-Si-Fe phase with the proportion being 0.1%-15%, and the dispersion index of the Al-Si phase and the dispersion index of the Al-Si phase in the aluminum-silicon coating are larger than or equal to 0.05. According to the aluminum-plated silicon steel, the Al-Si phase and the Al-Si-Fe phase in the aluminum-silicon plating layer are appropriate in proportion and dispersion index, so that a thermal forming component produced subsequently is small in grain and has double Al-rich intermetallic compound layers, the plating layer toughness and environmental tolerance of the thermal forming component are improved, the crack sensitivity of the thermal forming component is reduced, and the service life of the thermal forming component is prolonged. And the thermoforming component also has the advantages of improving hydrogen embrittlement resistance, corrosion resistance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This invention patent application is a divisional application of the invention patent application with application date of May 27, 2024, application number 202410661792.0, and invention name "Aluminum-coated silicon steel and preparation method, pre-coated steel, and production process of hot-formed components". Technical Field

[0002] The present invention relates to the field of hot-formed steel, and in particular to aluminum-silicon-coated steel and a preparation method thereof, pre-coated steel, and a production process for hot-formed components. Background Art

[0003] At present, the strength of commercial hot-formed steel has exceeded 1500MPa, and 2000MPa hot-formed steel is becoming a hot spot for automotive steel. These hot-formed steels pursue strength while hoping to obtain higher toughness and better crack sensitivity. The strength of materials for collision energy absorption has also reached the 1000MP level. The coating of traditional aluminum-silicon hot-formed steel has a typical four-layer structure, namely (a) interdiffusion layer; (b) middle; (c) Al-rich intermetallic compound layer; (d) surface layer. This structure can be produced within a wider hot forming austenitizing processing window, not only to obtain higher strength, but also the welding performance of the coating is very excellent.

[0004] As the requirements for material costs increase, a type of thin-coated hot-formed steel has appeared on the market, but the coating of this type of material is not conducive to welding process control, and the corrosion resistance of the thin coating is low. Furthermore, as the material strength increases to more than 2000MPa, the hydrogen embrittlement problem has become the focus of attention. The processing window of hot-forming austenitization that takes into account both toughness and hydrogen embrittlement is an urgent need for most customers at present. Summary of the invention

[0005] The main purpose of the present invention is to provide an aluminum-coated silicon steel, a hot-formed component and a production process thereof, so as to solve the technical problem that conventional aluminum-coated silicon steel cannot take into account both toughness and hydrogen embrittlement.

[0006] To achieve the above-mentioned purpose, the present application provides an aluminum-silicon-plated steel, comprising a steel substrate and a pre-plated layer arranged on the steel substrate;

[0007] The pre-plating layer includes an intermediate layer and an aluminum silicon coating layer; the nominal thickness of the aluminum silicon coating layer is 10 μm to 33 μm; the aluminum silicon coating layer contains 5 to 40% of an Al-Si phase and 0.1 to 15% of an Al-Si-Fe phase, and the dispersion index of the Al-Si phase and the Al-Si-Fe phase in the aluminum silicon coating layer is ≥0.05;

[0008] The mass fraction of silicon in the Al-Si phase is 30-50%; the mass fraction of iron in the Al-Si-Fe phase is 10-35%, and the mass fraction of silicon is 3-15%;

[0009] Preferably, the aluminum-silicon coating contains 10-30% of an Al-Si phase and 0.1-10% of an Al-Si-Fe phase, wherein the mass fraction of silicon in the Al-Si phase is 30-50%; the mass fraction of iron in the Al-Si-Fe phase is 10-35%, and the mass fraction of silicon is 3-15%.

[0010] According to an embodiment of the present application, the Al-Si phase includes Al n Si m Phase; wherein n:m=(1.0~3.0):1; the Al n Si m The proportion of the phase in the Al-Si phase is ≥50%.

[0011] According to an embodiment of the present application, the Al n Si m The phase includes at least one of Al4Si3 and Al4Si2.

[0012] According to an embodiment of the present application, the Al-Si-Fe phase includes Fe a Si b Al c phase; wherein a:b:c=(1~2):1:(4~9); the Fe a Si b Al c The proportion of the Al-Si-Fe phase in the Al-Si-Fe phase is ≥50%. a Si b Al c The phases include FeSiAl4 phase and Fe2SiAl7 phase.

[0013] The present application provides another aluminum-silicon-plated steel, comprising a steel substrate and a pre-plated layer arranged on the steel substrate; the pre-plated layer comprises an intermediate layer and an aluminum-silicon coating layer; the aluminum-silicon coating layer comprises aluminum flowers; the nominal thickness of the aluminum-silicon coating layer is 10 to 20 μm, and the aluminum flowers meet the aluminum flower area (mm 2 ) and the aluminum flower convexity (μm) form a coordinate point located within the first convex pentagon, wherein the first convex pentagon is surrounded by five points: (2, 3), (150, 3), (350, 7), (350, 35), and (2, 35).

[0014] According to the implementation mode of the present application, the aluminum silicon coating includes aluminum flowers; the nominal thickness of the aluminum silicon coating is 19 to 33 μm, and the aluminum flowers meet the aluminum flower area (mm2 ) and the aluminum flower convexity (μm) form a coordinate point located within a second convex pentagon, wherein the second convex pentagon is surrounded by five points: (4, 5), (170, 5), (400, 12), (400, 40), and (4, 40).

[0015] According to an embodiment of the present application, the aluminum-silicon coating includes aluminum flowers; the nominal thickness of the aluminum-silicon coating is 10 to 20 μm, and the aluminum flowers satisfy the conditions that the coordinate points formed by the aluminum flower boundary length per unit area (1 / mm) and the aluminum flower convexity (μm) are located within a third convex pentagon, and the third convex pentagon is surrounded by five points: (0.1, 7), (0.17, 3), (10, 3), (10, 35), and (0.1, 35).

[0016] According to an embodiment of the present application, the aluminum-silicon coating includes aluminum flowers; the nominal thickness of the aluminum-silicon coating is 19 to 33 μm, and the aluminum flowers satisfy the condition that the coordinate points formed by the aluminum flower boundary length per unit area (1 / mm) and the aluminum flower convexity (μm) are located within the fourth convex pentagon, and the fourth convex pentagon is surrounded by five points: (0.08, 12), (0.16, 5), (8, 5), (8, 40), and (0.08, 40).

[0017] The present application discloses a method for preparing aluminum-plated silicon steel, comprising the following steps:

[0018] After annealing the steel substrate to be plated, the substrate is dip-plated in a plating solution to obtain a dip-plated steel substrate; the plating solution comprises, by mass percentage, 8 to 11% Si; 1 to 4% Fe; and the remainder is Al and unavoidable impurities;

[0019] Cooling the dip-plated steel substrate to 570°C to 650°C at a rate of 2 to 20°C / s, and maintaining the temperature at 570°C to 650°C for 1 to 20 seconds to obtain primary cold dip-plated steel;

[0020] The primary cold-dip plated steel is placed in a temperature regulating device and, under the condition of heated gas, continuously cooled to 300°C at an average cooling rate of 5-25°C / s, and the holding time is 2-30 seconds, to obtain secondary cold-dip plated steel; the temperature of the temperature regulating device is 300°C-570°C; the temperature of the heated gas is ≥100°C, and the total suspended particulate matter in the gas is ≤0.2mg / m3;

[0021] The second cold-dip plated steel is cooled to room temperature to obtain pre-coated plated steel.

[0022] According to an embodiment of the present application, the dip-plated steel substrate is cooled to 570° C. at a rate of 2 to 15° C. / s, and maintained at 570° C. for 1 to 10 seconds to obtain the initial cold dip-plated steel.

[0023] According to an embodiment of the present application, the primary cold-dip plated steel is cooled to 300° C. at an average cooling rate of 5 to 20° C. / s, and the holding time is 2 to 20 seconds to obtain the secondary cold-dip plated steel.

[0024] According to the implementation mode of the present application, the annealing temperature in the annealing step of the steel substrate to be plated is 700-850°C, and the annealing time is 1-20 minutes; the temperature of the steel substrate to be plated after annealing entering the immersion plating solution is 600-700°C.

[0025] The present application also discloses a pre-coated steel, which is obtained by cold rolling and skin-passing aluminum-silicon-coated steel; the pre-coated steel comprises a steel substrate and a skin-pass coating disposed on the steel substrate; the skin-pass coating is obtained by at least one of cold rolling and skin-passing;

[0026] The polished coating comprises an intermediate layer and an aluminum silicon coating; the nominal thickness of the aluminum silicon coating is 10 μm to 33 μm; the aluminum silicon coating contains 5 to 40% of an Al-Si phase and 0.1 to 15% of an Al-Si-Fe phase, and the dispersion index of the Al-Si phase and the Al-Si-Fe phase in the aluminum silicon coating is ≥0.05;

[0027] The mass fraction of silicon in the Al-Si phase is 30-50%; the mass fraction of iron in the Al-Si-Fe phase is 10-35%, and the mass fraction of silicon is 3-15%.

[0028] The present application also discloses a hot-formed component, comprising a steel substrate and a component coating; the component coating is produced by mutual diffusion between the steel substrate and the aluminum-silicon pre-coating layer;

[0029] The component coating comprises an interdiffusion layer, a first intermediate layer, a first Al-rich intermetallic compound layer, a second intermediate layer and a second Al-rich intermetallic compound layer stacked in sequence; the interdiffusion layer is located at the innermost side of the component coating;

[0030] The first Al-rich intermetallic compound layer is a discontinuous structure, accounting for ≤80% of the length of the layer; the second Al-rich intermetallic compound layer is a quasi-continuous structure, accounting for ≥20% of the continuous length of the layer;

[0031] Preferably, the first Al-rich intermetallic compound layer accounts for 1 to 50% of the length of the layer; the second Al-rich intermetallic compound layer accounts for ≥50% of the continuous length of the layer; more preferably, the second Al-rich intermetallic compound layer accounts for 50 to 90% of the continuous length of the layer.

[0032] According to an embodiment of the present application, the component plating further includes a surface layer located outside the second Al-rich intermetallic compound layer.

[0033] According to an embodiment of the present application, the grain size of the first intermediate layer, the second intermediate layer, and the surface layer is less than or equal to 30 μm; preferably, the grain size of the first intermediate layer, the second intermediate layer, and the surface layer is less than or equal to 25 μm; more preferably, the grain size of the first intermediate layer, the second intermediate layer, and the surface layer is less than or equal to 15 μm. The grain size of the intermediate layer of the coating of the present invention is the average grain size of the coating observed in cross section.

[0034] According to an embodiment of the present application, the total coating thickness of the component is 5 μm to 60 μm; preferably, the total coating thickness of the component is 20 μm to 55 μm; preferably, the total coating thickness of the component is 26 μm to 50 μm; further preferably, the total coating thickness of the component is 30 μm to 50 μm.

[0035] The present application also discloses another hot-formed component, comprising a steel substrate and a component coating; the component coating is produced by mutual diffusion between the steel substrate and the aluminum-silicon pre-coating layer; the component coating has at least four Si concentration peaks along the thickness direction.

[0036] According to an embodiment of the present application, the at least four Si concentration peaks include a first Si concentration peak, a second Si concentration peak, a third Si concentration peak and a fourth Si concentration peak from the component coating surface to the steel substrate;

[0037] The distance between the first Si concentration peak and the surface of the component coating is ≥0.25 μm.

[0038] According to an embodiment of the present application, the distance between the first Si concentration peak and the surface of the component coating is ≥0.45 μm.

[0039] According to an embodiment of the present application, the distance between the first Si concentration peak and the surface of the component coating is ≥0.75 μm.

[0040] According to an embodiment of the present application, the distance between the first Si concentration peak and the surface of the component coating is ≥1.5 μm.

[0041] According to an embodiment of the present application, after deducting the background from the at least four Si concentration peaks, the concentration value of the minimum peak therein is ≥0.01%.

[0042] According to an embodiment of the present application, the concentration value of the minimum peak value is ≥ 0.025%.

[0043] According to an embodiment of the present application, the concentration value of the minimum peak value is ≥ 0.05%.

[0044] According to an embodiment of the present application, the concentration value of the minimum peak is ≥ 0.25%.

[0045] The present invention also discloses a production process of a thermoforming component, comprising the following steps:

[0046] The aluminum-silicon-plated steel or the pre-coated steel is heated to the austenite range, the holding temperature range is 880-950°C, and the holding time is 3-15 minutes; the heating atmosphere is air, and the dew point is ≤0°C;

[0047] The steel plate after insulation is cooled, and the heated steel plate is taken out and deformed by pressing with a mold within 10 seconds, and cooled to below 200°C at the same time.

[0048] The invention also discloses a motor vehicle, comprising the above-mentioned hot-formed component.

[0049] In the above-mentioned aluminum-silicon steel, the ratio of Al-Si phase and Al-Si-Fe phase in the aluminum-silicon coating is appropriate, and the dispersion index is appropriate, which helps the subsequent hot-formed components to have smaller grains and a double-layer Al-rich intermetallic compound layer, thereby improving the coating toughness and environmental tolerance of the hot-formed components, reducing their crack sensitivity, and making the hot-formed components also have the advantages of improved hydrogen embrittlement resistance and corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0051] Figure 1 This is a typical aluminum flower morphology of the coated steel strip of the present invention before hot forming;

[0052] Figure 2 This is a typical aluminum flower morphology of the component of the present invention after hot forming;

[0053] Figure 3 It is a typical metallographic structure of the coating of the component of the present invention after hot forming;

[0054] Figure 4 It is the typical metallographic structure of the coating of the conventional hot-formed component after hot-forming;

[0055] Figure 5 The component of the present invention is a deformed coating structure after thermoforming;

[0056] Figure 6 It is a deformed coating structure of a conventional hot-formed steel component after hot forming;

[0057] Figure 7 It is a diagram of the structure of the pre-plating layer before hot forming;

[0058] Figure 8 The coating structure of the component of the present invention after thermoforming;

[0059] Fig. 9 It is the coating structure of the traditional thermoformed component after thermoforming;

[0060] Fig.10 The distribution of Si and Fe elements in the cross section of the aluminum-silicon steel coating of the present invention;

[0061] Fig.11 The aluminum flower area of ​​the steel strip before hot forming is ≥ 200 mm. 2 ;

[0062] Fig.12 It shows that the aluminum flower area on the surface of the strip steel of the present invention before hot forming is ≤9mm 2 ;

[0063] Fig.13 is the coating composition characteristic of the component of the present invention after thermoforming;

[0064] Fig.14 It is the coating composition characteristic of traditional components after hot forming.

[0065] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0066] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0067] It should be noted that all directional indications (such as up, down, etc.) in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0068] In addition, in the present invention, the descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features.

[0069] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0070] The applicant has conducted a lot of research on hot-formed components. Most existing hot-formed components are four-layer structures, which specifically include: (a) interdiffusion layer; (b) intermediate layer; (c) Al-rich intermetallic compound layer; (d) surface layer. In addition, the Al-rich intermetallic compound layer is a quasi-continuous structural layer. That is, in the metallographic image, the length of the Al-rich intermetallic compound layer accounts for a large proportion of the length of the structural layer, such as 90%. The visual metallographic image is basically continuous as a whole. The length of the structural layer is the total length of the coating measurement.

[0071] The inventors have found that there are often brittle Al-rich intermetallic compounds at the interface between the interdiffusion layer and the first intermediate layer (i.e., the surface of the interdiffusion layer). When the Al-rich intermetallic compound on the surface of the interdiffusion layer is thicker, the cracks initiated on the surface of the coating will almost all extend to the steel matrix during the bending process of the material. However, when the Al-rich intermetallic compound on the surface of the interdiffusion layer is reduced, the difficulty of crack extension from the outside to the inside of the interdiffusion layer increases, and even the interdiffusion layer remains intact while cracks initiate in the steel matrix. This shows that reducing the thickness of the Al-rich intermetallic compound on the surface of the interdiffusion layer helps to improve the plasticity of the interdiffusion layer, and further can prevent the propagation of cracks from the surface to the inside of the steel matrix. Further research found that the first Al-rich intermetallic compound layer easily merges with the Al-rich intermetallic compound on the surface of the interdiffusion layer and disappears. This merger not only thickens the Al-rich intermetallic compound on the surface of the interdiffusion layer, but also easily leads to the formation of sharp edges and corners of the Al-rich intermetallic compound on the surface of the interdiffusion layer. Stress concentration is often at the edges and corners, which makes it easy for cracks to initiate and propagate. If the cracks at this location continue to propagate and expand inward, they will reach the interface between the steel matrix and the interdiffusion layer, further causing the steel matrix to crack.

[0072] After deformation (such as bending), if a large number of cracks appear in the interdiffusion layer, it will help the intrusion of hydrogen into the martensite structure of the steel matrix. Therefore, a complete interdiffusion layer can not only improve the bending toughness of the material, but also improve the material's resistance to hydrogen embrittlement to a certain extent.

[0073] Therefore, the first Al-rich intermetallic compound layer specially provided in the present invention can share the enrichment degree of the Al-rich intermetallic compound in the interdiffusion layer, thereby improving the plasticity of the interdiffusion layer. In particular, when the thickness of the coating after hot forming exceeds 26 μm, sufficient Al-rich intermetallic compounds can be formed in the coating. The present invention cleverly decomposes a portion of the Al-rich intermetallic compounds on the surface of the interdiffusion layer to form a new first Al-rich intermetallic compound layer, thereby improving the plasticity of the interdiffusion layer and reducing the number of crack penetrations.

[0074] To form the hot-formed components of the above structure, the raw material aluminum-plated silicon steel or aluminum-plated silicon steel after skin-finishing (i.e., pre-coated steel hereinafter) must meet specific conditions. The aluminum-plated silicon steel or aluminum-plated silicon steel after skin-finishing (i.e., pre-coated steel hereinafter) are introduced below.

[0075] To achieve the above-mentioned purpose, the present application provides an aluminum-silicon-plated steel, comprising a steel substrate and a pre-plated layer arranged on the steel substrate;

[0076] The pre-plating layer includes an intermediate layer and an aluminum silicon coating layer. The nominal thickness of the aluminum silicon coating layer is 10 μm to 33 μm. The aluminum silicon coating layer contains 5 to 40% of Al-Si phase and 0.1 to 15% of Al-Si-Fe phase, and the dispersion index of the Al-Si phase and the Al-Si-Fe phase in the aluminum silicon coating layer is ≥ 0.05. Among them, the mass fraction of silicon in the Al-Si phase is 30 to 50%. The mass fraction of iron in the Al-Si-Fe phase is 10 to 35%, and the mass fraction of silicon is 3 to 15%.

[0077] Energy dispersive spectrometer (EDS) can be used to scan the Si and Fe element distribution of the coating cross section (such as Fig.10 ) The phases with dense and bright distribution of Si and Fe elements in the coating are Al-Si and Al-Si-Fe phases respectively. Then use image software (such as Image-pro Plus) to calculate the proportion of Al-Si phase and Al-Si-Fe in the coating. When calculating the proportion, the interdiffusion layer between the coating and the substrate should be removed. In order to ensure that the test results are representative, the continuous coating section length ≥ 100mm can generally be cumulatively tested.

[0078] Aluminum-silicon coated steel is usually formed by hot-dip coating of a steel substrate. The steel substrate includes steel billets, hot-rolled strip steel and cold-rolled strip steel. The steel substrate to be plated is generally in the form of a flat steel strip. The size of the steel strip is referred to GB708-2006. It is also called steel strip, strip steel or steel plate in the industry. Such naming does not affect the interpretation of the present invention. The thickness of the steel substrate to be plated is usually 0.5 to 3.5 mm.

[0079] The steel substrate to be plated referred to in the present invention is the steel material used for hot-dip plating, including hot-rolled steel plates and cold-rolled steel plates, or collectively referred to as strip steel. The steel substrate to be plated can exist in geometric forms such as coils, sheets, parts, etc., and the steel substrate to be plated for continuous annealing is generally in the form of coils. Regardless of the geometric form in which the steel substrate to be plated exists, it does not affect the interpretation of the present invention. The strip steel after hot-dip plating is cut into steel plates of suitable sizes, and the steel plates are thermoformed to obtain components in the shape of parts, sheets, etc. with the required geometric dimensions. Regardless of the geometric form in which the components after thermoforming exist, it does not affect the interpretation of the present invention. The coating referred to in the present invention can be a double-sided coating on the upper and lower sides, or a coating on one side.

[0080] In some embodiments, the steel substrate is a boron-containing anti-intrusion automotive hot-formed steel comprising Or including composition range: C: 0.18-0.45%, Mn: 0.3-3.0%, B: 0.0008-0.005%, alloying elements can be added. The tensile strength of the material after hot forming is ≥1500MPa, and this embodiment is particularly aimed at materials with a tensile strength of ≥1800MPa after hot forming.

[0081] In some embodiments, the steel material is a hot-formed steel for automobiles for collision energy absorption containing niobium, comprising Or including composition range: C: 0.03-0.12%, Mn: 0.15-2.5%, Nb: 0.02-0.10%, alloying elements that can be added, including B: 0.0008-0.005%. The tensile strength of the material after hot forming is ≤1500MPa, and this embodiment is particularly for materials with a tensile strength of 900MPa-1500MPa after hot forming.

[0082] The aluminum silicon coating of aluminum silicon steel comprises (1) an intermediate layer; (2) an aluminum silicon coating. The aluminum silicon coating contains 5 to 40% of an Al-Si phase, and the mass fraction of silicon in the Al-Si phase is 30 to 50%; the aluminum silicon coating contains 0.1 to 15% of an Al-Si-Fe phase, and the mass fraction of iron in the Al-Si-Fe phase is 10 to 35%, and the mass fraction of silicon is 3 to 15%.

[0083] After careful research, the inventors found that by reasonably controlling the manufacturing process, a certain proportion of Al-Si phase and Al-Si-Fe phase (such as Fig. 9). Al-Si phase and Al-Si-Fe phase are the key sources of Al-rich intermetallic compounds in the coating during the hot forming process. The distribution form and quantity of the Al-Si phase and Al-Si-Fe phase in the pre-plating layer largely determine the position and quantity of the Al-rich intermetallic compounds after hot forming. When the Al-Si phase and Al-Si-Fe phase in the pre-plating layer are more and dispersed in the coating, it is conducive to the formation of the first Al-rich intermetallic compound layer after hot forming. When the Al-Si phase and Al-Si-Fe phase in the pre-plating layer are less and concentrated in the coating, the first Al-rich intermetallic compound layer after hot forming is difficult to appear, and is replaced by a single-layer Al-rich intermetallic compound of traditional hot forming steel, so that the double-layer Al-rich intermetallic compound of the present invention cannot be obtained.

[0084] In order to obtain the above-mentioned double-layer Al-rich intermetallic compound structure after hot forming, the Al-Si phase and the Al-Si-Fe phase should be dispersed in the pre-plating layer, not aggregated into lines or large blocks. The aluminum-silicon coating should contain 5-40% of the Al-Si phase, and the mass fraction of silicon in the Al-Si phase is 20-50%; the aluminum-silicon coating should contain 0.1-15% of the Al-Si-Fe phase, the mass fraction of iron in the Al-Si-Fe phase is 10-35%, and the mass fraction of silicon is 3-15%. Preferably, the aluminum-silicon coating contains 10-30% of the Al-Si phase, and the mass fraction of silicon in the Al-Si phase is 30-50%; the aluminum-silicon coating contains 0.1-15% of the Al-Si-Fe phase, and the mass fraction of iron in the Al-Si-Fe phase is 10-35%, and the mass fraction of silicon is 3-15%.

[0085] In order to better illustrate the characteristics of the present invention, the dispersion degree of the Al-Si phase and Al-Si-Fe of the present invention is explained by the dispersion index. Within the range of 20×100 square microns of the aluminum silicon coating (1), each uniformly sized and significantly discontinuous Al-Si phase and Al-Si-Fe phase is simplified to a particle at the geometric center, or a single Al-Si phase and Al-Si-Fe phase with an area ≥1 square micron is simplified to a particle, and three adjacent particles are connected. If the triangle formed by connecting the three particles is a non-obtuse triangle, it is recorded as a type A triangle. If it is an obtuse triangle, it is recorded as a type B triangle. The dispersion index is defined as the ratio of type A triangles to the total number of triangles. The larger the index, the greater the degree of dispersion. For the present invention, when the dispersion index is ≥0.05, there is a tendency to form a first Al-rich intermetallic compound layer at this position, that is, after hot forming, a 6-layer coating structure containing a double layer of Al intermetallic compounds (a first Al-rich intermetallic compound layer and a second layer) is easily formed. Preferably, the local dispersion index is ≥0.1.

[0086] When the above conditions are met, the Al-Si phase and Al-Si-Fe phase of the coating will have the following situation: ③ less quantity and clear boundary. Otherwise, the Al-Si phase and Al-Si-Fe phase of the coating will have the following situation: ① more quantity and fuzzy boundary; ② less quantity and fuzzy boundary.

[0087] In order to avoid the local aggregation of Al-Si phase and Al-Si-Fe phase, which leads to the excessive thickness and sharpness of Al-rich intermetallic compounds on the surface of the interdiffusion layer, the dispersed distribution of the present invention is particularly important for this position. The dispersed distribution can promote the formation of the first Al-rich intermetallic compound layer and avoid the excessive thickness and sharpness of Al-rich intermetallic compounds on the surface of the interdiffusion layer. While the present invention meets the requirements of the content ratio and dispersion index of Al-Si phase and Al-Si-Fe phase, the proportion of the discontinuous first Al-rich intermetallic compound layer in the considered structural layer will exceed 0.5%. Preferably, the proportion of the first Al-rich intermetallic compound layer in the considered structural layer exceeds 1%. This ratio is the ratio of the length obtained by connecting the first Al-rich intermetallic compound layer to the length of the structural layer, and the length of the structural layer is the total length measured by the coating.

[0088] In the above-mentioned aluminum-silicon steel, the ratio of Al-Si phase and Al-Si-Fe phase in the aluminum-silicon coating is appropriate, and the dispersion index is appropriate, which helps the subsequent hot-formed components to have smaller grains and a double-layer Al-rich intermetallic compound layer, thereby improving the coating toughness and environmental tolerance of the hot-formed components, reducing their crack sensitivity, and making the hot-formed components also have the advantages of improved hydrogen embrittlement resistance and corrosion resistance.

[0089] The applicant also found that a large number of literatures have conducted detailed analysis on the coating structure of the existing pre-plating layer of hot-formed steel, and believed that before austenitization (before hot forming heating), the pre-plating layer of the strip steel is mainly composed of intermetallic compounds formed by the eutectic reaction of pure Al and pure Si. The coating consists of three parts. The outermost layer is a pure Al layer, which includes a small amount of Si-rich phase and Fe-Al-Si ternary alloy; the middle layer is a Fe-Al-Si ternary alloy phase; the inner layer is a Fe-Al alloy layer, the main components of which are Fe2Al5 and FeAl3. The pure Si phase is in the form of elongated strips and has a brighter color. There is a brighter intermediate layer between the coating and the steel substrate, with a thickness of about 5 mm, which is analyzed to be Fe2SiAl7 (τ5 phase). There is a thin compound layer composed of Fe2Al5 and FeAl3 between the intermetallic compound Fe2SiAl7 and the steel substrate.

[0090] The Al-Si phase is mainly composed of Al n Si m The cluster structure exists or contains no more than 1% Fe. The atomic structure stability of these aluminum-silicon phases is highly correlated with their bonding mode and binding energy.

[0091] In some embodiments, the Al-Si phase includes Al n Si m Phase. Where n:m=(1.0~3.0):1. The Al n Si m The ratio of the Al-Si phase to the Al-Si phase is ≥50%. n Si m The phase includes at least one of Al4Si3 and Al4Si2.

[0092] The present invention mainly controls the Al-Si phase with an atomic ratio n:m ranging from 1.0 to 3.0 to obtain a certain proportion of the desired Al-Si phase, which is conducive to the formation of the coating structure after hot forming of the present invention. Furthermore, the key precipitated phase includes a phase with an Al-Si atomic ratio between 1.3 and 2.5, such as Al4Si3 and Al4Si2. This type of Al-Si phase (including Al4Si3 and Al4Si2) is the precipitation phase requirement to be controlled by the present invention. Due to the bonding properties of the physical phases, the existence of Al4Si3 and Al4Si2 cannot be stable. The present invention uses a heat preservation cover, coating heating, high-purity dry air and other means during the controlled cooling process of the coating, which can improve the stability of Al4Si3 and Al4Si2 and obtain more particles and more effective Al-Si phases.

[0093] In some embodiments, the Al-Si-Fe phase includes Fe a Si b Al c phase; wherein a:b:c=(1~2):1:(4~9); the Fe a Si b Al c The proportion of the Al-Si-Fe phase in the Al-Si-Fe phase is ≥50%. a Si b Al c The phases include FeSiAl4 phase and Fe2SiAl7 phase.

[0094] Al-Si-Fe phase is the main form of Fe in the coating. This phase is the product of the Fe element of the steel matrix diffusing into the plating solution and recombining with the Al-Si phase to form the Al-Si-Fe phase. Existing studies have shown that during the cooling process of the hot-dip plating solution, a solid needle-shaped FeSiAl4 (τ6 phase) phase is generated in the coating. However, the inventors have found that in fact, there is also a Fe2SiAl7 (τ5 phase) phase in the coating. This type of Al-Si-Fe phase (mainly including τ5 and τ6 phases) is the precipitation phase required by the present invention.

[0095] In some embodiments, the aluminum silicon coating includes aluminum flowers. The nominal thickness of the aluminum silicon coating is 10 to 20 μm, and the aluminum flowers meet the aluminum flower area (mm 2 ) and the aluminum flower convexity (μm) form a coordinate point located within the first pentagon, wherein the first pentagon is surrounded by five points: (2, 3), (150, 3), (350, 7), (350, 35), and (2, 35).

[0096] Aluminum-silicon coated steel sheets form a single aluminum solidification layer at around 600°C. The phase structure of aluminum-silicon solidification forms a flower-shaped polygonal pattern during the solidification process. This flower-shaped polygonal pattern is called "aluminum flower".

[0097] There is a certain relationship between the coating thickness and the area of ​​aluminum flowers. The thicker the coating thickness, the easier it is for the aluminum flowers to grow. This is mainly related to the lower cooling rate of the thick coating. When the coating thickness is ≥10μm, the area of ​​the aluminum flowers is controllable. When the coating thickness is ≥19μm, the area of ​​the aluminum flowers is more appropriate. The average thickness of the pre-plating layer is 10μm to 33μm. Preferably, the average thickness of the pre-plating layer is 19μm to 33μm.

[0098] The inventors have found that the continuity of the first Al-rich intermetallic compound layer is related to the size of the aluminum flower. A larger aluminum flower area can also retain more complete aluminum dendrites and reduce the number of aluminum grain boundaries. Grain boundaries often have more precipitates, which become the gathering place of diffusible hydrogen. Once the conditions are met, this diffusible hydrogen will transfer into the steel matrix. There are fewer defects in complete grains, and the diffusible hydrogen is reduced accordingly, which can hinder the intrusion of hydrogen into the steel matrix to a certain extent. The hydrogen embrittlement resistance of hot-formed parts is related to coarse aluminum flowers. Therefore, increasing the area of ​​the aluminum flower to 4mm 2 And above, and keep the pre-plating thickness above 10μm, which helps to reduce the diffusible hydrogen content of the coating and alleviate the diffusion of hot hydrogen into the steel matrix. Average aluminum flower area ≥16mm 2 If the pre-plating thickness is kept above 19 μm, the number of grain boundaries will be significantly reduced, thereby reducing the amount of hydrogen diffusion from the grain boundaries of the aluminum flower to the inside. 2 And below, and the coating thickness is less than 10μm, the protective effect of the aluminum flowers will be affected. The reason is that the thickness of the aluminum flower boundary is thin, the invasion distance of hydrogen at this position will be greatly reduced, and the invasion of hydrogen into the steel matrix becomes easier. Small aluminum flowers and thin coatings are not conducive to blocking hydrogen intake.

[0099] In the related art, since the above protective effect of aluminum flowers has not been found, it is believed that aluminum flowers affect the appearance of the final hot-formed parts, and it is usually hoped that the area of ​​aluminum flowers is as small as possible, or there is no aluminum flower. For example, by controlling the coating process, the aluminum flowers are made smaller or there is no aluminum flower. Or the aluminum flowers are covered by powder spraying.

[0100] In this application, the nominal thickness is the set thickness of the aluminum silicon coating, that is, the target thickness of the aluminum silicon coating. For the convenience of comparative analysis and explanation, the aluminum flower convexity described in the present invention is the aluminum flower convexity of the strip steel produced when the surface treatment (such as skin finishing) is not applied.

[0101] The present invention needs to provide a larger aluminum flower for the coating. A larger aluminum flower will increase the thickness difference of the coating locally. The growth process of aluminum flower is the process of aluminum flower nucleation and growth. The center of the aluminum flower first forms nucleus and grows first. It continues to solidify and thicken during the growth process. The thickness here is larger. The edge of the aluminum flower solidifies and grows at the central nucleation point later. The thickness here is thinner. When the aluminum flower area is 4mm 2 When the aluminum flower area is 16mm, this uneven thickness will affect the distribution of Al-Si phase and Al-Si-Fe phase in the coating. 2 When the thickness is above 0.5, the unevenness is more obvious. After the aluminum flower is enlarged by the coating cooling process of the present invention, obvious thickness difference can be seen under a microscope, and even the coating feels uneven when touched by hand.

[0102] The fact that the coating thickness at the center of the aluminum flower is greater than the coating thickness at the boundary of the aluminum flower is one of the key factors that promote the appearance of a six-layer structure after hot forming in the present invention. The existence of this difference is conducive to promoting the formation of sufficient Al-Si phase and Al-Si-Fe phase near the center of the aluminum flower in the pre-plated layer. The aluminum flower convexity (C) is defined as: the difference between the three-point average value of the maximum coating thickness near the center of the aluminum flower on the pre-plated strip and the three-point average value of the minimum thickness near the edge of the aluminum flower. The aluminum flower convexity of the present invention is generally ≥1μm. In order to meet the quality requirements of the present invention, the aluminum flower convexity should be maintained at least ≥3μm, especially when the coating aluminum flower convexity is ≥5μm, the effect of promoting the six-layer structure after hot forming is more obvious. For materials with thicker thickness and a single-sided coating thickness of 19 to 33μm, the aluminum flower convexity is maintained at least ≥5μm.

[0103] Since the Al-Si phase and Al-Si-Fe phase in the coating have been basically formed before the coating is smoothed and straightened, even after smoothing, the aluminum flower convexity of less than 3μm can meet the requirements of the present invention. Therefore, the aluminum flower coating convexity requirement required by the present invention is the aluminum flower coating convexity requirement before surface treatment (such as smoothing, rolling, and hot forming). Generally, when the pre-plating thickness is set at 10 to 20μm (nominal thickness 10 to 20μm), due to the existence of the aluminum flower convexity, it can be 5 to 40μm, so the maximum aluminum flower convexity can be ≥35μm. When the layer thickness is set at 19 to 33μm (nominal thickness 19 to 33μm), the pre-plating thickness range can be 10 to 50μm, so the maximum aluminum flower convexity can be ≥40μm. Without the process treatment of the present invention, it is difficult to obtain the convexity required by the present invention.

[0104] Analysis shows that the aluminum flower convexity is related to the coating thickness and the aluminum flower size. Generally speaking, the thinner the coating, the smaller the aluminum flower convexity, and the smaller the aluminum flower area, the smaller the aluminum flower convexity. In order for the material properties after hot forming to meet the requirements of the present invention, the relationship between the aluminum flower convexity, the aluminum flower area and the coating thickness should meet the following requirements.

[0105] C≥a·S

[0106] In the above formula: C is the convexity of the aluminum flower, in μm; S is the area of ​​the aluminum flower, in mm 2 ; a is the coefficient, unit is μm / mm 2 , for the convenience of calculation and explanation, the value of a is 0.02.

[0107] As a preference, (1) when the average thickness of the single-sided coating is less than 19 μm, the coefficient is 0.02, that is, C ≥ 0.02S. However, in order to meet the distribution requirements of the coating precipitation phase, when the single-sided coating thickness is less than 19 μm, the aluminum flower convexity is at least 3 μm. (2) When the average thickness of the single-sided coating is ≥ 19 μm, the coefficient is 0.03, that is, C ≥ 0.03S. In order to meet the distribution requirements of the coating precipitation phase, when the single-sided coating thickness is ≥ 19 μm, the aluminum flower convexity is at least 5 μm.

[0108] Under ideal conditions, the growth of a single aluminum flower in three-dimensional space can be equiaxed, that is, the thickness of the aluminum flower is equal to the diameter of the aluminum flower. However, the aluminum flowers on the surface of the strip steel of the present invention are relatively large, and the thickness growth is limited. They will not become equiaxed, but flat. The convexity of the aluminum flower of the present invention should be subject to an upper limit control, otherwise it will cause the coating surface to be too uneven. Generally speaking, the convexity of the aluminum flower should be less than or equal to 0.8 times the average thickness of the single-sided coating. Preferably, the convexity of the aluminum flower is less than or equal to 0.7 times the average thickness of the single-sided coating. For ease of calculation and explanation, the maximum convexity of the aluminum flower should not exceed 40μm.

[0109] The five points that make up the first pentagon are (2, 3), (150, 3), (350, 7), (350, 35), and (2, 35). Each point is the area of ​​the aluminum flower (mm 2 ) and the aluminum flower convexity (μm). Taking the coordinate point (2, 3) as an example, it is expressed as the aluminum flower area (mm 2 ) is 2, and the aluminum flower convexity (μm) is 3.

[0110] The nominal thickness of the aluminum silicon coating is 10-20 μm, and the corresponding aluminum flower meets the aluminum flower area (mm 2) and the aluminum flower convexity (μm) form a coordinate point within the first pentagon. Under this condition, the continuity of the first Al-rich intermetallic compound layer of the hot-formed part can be reduced, and it is easier to generate a structure of a double Al-rich intermetallic compound layer, thereby improving the coating toughness and environmental tolerance of the hot-formed component, reducing its crack sensitivity, and making the hot-formed component also have the advantages of improved hydrogen embrittlement resistance and corrosion resistance.

[0111] In other embodiments, the nominal thickness of the aluminum silicon coating is 19 to 33 μm, and the aluminum flower satisfies the aluminum flower area (mm 2 ) and the aluminum flower convexity (μm) form a coordinate point located within a second pentagon, wherein the second pentagon is surrounded by five points: (4, 5), (170, 5), (400, 12), (400, 40), and (4, 40).

[0112] The definition of the five points constituting the second pentagon is the same as that of the five points constituting the first pentagon, and will not be repeated here. The nominal thickness of the aluminum silicon coating is 19 to 33 μm, and the corresponding aluminum flower meets the aluminum flower area (mm 2 ) and the aluminum flower convexity (μm) form a coordinate point within the second pentagon. Under this condition, the continuity of the first Al-rich intermetallic compound layer of the hot-formed part can be reduced, and it is easier to generate a structure of a double Al-rich intermetallic compound layer, thereby improving the coating toughness and environmental tolerance of the hot-formed component, reducing its crack sensitivity, and making the hot-formed component also have the advantages of improved hydrogen embrittlement resistance and corrosion resistance.

[0113] In some embodiments, the aluminum silicon coating includes aluminum flowers. The nominal thickness of the aluminum silicon coating is 10 to 20 μm, and the aluminum flowers satisfy the condition that the coordinate points formed by the aluminum flower boundary length per unit area (1 / mm) and the aluminum flower convexity (μm) are located within a third pentagon, and the third pentagon is surrounded by five points: (0.1, 7), (0.17, 3), (10, 3), (10, 35), and (0.1, 35).

[0114] Since hydrogen invasion is easier at the grain boundaries of aluminum flowers, a more rigorous approach is to control the cumulative length of the grain boundaries per unit area, rather than the area of ​​the aluminum flowers, let alone the simple aluminum flower length and width parameters in traditional technology. However, the present invention can obtain aluminum flowers that are close to equiaxed. An equiaxed aluminum flower means that the lengths of the sides of the aluminum flowers in all directions are close to equal, that is, the aluminum flowers are isotropic and the overall contour is approximately circular. That is, under the condition of the same area, the circumference of the equiaxed aluminum flower is smaller than that of the non-equiaxed aluminum flower (such as the difference between the lengths of the sides is large, such as aluminum flowers with an overall contour that is approximately rectangular).

[0115] Therefore, compared with the traditional aluminum plating technology, the cumulative border length of the aluminum flower of the present invention has been greatly reduced. Even when the aluminum flower area is small, the total border length of the aluminum flower is smaller than that of the aluminum plate produced by the uncontrolled traditional technology. Therefore, the aluminum flower convexity (μm) and the aluminum flower border length (mm) are the key technologies to determine the material performance of the present invention. Since the aluminum flower border length is not easy to measure, and the aluminum flower shape of the present invention is basically close to the equiaxial shape, the aluminum flower shape is highly stable, so the relationship between the aluminum flower area and the aluminum flower convexity can be used instead of the aluminum flower convexity and aluminum flower border length requirements.

[0116] After research, it is found that this alternative measurement scheme is effective in the present invention. For the traditional production process, even if the average area of ​​the aluminum flower is within the required range of the present invention, the shape of the aluminum flower is not controlled, which will cause the cumulative length of the aluminum flower boundary per unit area to exceed the requirements of the present invention. The present invention also provides the relationship between the aluminum flower convexity and the aluminum flower boundary length per unit area.

[0117] Therefore, in this embodiment, (1) when the nominal thickness of the single-sided coating is 10 to 20 μm, the aluminum flower boundary length per unit area (1 / mm) and the aluminum flower convexity (μm) should be within the pentagon formed by the five points (0.1, 7), (0.17, 3), (10, 3), (10, 35), and (0.1, 35).

[0118] In some embodiments, the nominal thickness of the aluminum-silicon coating is 19 to 33 μm, and the aluminum flower satisfies the condition that the coordinate points formed by the aluminum flower boundary length per unit area (1 / mm) and the aluminum flower convexity (μm) are located within the fourth pentagon, and the fourth pentagon is surrounded by five points: (0.08, 12), (0.16, 5), (8, 5), (8, 40), and (0.08, 40).

[0119] (2) The aluminum flower boundary length per unit area (1 / mm) and the aluminum flower convexity (μm) should be within the pentagon surrounded by the five points (0.08, 12), (0.16, 5), (8, 5), (8, 40), and (0.08, 40).

[0120] The convexity of the plated aluminum flower in the actual delivery state may be affected by skin finishing and straightening, and the convexity will be reduced. However, this will not have a serious adverse effect on the distribution of Al-Si and Al-Si-Fe in the coating.

[0121] Since the aluminum flowers prepared in the embodiment of the present application are close to equiaxed shapes, the aluminum flower area defined in the present invention, i.e., the average area of ​​aluminum flowers on the surface of the coating, is more conducive to the technical requirements of the present invention than the prior art. Therefore, in some embodiments, the aluminum flower area is measured by the following method:

[0122] (1) Take a 300mm×300mm sample at the 1 / 4 width of the steel plate;

[0123] (2) Draw three 100 mm long straight lines in the horizontal and vertical directions on the upper and lower surfaces of the sample, with the interval between the straight lines greater than 50 mm;

[0124] (3) Count the number of aluminum flowers on each line respectively, take the average number a for the horizontal aluminum flowers, and take the average number b for the vertical aluminum flowers;

[0125] (4) Calculate the area S of the aluminum flower, S = 100 × 100 / (a × b).

[0126] Note: The above sampling positions are only representative samples. If the strip size does not meet the requirements, the sampling position and line drawing position can be adjusted, but the evaluation area is generally not less than 90000mm 2 .

[0127] The present application discloses a method for preparing aluminum-plated silicon steel, comprising the following steps:

[0128] S100: After annealing the steel substrate to be plated, immersion plating is performed in a plating solution to obtain an immersion-plated steel substrate. In terms of mass percentage, the immersion plating solution includes: Si: 8-11%, Fe: 1-4%, and the rest is Al and unavoidable impurities.

[0129] The steel substrate to be plated (i.e., strip steel) used for hot-dip plating includes hot-rolled strip steel and cold-rolled strip steel with a thickness of 0.5 to 3.5 mm.

[0130] The plating solution is usually placed in an aluminum pot. The composition of the plating solution can also be expressed by the composition of the aluminum pot. That is, the composition of the aluminum pot: Si: 8-11%; Fe: 1-4%; the rest is Al and unavoidable impurities.

[0131] After annealing, the steel substrate to be plated enters the aluminum pot, and the temperature of the steel substrate entering the aluminum pot is the pot entry temperature. In some embodiments, the temperature of the annealed steel substrate entering the immersion bath is 600-700°C, that is, the steel strip entering the pot temperature is 600-700°C.

[0132] S200: Cooling the dip-plated steel substrate to 570°C to 650°C at a rate of 2 to 20°C / s, and maintaining the temperature at 570°C to 650°C for 1 to 20 seconds to obtain primary cold dip-plated steel.

[0133] In order to achieve the above-mentioned Al-Si phase and Al-Si-Fe phase requirements and coating uniformity requirements, the present invention adopts a method of controlling cooling of the coating and applying deformation to the coating, namely, the first cooling stage of step S200 and the second cooling stage of step S300.

[0134] In order to achieve the above-mentioned Al-Si phase and Al-Si-Fe phase requirements, the strip is cooled with air after hot dip coating, and the average cooling rate of the strip is controlled to be ≤50°C / s in the range from the aluminum pot to 300°C. Preferably, the average rate is 2 to 25°C / s. Preferably, the average rate of the coating from the aluminum pot to 570°C (first stage cooling) is 2 to 20°C / s. The average rate of the coating from 570°C to 300°C (second stage cooling) is 5 to 25°C / s. Controlled cooling helps the precipitation of the above-mentioned partial Al-Si phase and Al-Si-Fe phase.

[0135] In the first stage of cooling, the general holding temperature range is 570℃~650℃, and the holding time is 1~20 seconds. The heat preservation box can also be replaced by a heat insulation board. When using a heat insulation board, it should be set on both sides of the upper and lower surfaces of the coating. The heat preservation measures help to prolong the time that the coating of the strip stays in the high temperature zone, maintain the surface tension of the aluminum flower, and thus improve the convexity of the aluminum flower after the coating solidifies.

[0136] S300: The primary cold-dip plated steel is placed in a temperature regulating device and, under the condition of heated gas, is continuously cooled to 300°C at an average cooling rate of 5-25°C / s, and the holding time is 2-30 seconds to obtain a secondary cold-dip plated steel. The temperature of the temperature regulating device is 300°C to 570°C. The temperature of the heated gas is ≥100°C, and the total suspended particulate matter in the gas is ≤0.2mg / m3.

[0137] In order to obtain the aluminum flower convexity and aluminum flower area required by the present invention, the cooling rate should be avoided to be too high, and the cooling rate of the second section should be less than or equal to 15°C / s. The cooling section can be provided with a temperature regulating device, and its insulation temperature is 300°C to 570°C, and the insulation time is 2 to 30 seconds. Preferably, the insulation temperature is 300°C to 570°C, and the insulation time is 5 to 20 seconds.

[0138] Cooling, heat preservation and other measures may not meet the requirements for aluminum flower growth. In order to meet the requirements for aluminum flower area and convexity, the cooling section of the present invention is provided with a gas heating device. The gas temperature during heating is ≥300°C, the temperature range of the strip steel during heating is 300°C to 650°C, and the heating rate of the strip steel needs to be controlled at 0 to 25°C / s. The total suspended particulate matter (TSP) in the gas is ≤0.2mg / cubic meter. The purpose of controlling the upper limit of TSP is to reduce the particulate matter in the gas, which may become aluminum flower points, thereby increasing the aluminum flowers and increasing the aluminum flower boundary length per unit area.

[0139] The inventors have deeply analyzed the effect of the phase change heat release of the material on the aluminum flower. When the material releases heat during the cooling process, it has the effect of maintaining the temperature of the strip, which is beneficial to the growth of the aluminum flower, especially to the Al-Si and Al-Si-Fe phases satisfying the dispersion index of the present invention. Therefore, the energy applied by the above-mentioned insulation can be appropriately reduced, that is, the heating gas temperature in the cooling section can be appropriately reduced. Generally speaking, when the composition meets C: 0.18-0.45%, Mn: 0.3-3.0%, B: 0.0008-0.005%, and the annealing insulation temperature is ≥730, and the insulation time is ≥1 minute, there is a phase change heat release effect in the cooling process after plating, and the gas temperature during heating in the cooling section can be appropriately reduced, such as controlling the upper limit of the gas temperature, that is, ≤650℃. Furthermore, C: 0.28-0.45%, Mn: 0.3-3.0%, B: 0.0008-0.005%, the annealing holding temperature is ≥730, the holding time is ≥1 minute, and the gas temperature during heating implemented in the cooling section is 640°C.

[0140] When a certain amount of Cr, Ni, V, and Mo is added to the strip, the temperature range of heat release tends to decrease, and the auxiliary heating of the heating gas should be advanced to prevent the phase change heat release time from being delayed and affecting the growth of aluminum flowers. Specifically, when the strip meets C: 0.18-0.45%, Mn: 0.3-3.0%, B: 0.0008-0.005%, Cr: 0.1-0.5%, the annealing holding temperature is ≥730, the holding time is ≥1 minute, and the temperature of the strip gas heating in the cooling stage is ≥305℃. Further, when the strip meets C: 0.18-0.45%, Mn: 0.3-3.0%, B: 0.0008-0.005%, Cr: 0.1-0.5%; Ni+V+Mo: 0.1-1.5%, the annealing holding temperature is ≥730, the holding time is ≥1 minute, and the temperature of the strip gas heating in the cooling stage is ≥310℃. Furthermore, when the strip satisfies C: 0.28-0.45%, Mn: 0.3-3.0%, B: 0.0008-0.005%, Cr: 0.1-0.5%; Ni+V+Mo: 0.1-1.5%, and two of the three elements Ni, V, and Mo simultaneously meet ≥0.1%, the annealing holding temperature is ≥730, the holding time is ≥1 minute, and the temperature of the strip during gas heating in the cooling stage is ≥315°C.

[0141] S400: Cooling the second cold-dip plated steel to room temperature to obtain pre-coated plated steel.

[0142] In this step, the steel strip may be cooled from 300°C to room temperature using air and / or water.

[0143] In some embodiments, the dip-plated steel substrate is cooled to 570° C. at a rate of 2 to 15° C. / s, and maintained at 570° C. for 1 to 10 seconds to obtain the initially cold-dip-plated steel.

[0144] In some embodiments, the primary cold-dip plated steel is cooled to 300° C. at an average cooling rate of 5 to 20° C. / s, and the holding time is 2 to 20 seconds to obtain the secondary cold-dip plated steel.

[0145] In some embodiments, the annealing temperature in the step of annealing the steel substrate to be plated is 700-850° C., and the annealing time is 1-20 minutes.

[0146] The cold-rolled strip is annealed at a temperature of 700-880°C for 1-20 minutes. Preferably, the annealing temperature is 700-850°C for 3-15 minutes. For the hot-rolled strip that has not been cold-rolled, the annealing temperature of the strip may be lower than 700°C.

[0147] In some embodiments, between step S100 and step S200, a process is further performed to remove excess plating solution from the surface by blowing (e.g., using a nozzle blowing system, i.e., an air knife) to obtain a steel strip having an average pre-plating thickness (single side) of 10 μm to 33 μm. Preferably, the average plating thickness of the pre-plated steel strip is 19 μm to 33 μm.

[0148] In some embodiments, after the excess plating solution on the surface is purged and removed, the method further includes applying at least an alternating magnetic field to the coating in a liquid state, wherein the frequency of the alternating magnetic field is ≥ 1 Hz.

[0149] The present invention needs to control the grain distribution direction of the Al-Si-Fe phase in the coating. After the strip gas knife is discharged, at least an alternating magnetic field can be applied to the coating still in a liquid state to control the distribution of the Al-Si-Fe phase. The frequency of the alternating magnetic field is ≥1Hz. The alternating magnetic field also has a stirring effect on the coating, which can prevent the formation of too many unfavorable cast coating grains, and this stirring is conducive to changing the distribution state of the Al-Si phase and the Al-Si-Fe phase, and improving the dispersion index. Properly increasing the frequency of the alternating magnetic field, such as ≥50Hz, has a more significant electromagnetic stirring effect on the coating.

[0150] The present application also discloses a pre-coated steel, which is obtained by cold rolling and skin-passing aluminum-silicon steel. The pre-coated steel comprises a steel substrate and a skin-pass coating layer arranged on the steel substrate. The skin-pass coating layer is obtained by at least one of cold rolling and skin-passing.

[0151] The polished coating includes an intermediate layer and an aluminum silicon coating. The nominal thickness of the aluminum silicon coating is 10 μm to 33 μm. The aluminum silicon coating contains 5 to 40% of an Al-Si phase and 0.1 to 15% of an Al-Si-Fe phase, and the dispersion index of the Al-Si phase and the Al-Si-Fe phase in the aluminum silicon coating is ≥0.05.

[0152] The mass fraction of silicon in the Al-Si phase is 30-50%. The mass fraction of iron in the Al-Si-Fe phase is 10-35%, and the mass fraction of silicon is 3-15%.

[0153] Pre-coated steel is obtained by cold rolling and skin-passing of aluminum-coated silicon steel. Pre-coated steel also has aluminum flowers. The convexity of the aluminum flowers of pre-coated steel may be affected by skin-passing and straightening, and the convexity will decrease. However, this will not have a serious adverse effect on the distribution of Al-Si and Al-Si-Fe in the coating, which is basically the same as that in aluminum-coated silicon steel. Therefore, the proportion, composition, and area of ​​aluminum flowers of pre-coated steel can refer to aluminum-coated silicon steel, and will not be repeated.

[0154] The application also discloses a hot-formed component, comprising a steel substrate and a component coating, wherein the component coating is produced by mutual diffusion between the steel substrate and the aluminum-silicon pre-coating layer.

[0155] The component coating comprises an interdiffusion layer, a first intermediate layer, a first Al-rich intermetallic compound layer, a second intermediate layer and a second Al-rich intermetallic compound layer stacked in sequence. The interdiffusion layer is located at the innermost side of the component coating.

[0156] The first Al-rich intermetallic compound layer is a discontinuous structure, accounting for ≤80% of the length of the layer. The second Al-rich intermetallic compound layer is a quasi-continuous structure, accounting for ≥20% of the continuous length of the layer.

[0157] In order to more clearly describe the structure of the thermoforming component, a thermoforming component with a more complete structure is taken as an example for explanation, including a coating layer having 6 structural layers. It should be noted that the surface layer is not a necessary structure.

[0158] The component coating after hot forming includes (a) an interdiffusion layer; (b) a first intermediate layer; (c) a first Al-rich intermetallic compound layer; (d) a second intermediate layer; (e) a second Al-rich intermetallic compound layer; and (f) a surface layer.

[0159] in:

[0160] (a) Interdiffusion layer: The thickness is 5 to 18 μm, and the hardness of the layer is HV50g 230 to 420. The layer contains, by weight percentage, 80 to 95% Fe, 4 to 10% Al, and 0 to 5% Si. An intermetallic compound having the same composition as the first Al-rich intermetallic compound layer exists at the interface between the interdiffusion layer and the first intermediate layer.

[0161] (b) First intermediate layer: thickness is 0-25 μm, hardness of the layer is HV50g 800-1000. The layer contains, by weight percentage, 35-47% Fe, 50-61% Al, and 0-2% Si.

[0162] (c) The first Al-rich intermetallic compound layer: the thickness is 0 to 15 μm, and the hardness of the layer is HV50g 450 to 650. The layer contains, by weight percentage, 50 to 70% Fe, 30 to 35% Al, and 2 to 6% Si. The first Al-rich intermetallic compound layer is a discontinuous structure, accounting for ≤80% of the continuous length of the layer. Preferably, the first Al-rich intermetallic compound layer is a discontinuous structure, accounting for 1 to 50% of the continuous length of the layer. In the layer, the Al-rich intermetallic compound should have an uneven coating thickness, and the thinner coating area (coating thickness ≤ 26 μm) is more difficult to form and has poorer continuity. The continuity of the first Al-rich intermetallic compound layer is affected by the heating state, and the heating process should maintain continuous heating rather than setting different heating temperatures in sections. In particular, a set temperature exceeding 940°C should be avoided, and the actual temperature of the component should be avoided from exceeding 950°C. Otherwise, when the insulation time is long enough, the first Al-rich intermetallic compound layer formed under high-temperature insulation will be completely merged by the interdiffusion layer, so that the layer disappears completely.

[0163] The inventors found that the average area of ​​the pre-plated aluminum flowers is ≥16mm 2 When the aluminum flower average area is ≥64mm, it is easy to obtain a large amount of the first Al-rich intermetallic compound layer. 2 At the same time, the coating thickness of the pre-plated strip steel is more than 10μm, the first Al-rich intermetallic compound layer is more continuous, and the Al-rich intermetallic compound accounts for 1-30% of the continuous length of the layer. When the average area of ​​aluminum flowers is ≥64mm 2 At the same time, the coating thickness of the pre-plated strip steel is above 19μm, the first Al-rich intermetallic compound layer is more continuous, and the Al-rich intermetallic compound accounts for 1-50% of the continuous length of the layer. When the maximum area of ​​the aluminum flower is ≥100mm 2, it is easy to obtain a more typical and excellent 6-layer structure of the coating after hot forming. The continuity of the first Al-rich intermetallic compound layer is related to the coating change after hot forming. For example, when the coating thickness after hot forming is less than 26μm, the distance between the first Al-rich intermetallic compound layer and the Al-rich intermetallic compound on the surface of the interdiffusion layer is close, resulting in the first Al-rich intermetallic compound layer almost merging with the interdiffusion layer. In addition, if the thickness of the interdiffusion layer is too large, it will affect the generation of the first Al-rich intermetallic compound layer. For example, when the thickness of the interdiffusion layer is ≥16μm, the first Al-rich intermetallic compound layer almost disappears. The influence of aluminum flowers on the formation of the first Al-rich intermetallic compound layer is mainly affected by the distribution of Al-Si phase and Al-Si-Fe phase in the pre-plating layer. When the aluminum flower increases, it is easier to form more Al-Si phase and Al-Si-Fe phase in the vicinity of the center of the aluminum flower. When the area of ​​the aluminum flower decreases, this aggregation effect decreases, and the double-layer Al-rich intermetallic compound structure effect decreases. The amount of Al-Si phase and Al-Si-Fe phase nucleation required by the present invention has been controlled in the aluminum pot before plating. Then, through the subsequent process of the present invention, the distribution of Al-Si phase and Al-Si-Fe phase gradually meets the requirements of the present invention.

[0164] After hot forming, the present invention should avoid the appearance of too many traditional hot-formed steel 4-layer structures, or fewer structural layers. Because when the number of structural layers is too small, the Al-rich intermetallic compounds on the surface of the interdiffusion layer will thicken. And it cannot meet the requirements of the present invention, further leading to a decrease in the plasticity, toughness and hydrogen embrittlement resistance of the material. However, even if the local existence of the coating in the present invention is inevitably less than 6 layers of structure, that is, the first Al-rich intermetallic compound layer partially disappears, but through the implementation of the technology of the present invention, the plasticity, toughness and hydrogen embrittlement resistance of the material's interdiffusion layer are also improved, and the reason is related to the distribution characteristics of the aluminum flowers, Al-Si phase and Al-Si-Fe phase of the coating. More importantly, the grains in the coating have been refined.

[0165] (d) Second intermediate layer: The second intermediate layer has the same composition as the first intermediate layer. In the area where the first Al-rich intermetallic compound layer has low continuity, the first intermediate layer and the second intermediate layer will fuse together. The smaller the area of ​​the aluminum flower and the thinner the coating, the easier this fusion will occur.

[0166] (e) Second Al-rich intermetallic compound layer: The second Al-rich intermetallic compound layer has the same composition as the first Al-rich intermetallic compound layer and is a quasi-continuous structure, generally accounting for ≥20% of the continuous length of the layer.

[0167] In some embodiments, the continuity is improved, and the Al-rich intermetallic compound occupies a continuous length ratio of ≥50% of the layer. Preferably, the second Al-rich intermetallic compound layer is a quasi-continuous structure, accounting for 50-90% of the continuous length of the layer. The reason why the proportion of the second Al-rich intermetallic compound layer is reduced from the traditional lower limit of 90% to 50% is because a part of the Al-rich intermetallic compound in the coating that was originally used to form the second layer also forms a new first Al-rich intermetallic compound layer. When a part of the second Al-rich intermetallic compound layer is fused with the first Al-rich intermetallic compound layer, the intermetallic compounds in the second Al-rich intermetallic compound layer account for 50-75% of the continuous length of the layer.

[0168] (f) Surface layer: The composition of the surface layer is almost the same as that of the first intermediate layer and the second intermediate layer. The layer contains, by weight percentage, 35-47% Fe, 50-61% Al, and 0-2% Si. This layer also contains less than 30% Al-rich intermetallic compounds. Generally, the Al-rich intermetallic compounds are between 2% and 15%. The Al-rich intermetallic compounds in this layer contain, by weight percentage, 50-70% Fe, 30-35% Al, and 2-6% Si. There may also be a pure aluminum or aluminum oxide layer with a continuity of ≥90% on the outer surface of the surface layer. Therefore, after subdividing the surface layer, the surface layer can be divided into 3 or even more levels. For ease of explanation, the present invention is consistent with the traditional aluminum-silicon hot-formed steel and is collectively referred to as the surface layer.

[0169] It should be noted that there is a continuous Al-rich intermetallic compound layer at the interface between the interdiffusion layer and the first intermediate layer, and the composition of the layer is the same as or similar to that of the first Al-rich intermetallic compound layer and the second layer.

[0170] More critically, the coating of the present invention with a 6-layer structure after hot forming has finer grains and more grain boundaries in the coating. After hot forming, more grain boundaries in the coating are conducive to the diffusion of hydrogen in the steel matrix through the grain boundaries, and at the same time, the discontinuous Al-rich intermetallic compound layer reduces the blocking effect on the matrix, thereby alleviating the risk of hydrogen embrittlement of the material. The refinement of the grains in the coating is related to the distribution of Al-Si phase and Al-Si-Fe phase in the coating before hot forming. When the dispersion index requirements of the present invention are met, during the hot forming heating process, the Al-Si phase and Al-Si-Fe phase easily hinder the growth of the coating grains, which helps to refine the grains of the middle layer. As a result, the Al-rich intermetallic compounds of the first and second layers formed after hot forming separate the first and second middle layers, making the grains finer, further improving the toughness of the coating, reducing crack sensitivity, and improving the environmental tolerance of the coating. It also has the advantages of improving hydrogen embrittlement resistance and corrosion resistance.

[0171] In some embodiments, the grain size of the first intermediate layer, the second intermediate layer, and the surface layer of the present invention is generally less than or equal to 30 μm; preferably, the grain size of the intermediate layer can be less than or equal to 25 μm; preferably, the grain size of the first intermediate layer, the second intermediate layer, and the surface layer can be less than or equal to 20 μm. More preferably, the grain size of the first intermediate layer, the second intermediate layer, and the surface layer can be less than or equal to 15 μm.

[0172] However, conventional hot-formed steel does not have the distribution characteristics of the Al-Si phase and Al-Si-Fe phase of the present invention. The intermediate layer of the coating after hot forming has coarse grains and few grain boundaries. In addition, the Al-rich intermetallic compound is basically continuous and has high continuity, which is not conducive to the diffusion of hydrogen in the environment. It has a high blocking effect on the diffusion of hydrogen and is more sensitive to hydrogen embrittlement. At the same time, the coarse coating grains, basically continuous intermediate layer, and Al-rich intermetallic compound layer of conventional hot-formed steel make the coating more brittle.

[0173] It should be noted that by adjusting the hot forming process, the thickness of the interdiffusion layer can be changed, thereby reducing the thickness of the intermediate layer, so that the coating has less than 6 layers. However, the presence of a double-layer Al-rich intermetallic compound layer in the coating also meets the requirements of the double-layer Al-rich intermetallic compound layer of the present invention.

[0174] The coating structure after hot forming of the present invention can be detected and observed by metallographic method. The hot formed sample is cut into samples of about 10mm×20mm, and the 20mm side length is perpendicular to the rolling direction, which is the rolling direction of the strip steel substrate during cold rolling. The observation surface is a 20mm coating section. The sample is carefully polished to ensure that the surface layer is not damaged. The sample is soaked in 4% nitric acid alcohol for a certain time, such as 20 seconds, and the structural characteristics of the coating can be displayed under an optical microscope. Taking a 1.0mm sample as an example, 50 samples are cumulatively tested, and the distance between each point is at least 50mm, that is, try to avoid taking more than one sample continuously within a radius of 50mm on the component for testing. Calculated by observing a 20mm coating section for each sample, that is, the total cumulative coating section length observed under a microscope for at least 50 samples should be ≥1000mm. Sampling at the edge of the component should be avoided as much as possible. When the component is large enough, the position of the sample detection should be ≥50mm away from the edge. When the component size is not enough, try to get as close to the middle of the component, or use multiple components for verification. Among these samples, there is at least one sample in which one field of view (1000 times) has a double-layer Al-rich intermetallic compound layer of the present invention, that is, it shows the 6-layer structural characteristics of the present invention. However, when the cumulative total length required for detection is not reached (the cumulative length is the cross-sectional length of the coating observed under a microscope for at least 50 samples with a total cumulative length of ≥1000mm), it is discovered in advance that there is such a Figure 3If the 6-layer structural characteristics are present, it can be considered that the material after hot forming also meets the structural requirements of the present invention. Generally, 50 samples are cumulatively tested (the cumulative length is the length of the coating cross section observed for at least 50 samples under a microscope, which is ≥1000mm), the distance between each point is at least 50mm, and there are at least 5 samples, each of which has a double-layer Al-rich intermetallic compound layer in one field of view (1000 times) of the present invention. Preferably, 50 samples are cumulatively tested, the distance between each point is at least 50mm, and there are at least 10 samples, each of which has a double-layer Al-rich intermetallic compound layer in one field of view (1000 times) of the present invention.

[0175] Since the detection range of optical microscope is very small, it is not convenient to effectively reflect the actual structural characteristics of the coating. GDOES (glow discharge spectrometer) can be used to perform layered analysis on the coating after hot forming. The structural characteristics of the coating can be obtained from the distribution of Al, Si and Fe contents in the coating. Fig.13 is the Si concentration distribution characteristic of the coating of the component of the present invention after hot forming, Fig.14 It is the Si concentration distribution characteristic of the coating of traditional components after hot forming.

[0176] like Fig.13 , find a valley value with the lowest Si concentration from the surface to the steel matrix, and near the bottom of the valley, common tangent line 1 and common tangent line 2 can be drawn to the left and right of the curve respectively. Peaks 1, 2, 3 and 4 far from the common tangent lines can be found above these two common tangent lines. There is a peak of Si concentration of surface oxidation in the range of about 0 to 0.2 μm from the surface, and this peak is not one of the four peaks mentioned. These peaks refer to the peaks of the difference between the common tangent lines on the Y axis, that is, the peaks formed by subtracting the common tangent concentration value of the common tangent area from the detected concentration. The lowest valley value is generally the second valley value, but it may also be the first or third valley value. Similarly, common tangent line 1 and common tangent line 2 can be drawn to the left and right of the curve near the bottom of the second valley, and peaks 1, 2, 3 and 4 relative to the distance between the common tangent lines can be found above each oblique line.

[0177] The third peak may be affected by the structural stability and is not significant. It can be measured by increasing the sampling area of ​​GDOES. Taking a sample with a material thickness of 1.0 mm as an example, when the single sampling diameter of GDOES is 4 mm, 100 sampling points are cumulatively tested, and the distance between each point is at least 50 mm, that is, try to avoid taking more than one sample continuously within a radius of 50 mm for GDOES testing. The area of ​​each test point is 12.56 mm 2 Calculation, that is, for at least the 100 samples, the total cumulative detection area is ≥ 1256mm 2. Sampling at the edge of the component should be avoided as much as possible. When the component is large enough, the position of the sample detection should be ≥50mm away from the edge; when the component size is not enough, try to get close to the middle of the component, or use multiple components for verification. There is at least one sampling point that has the above-mentioned peak 1, peak 2, peak 3 and peak 4 characteristics of the present invention. Generally, when the single sampling diameter of GDOES is 4mm, 100 sampling points are cumulatively detected, and the distance between each point is at least 50mm. There are at least 5 sampling points that have the above-mentioned peak 1, peak 2, peak 3 and peak 4 characteristics of the present invention. Preferably, when the single sampling diameter of GDOES is 4mm, 100 sampling points are cumulatively detected, and the distance between each point is at least 50mm. There are at least 10 sampling points that have the above-mentioned peak 1, peak 2, peak 3 and peak 4 characteristics of the present invention. Preferably, when the single sampling diameter of GDOES is 4 mm, 100 sampling points are cumulatively detected, the distance between each point is at least 50 mm, and at least 20 sampling points have the above-mentioned peak 1, peak 2, peak 3 and peak 4 characteristics of the present invention. Further preferably, when the single sampling diameter of GDOES is 4 mm, 100 sampling points are cumulatively detected, the distance between each point is at least 50 mm, and at least 50 sampling points have the above-mentioned peak 1, peak 2, peak 3 and peak 4 characteristics of the present invention.

[0178] like Fig.14 , a valley with the lowest Si concentration is found from the surface to the steel matrix, and a common tangent line 1 can be drawn to the left of the curve near the bottom of the valley. However, when looking for a tangent point to the right near the bottom of the valley, no other significant tangent point can be found except for the tangent point near the interface between the coating and the substrate. Therefore, only peaks 1, 2, and 3 far away from the common tangent line can be found above this common tangent line 1. There is a peak of Si concentration of surface oxidation in the range of about 0 to 0.2 μm from the surface, and this peak is not one of the three peaks mentioned. The lowest valley is generally the second valley, or it may be the first valley. Similarly, a common tangent line can be drawn to the right of the curve near the bottom of the valley, and peaks 1, 2, and 3 can be found. In terms of microstructure, from outside to inside, peak 1 corresponds to Al-rich intermetallic compounds in the surface layer, peak 2 corresponds to the Al-rich intermetallic compound layer, and peak 3 corresponds to Al-rich intermetallic compounds between the interdiffusion layer and the intermediate layer (i.e., the surface of the interdiffusion layer).

[0179] When using GDOES testing, the cumulative testing area should generally be ≥1000mm 2 That is, when the single sampling diameter of GDOES is 4mm, the cumulative detection exceeds 100 sampling points, and the distance between each point is at least 50mm, which can meet the detection requirements. However, when the cumulative total area required for detection is not reached, it is found in advance that there are Fig.13If the 4 Si peaks are characteristic, it can be considered that the material after hot forming also meets the structural requirements of the present invention.

[0180] The present invention has at least four Si concentration peaks, namely, peak 1, peak 2, peak 3 and peak 4. From the outside to the inside in the microstructure, peak 1 corresponds to the Al-rich intermetallic compound in the surface layer, peak 2 corresponds to the second layer of the Al-rich intermetallic compound, peak 3 corresponds to the first layer of the Al-rich intermetallic compound, and peak 4 corresponds to the Al-rich intermetallic compound between the interdiffusion layer and the first intermediate layer (i.e., the surface of the interdiffusion layer). There is a surface oxidized Si concentration peak within a range of about 0 to 0.2 μm from the surface, and this peak is not one of the four peaks. It can be seen that peaks 2 and 3 (double-layer Al-rich intermetallic compound layer) of the present invention replace the traditional single-layer Al-rich intermetallic compound layer, reduce the segregation of Si concentration inside the coating, improve the toughness of the coating and improve the crack sensitivity of the steel substrate, and further improve the bending performance of the material. On the other hand, the double-layer Al-rich intermetallic compound layer containing a high Si concentration not only refines the coating grains, but also has the ability to block the entry of hydrogen elements, further improving the material's resistance to hydrogen embrittlement. This is because during the hot forming process, the fine coating grains and the double-layer Al-rich intermetallic compound layer with high Si concentration are not conducive to the diffusion of external hydrogen into the steel matrix. The traditional single-layer Al-rich intermetallic compound not only causes the coating grains to coarsen, but also the single-layer structure cannot prevent hydrogen from diffusing into the steel matrix.

[0181] For the surface layer after hot forming, the present invention has the effect of migrating the Al-rich intermetallic compounds in the surface layer inward, so that the amount of Al-rich intermetallic compounds exposed or close to the surface is reduced. Fig.13 and Fig.14It can be seen that the Si concentration peak 1 in the coating after hot forming of the present invention is at a distance of 1.50 μm from the surface, while the Si concentration peak 1 in the coating after traditional hot forming is about 0.25 μm from the surface. This change can significantly improve the structural density of the coating surface, which is beneficial to improving the toughness and hydrogen immersion resistance of the coating. Obviously, this dense coating structure is also beneficial to improving the environmental corrosion resistance of the coating after hot forming, because after the Al-rich intermetallic compounds in the surface layer of the present invention migrate inward, fewer Al-rich intermetallic compounds remain on the surface, thereby reducing the number of effective galvanic cells formed by the Al-rich intermetallic compounds and the nearby coating, and reducing the reaction rate of the coating in the environment. In the neutral salt spray test, the present invention has better corrosion resistance than traditional coatings. Generally, the first peak (peak 1) of the Si concentration in the coating of the present invention is at a distance of ≥0.25 μm from the surface. Preferably, the first peak (peak 1) of the Si concentration in the coating of the present invention is at a distance of ≥0.45 μm from the surface. Preferably, the first peak (peak 1) of Si concentration in the coating of the present invention is at a distance of ≥0.75 μm from the surface. Another method for calculating the peak concentration is to obtain peak size data by deducting the background, which can be operated using relevant software (such as Origin). After obtaining the background curve, the required peak curve can be obtained by subtracting the background curve from the original data. This method can effectively evaluate the impact of the peak situation on material properties. For the convenience of calculation, the background curve of the present invention is the common tangent 1 and the common tangent 2 cut below the Si concentration curve of the coating. It should be noted that after deducting the background, there is a tiny false peak at the depth of the lowest valley. The peak is caused by the calculation method and appears after the intersection of the two common tangents deviates from the lowest valley. The false peak value should be removed and not considered. Generally, when the peak value after deducting the background reaches more than 4, and when the minimum peak concentration value is ≥0.01%, the segregation of Si in the coating can be alleviated, the coating toughness and hydrogen intrusion resistance of the material can be improved, and the corrosion resistance of the coating can be significantly improved. Preferably, after deducting the background, the number of peaks reaches more than 4, and the minimum peak concentration value is ≥ 0.025%. Preferably, after deducting the background, the number of peaks reaches more than 4, and the minimum peak concentration value is ≥ 0.05%, which can effectively improve the bending and hydrogen intrusion resistance of the material. Further preferably, after deducting the background, the number of peaks reaches more than 4, and the minimum peak concentration value is ≥ 0.25%, which can significantly improve the bending and hydrogen intrusion resistance of the material. Due to the errors between the precision of each detection equipment, there will be differences in the test results, but when the equipment accuracy is sufficient, the number of peaks will not change.

[0182] When the coating thickness before hot forming is lower than 19 μm, it becomes more difficult to form the double-layer Al-rich intermetallic compound layer of the present invention in terms of process control, and the thickness of each layer is significantly reduced, and the ability to resist hydrogen intrusion is reduced. These are one of the reasons why the present invention recommends a pre-plating layer of more than 19 μm.

[0183] By reducing the coating thickness, the surface layer thickness can be removed or reduced, or the continuity of the surface layer can be reduced, so that the coating has a 5-layer structure. However, the coating still has a double-layer intermediate layer and a double-layer Al-rich intermetallic compound layer of the present invention, which also meets the requirements of the double-layer Al-rich intermetallic compound layer of the present invention.

[0184] Preferably, the first Al-rich intermetallic compound layer accounts for 1-50% of the length of the layer. The second Al-rich intermetallic compound layer accounts for ≥50% of the continuous length of the layer. More preferably, the second Al-rich intermetallic compound layer accounts for 50-90% of the continuous length of the layer.

[0185] In some embodiments, the component coating further includes a surface layer located outside the second Al-rich intermetallic compound layer.

[0186] In some embodiments, the grain size of the first intermediate layer, the second intermediate layer, and the surface layer is less than or equal to 30 μm. Preferably, the grain size of the first intermediate layer, the second intermediate layer, and the surface layer is less than or equal to 25 μm. More preferably, the grain size of the first intermediate layer, the second intermediate layer, and the surface layer is less than or equal to 15 μm.

[0187] In some embodiments, the total thickness of the component coating is 5 μm to 60 μm. Preferably, the total thickness of the component coating is 20 μm to 55 μm. Preferably, the total thickness of the component coating is 26 μm to 50 μm. Further preferably, the total thickness of the component coating is 30 μm to 50 μm.

[0188] The present invention also discloses a production process of a thermoforming component, comprising the following steps:

[0189] The aluminum-silicon-plated steel or the pre-coated steel is heated to the austenite range, the holding temperature range is 880-950°C, the holding time is 3-15 minutes. The heating atmosphere is air, and the dew point is ≤0°C.

[0190] The steel plate after insulation is cooled, and the heated steel plate is taken out and deformed by pressing with a mold within 10 seconds, and cooled to below 200°C at the same time.

[0191] Specifically, the pre-plated steel sheet is heated to the austenite range, the holding temperature range is 880-950°C, and the holding time is 3-15 minutes. The austenitizing furnace is filled with air, and the dew point in the austenitizing furnace is ≤0°C. The steel sheet after holding is cooled, and the time between taking out the heated steel sheet from the furnace and transferring it to the punching machine is ≤10 seconds, and then the die is used to press and deform it, and it is cooled to below 200°C at the same time.

[0192] During the hot forming process, the aluminum flowers on the surface of the pre-plated layer will decompose, oxidize and restructure, and alloying will occur inside the plating layer. However, the average visible area of ​​the surface of the component after hot forming is ≥16mm 2 The aluminum flower pattern is usually called "fish scale pattern". The finishing process (also called flattening) after hot-dip plating has a certain effect on the clarity of the aluminum flowers after hot forming. When the finishing elongation increases, the recognition of the aluminum flowers after hot forming decreases. Similarly, the mold pressure in the hot forming process has a great influence on the clarity of the aluminum flowers after hot forming. When the pressure increases, the recognition of the aluminum flowers decreases. The surface where the component after hot forming contacts the lower stamping die is also not suitable for identifying aluminum flowers. However, after polishing the surface with sandpaper (such as a specification of 1200 mesh), the pattern left by the aluminum flowers after hot forming can be seen. Or adjust the light source parameters for easy observation.

[0193] The total coating thickness of the component after thermoforming is 5 μm to 60 μm. Preferably, the total coating thickness of the component after thermoforming is 20 μm to 55 μm. Preferably, the total coating thickness of the component after thermoforming is 26 μm to 50 μm. Further preferably, the total coating thickness of the component after thermoforming is 30 μm to 50 μm.

[0194] The invention also discloses a motor vehicle, comprising the above-mentioned hot-formed component.

[0195] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0196] Example 1

[0197] The steel substrate to be plated is provided with the following chemical composition and material thickness of 1.5 mm.

[0198] Table 1 Chemical composition of the steel substrate to be plated, by weight %

[0199] C Si Mn P S Al B Cr Ti Nb N 0.36 0.49 1.09 0.012 0.0003 0.034 0.0033 0.33 0.018 0.022 0.0051

[0200] The steel substrate to be plated in Table 1 is cleaned and dried, and then heated to a desired annealing temperature for insulation, which in this embodiment is 800° C. for 10 minutes.

[0201] The steel substrate to be plated in Table 1 is cooled, and the temperature of the steel substrate to be plated is controlled between 600 and 700° C. before entering the aluminum pot, and is 660° C. in this embodiment.

[0202] The aluminum pot has the following composition mass fractions: Si: 8-11%; Fe: 1-4%; the rest is Al and inevitable impurities. The aluminum pot in this embodiment has a Si content of 10%, an Fe content of 1.5%, and the rest is Al and inevitable impurities.

[0203] After hot-dip plating of the steel substrate to be plated, an air knife (a known technology) is used to remove excess plating solution to obtain a pre-plated steel strip, the plating layer of the steel strip (the plating layer before hot forming is called the pre-plating layer) having a thickness of 25 μm.

[0204] The cooling of the strip after hot-dip aluminum silicon coating is divided into two stages. The first stage of cooling is implemented after the strip coating control is completed until it is cooled to 570°C. The second stage of cooling is implemented from 570°C to 300°C. The cooling rate is shown in Table 2. The third stage of cooling: the strip is cooled from 300°C to room temperature using air and / or water.

[0205] The Al-Si phase and Al-Si-Fe phase of the steel coils numbered 1 to 5 are relatively coarse and have a high dispersion index. The aluminum-silicon coating should contain 20 to 40% of the Al-Si phase, which includes Al n Si m Phase. Where n:m=(1.0~3.0):1. The Al n Si m The proportion of the Al-Si phase in the Al-Si phase is ≥50%. The Al-Si-Fe phase should contain 5-15% of the Al-Si-Fe phase. The Al-Si-Fe phase includes Fe a Si b Al c phase; wherein a:b:c=(1~2):1:(4~9); the Fe a Si b Al c The proportion of the phase in the Al-Si-Fe phase is ≥50%.

[0206] The Al-Si phase and Al-Si-Fe phase of the steel coil number 6 to 7 are relatively fine and have a low dispersion index. The aluminum silicon coating should contain 5 to 30% of the Al-Si phase, which includes Al n Si m Phase. Where n:m=(1.0~3.0):1. The Al n Si m The proportion of the Al-Si phase in the Al-Si phase is ≥50%. The Al-Si-Fe phase should contain 0.1-8% of the Al-Si-Fe phase. The Al-Si-Fe phase includes Fe a Si b Al c phase; wherein a:b:c=(1~2):1:(4~9); the Fea Si b Al c The proportion of the phase in the Al-Si-Fe phase is ≥50%.

[0207] The Al-Si phase and Al-Si-Fe phase of the steel coil number 8 to 10 are extremely fine, with a low dispersion index and difficult to evaluate. The aluminum-silicon coating should contain a fine Al-Si phase ratio of ≤5%, or these fine Al-Si phases are not valid evaluation objects. The aluminum-silicon coating should contain very little Al-Si-Fe, and these fine Al-Si phases are not valid evaluation objects.

[0208] Table 2 Coating cooling rate and aluminum flower area

[0209]

[0210] like Figure 1 This is a typical surface aluminum flower morphology. Figure 2 This is a typical surface aluminum flower trace morphology after hot forming. Fig.11 Aluminum flower area ≥ 200mm 2 , (200~400mm 2 ); Fig.12 Aluminum flower area ≤ 9mm 2 (4~9mm 2 ).

[0211] The aluminum flower area and aluminum flower convexity of steel coils No. 8 to 10 are too small, which does not meet the requirements of the present invention. The aluminum flower convexity and aluminum flower area of ​​No. 1 to 7 can meet the requirements of the present invention.

[0212] It can be seen that the first stage of cooling determines the size of the aluminum flower area to a large extent. The greater the cooling rate, the smaller the aluminum flower. The second stage also has an impact on the size of the coated aluminum flower. The greater the cooling rate, the smaller the aluminum flower. Compared with the first stage, the cooling rate in the second stage has less effect on the size of the aluminum flower.

[0213] Example 2

[0214] The steel substrate to be plated in Table 1 is cleaned and dried, and then heated to a desired annealing temperature for insulation, which in this embodiment is 800° C. for 10 minutes.

[0215] The steel substrate to be plated in Table 1 provided is cooled, and the temperature of the steel substrate to be plated is controlled to be 660° C. before entering the aluminum pot.

[0216] The aluminum pot of this embodiment has a Si content of 10%, an Fe content of 1.5%, and the remainder being Al and unavoidable impurities.

[0217] After hot-dip plating of the steel substrate to be plated, an air knife is used to remove excess plating solution to obtain a pre-plated steel strip. The thickness of the pre-plated steel strip is controlled according to Table 3.

[0218] The cooling of the strip after hot-dip aluminum silicon coating is divided into two stages. The first stage of cooling is implemented after the strip coating control is completed until it cools to 570℃, and the cooling rate is 10℃ / s. The second stage of cooling is implemented from 570℃ to 300℃, and the cooling rate is 10℃ / s. The third stage of cooling: the strip is cooled from 300℃ to room temperature using air and / or water.

[0219] Table 3 Pre-plating thickness and aluminum flower area

[0220]

[0221] It can be seen that the coating thickness has a certain influence on the area of ​​aluminum flowers. This is mainly because the thinner the coating, the more nucleation points there are, and the more restricted the growth of aluminum flower dendrites. In general, when the coating thickness is above 10μm, the area of ​​aluminum flowers is ideal; when the coating thickness is above 19μm, the area of ​​aluminum flowers is relatively stable; but when it exceeds 33μm, the growth of aluminum flowers is not obvious.

[0222] Example 3

[0223] The steel substrate to be plated in Table 1 is cleaned and dried, and then heated to a desired annealing temperature for insulation, which in this embodiment is 800° C. for 10 minutes.

[0224] The steel substrate to be plated in Table 1 provided is cooled, and the temperature of the steel substrate to be plated is controlled to be 660° C. before entering the aluminum pot.

[0225] The aluminum pot of this embodiment has a Si content of 10%, an Fe content of 1.5%, and the remainder being Al and unavoidable impurities.

[0226] After hot-dip plating of the steel substrate to be plated, an air knife is used to remove excess plating solution to obtain a pre-plated steel strip. The thickness of the pre-plated steel strip is as shown in Table 4.

[0227] The cooling of the strip after hot-dip aluminum silicon coating is divided into two stages. The first stage of cooling is implemented after the strip coating is completed until it cools to 570°C. The second stage of cooling is implemented from 570°C to 300°C. The third stage of cooling: air and / or water are used to cool the strip from 300°C to room temperature.

[0228] The pre-plated steel plate is heated to the austenite range, the holding range is 900℃, and the holding time is 8 minutes. The austenitizing furnace is filled with air, the dew point in the austenitizing furnace is ≥0℃, and the dew point of each sample is controlled to be the same. A certain amount of hydrogen is introduced into the austenitizing furnace. The steel plate after insulation is cooled, and the time between taking out the heated steel plate from the furnace and transferring it to the punching machine is ≤10 seconds, and then the die is used for pressing, deformation and quenching, and cooled to below 200℃.

[0229] Table 4 The proportion of the first Al-rich intermetallic compound layer in the layer and the performance results obtained with different coating thickness and aluminum flower area

[0230]

[0231]

[0232] Note: In order to obtain the three-point bending angle and four-point bending delayed cracking time of the material, the production process was adjusted in the experiment. It is only used to illustrate the performance improvement of the material by the present invention, and does not represent the final service performance. The final service performance of the material is closely related to the hot forming process. The use of the material of the present invention is helpful to improve the toughness and hydrogen embrittlement resistance of the material.

[0233] It can be seen that the greater the coating thickness, the more conducive it is to obtain the first Al-rich intermetallic compound layer, thereby improving the bending performance and enhancing the ability to resist delayed cracking. The larger the aluminum flower area, the more conducive it is to obtain the first Al-rich intermetallic compound layer, thereby improving the bending performance and enhancing the ability to resist delayed cracking. Plating pressure is conducive to obtaining the first Al-rich intermetallic compound layer, and the ability to resist delayed cracking is also stronger.

[0234] Except for the T1 sample which does not meet the requirements of the first Al-rich intermetallic compound layer of the present invention, the other samples all meet the requirements of the hot forming thickness coating structure. The coating of the components of the other samples after hot forming includes (a) an interdiffusion layer; (b) a first intermediate layer; (c) a first Al-rich intermetallic compound layer; (d) a second intermediate layer; (e) a second Al-rich intermetallic compound layer; and (f) a surface layer.

[0235] The coating structure of the samples was analyzed after hot forming. Figure 3 The coating diagram of T8 after hot forming shows the typical 6-layer structure of the hot forming steel after hot forming of the present invention. Figure 4 This is an illustration of the coating of T9 after hot forming. The coating has a 4-layer structure of the coating after hot forming of traditional hot forming steel.

[0236] The hot-formed T8 and T9 were subjected to 2% tensile deformation and the crack morphology of the coating was observed. Figure 5The figure is a diagram of the coating of T8 that is still deformed after hot forming, and the coating has a double layer of Al-rich intermetallic compound hot forming steel. After deformation, the interdiffusion layer has good plasticity, and the cracks fail to penetrate the interdiffusion layer, but cracks exist in the steel matrix.

[0237] like Figure 6 This is a diagram of the coating of T9 after conventional hot forming and deformation. The coating is a hot-formed steel with only one layer of Al-rich intermetallic compounds. After deformation, the interdiffusion layer is broken, but the steel matrix is ​​intact without cracks.

[0238] Figure 8 The coating structure of the component of the present invention after hot forming is that the double-layer Al-rich intermetallic compound separates the coating, and the grains in the coating are finer, and the average grain size of the fine grains in the coating is less than or equal to 25 μm.

[0239] Fig. 9 It is the coating structure of traditional hot-formed components after hot forming, and the grains in the coating are coarse. The average grain size is greater than or equal to 20μm, especially the grains in the middle layer are coarse, and the maximum cross-sectional size can exceed 30μm. The grains in the middle layer penetrate most of the coating, and this coarse organizational structure has a significant adverse effect on the coating performance.

[0240] Example 4

[0241] The steel substrate to be plated in Table 1 is cleaned and dried, and then heated to a desired annealing temperature for insulation, which in this embodiment is 800° C. for 10 minutes.

[0242] The steel substrate to be plated in Table 1 provided is cooled, and the temperature of the steel substrate to be plated is controlled to be 660° C. before entering the aluminum pot.

[0243] The aluminum pot of this embodiment has a Si content of 10%, an Fe content of 1.5%, and the remainder being Al and unavoidable impurities.

[0244] The method of the present invention is used to prepare materials T14 to T17 with different dispersion indexes of Al-Si and Fe-Al-Si phases in the coating required for the experiment, and a hot forming process is performed on these pre-coated samples. The hot forming process used in this embodiment is to keep the temperature at 930°C for 5 minutes. The austenitizing furnace is filled with air, the dew point in the austenitizing furnace is ≥0°C, the dew point of each sample is controlled to be the same, and a certain amount of hydrogen is introduced into the austenitizing furnace.

[0245] GDOES was used to detect the Si concentration of the coating on the samples, and the required Si concentration peak data was obtained after deducting the background. The coating structure, peak data and related performance results of these materials are shown in Table 5.

[0246] It can be seen that the dispersion index of this embodiment is more conducive to forming the double-layer Al-rich intermetallic compound layer required by the present invention, that is, 4 Si concentration peaks appear. Furthermore, a higher Si concentration peak is conducive to improving the bending angle and delayed cracking resistance of the material.

[0247] The neutral salt spray test method was used to study samples T14 to T17. The results showed that all test samples had slight red rust after 2 hours; after 12 hours, the red rust area of ​​T14 was larger, about 80%; the red rust area of ​​T15 was about 60%, and the red rust area of ​​T16 and T17 was about 50%. After 72 hours of salt spray test, the samples were taken out and dried, and the unit area weight gain data of the samples were measured as shown in Table 5. The unit area weight gain reflects the degree of oxidation of the coating in an oxidizing environment, that is, the weight gain of the coating after obtaining elements such as oxygen. It can be seen that the weight gain caused by oxidation of the samples that meet the four Si concentration peaks of the present invention is significantly lower than that of the samples with three Si concentration peaks. Among them, the higher the minimum Si concentration peak, the smaller the unit area weight gain; when the minimum Si concentration peak exceeds 0.10%, the unit area weight gain is 2.7 mg / cm 2 As shown below, the corrosion resistance of the coating can be significantly improved by having a complete 6-layer structure (4 Si concentration peaks) according to the present invention after hot forming.

[0248] Table 5 Effect of different dispersion indexes on coating and performance

[0249]

[0250]

[0251] The above technical solutions of the present invention are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

[0252] This application discloses the following notes:

[0253] Note 1. An aluminum-silicon-coated steel, characterized in that it comprises a steel substrate and a pre-plating layer arranged on the steel substrate;

[0254] The pre-plating layer includes an intermediate layer and an aluminum silicon coating layer; the nominal thickness of the aluminum silicon coating layer is 10 μm to 33 μm; the aluminum silicon coating layer contains 5 to 40% of an AlSi phase and 0.1 to 15% of an AlSiFe phase, and the dispersion index of the AlSi phase and the AlSiFe phase in the aluminum silicon coating layer is ≥0.05;

[0255] The mass fraction of silicon in the AlSi phase is 30-50%; the mass fraction of iron in the AlSiFe phase is 10-35%, and the mass fraction of silicon is 3-15%.

[0256] Note 2. The aluminum-silicon-coated steel according to Note 1 is characterized in that the aluminum-silicon coating contains 10-30% of AlSi phase and 0.1-10% of AlSiFe phase.

[0257] Note 3. The aluminum-plated silicon steel according to Note 1 is characterized in that the AlSi phase includes an AlnSim phase; wherein n:m=(1.0~3.0):1; and the proportion of the AlnSim phase in the AlSi phase is ≥50%.

[0258] Note 4. The aluminum-plated silicon steel according to Note 1 is characterized in that the AlnSim phase includes at least one of Al4Si3 and Al4Si2.

[0259] Note 5. The aluminum-coated silicon steel according to Note 1 is characterized in that the AlS iFe phase includes Fea Si b Alc phase; wherein a:b:c=(1~2):1:(4~9); the proportion of the Fea Si ib Alc phase in the AlS i-Fe phase is ≥50%.

[0260] Note 6. The aluminum-plated silicon steel according to Note 5 is characterized in that the Fe a S i b Al c The phases include FeS i A l4 phase and Fe2S i A l7 phase.

[0261] Note 7. An aluminum-silicon-plated steel, characterized in that it comprises a steel substrate and a pre-plated layer arranged on the steel substrate; the pre-plated layer comprises an intermediate layer and an aluminum-silicon coating layer;

[0262] The aluminum-silicon coating includes aluminum flowers; the nominal thickness of the aluminum-silicon coating is 10 to 20 μm, and the aluminum flowers satisfy the conditions that the coordinate points formed by the aluminum flower area in mm2 and the aluminum flower convexity in μm are located within the first convex pentagon, and the first convex pentagon is surrounded by five points: (2, 3), (150, 3), (350, 7), (350, 35), and (2, 35).

[0263] Note 8. The aluminum-silicon steel according to Note 7 is characterized in that the aluminum-silicon coating includes aluminum flowers; the nominal thickness of the aluminum-silicon coating is 19 to 33 μm, and the aluminum flowers satisfy the conditions that the coordinate points formed by the aluminum flower area in mm2 and the aluminum flower convexity in μm are located within a second convex pentagon, and the second convex pentagon is surrounded by five points: (4, 5), (170, 5), (400, 12), (400, 40), and (4, 40).

[0264] Note 9. The aluminum-coated silicon steel according to Note 7 is characterized in that the aluminum-silicon coating includes aluminum flowers; the nominal thickness of the aluminum-silicon coating is 10 to 20 μm, and the aluminum flowers satisfy the conditions that the coordinate points formed by the aluminum flower boundary length per unit area in units of 1 / mm and the aluminum flower convexity in units of μm are located within a third convex pentagon, and the third convex pentagon is surrounded by five points: (0.1, 7), (0.17, 3), (10, 3), (10, 35), and (0.1, 35).

[0265] Note 10. The aluminum-coated silicon steel according to Note 7 is characterized in that the aluminum-silicon coating includes aluminum flowers; the nominal thickness of the aluminum-silicon coating is 19 to 33 μm, and the aluminum flowers satisfy the conditions that the coordinate points formed by the aluminum flower boundary length per unit area in units of 1 / mm and the aluminum flower convexity in units of μm are located within the fourth convex pentagon, and the fourth convex pentagon is surrounded by five points: (0.08, 12), (0.16, 5), (8, 5), (8, 40), and (0.08, 40).

[0266] Note 11. A method for preparing aluminum-plated silicon steel, characterized in that it comprises the following steps:

[0267] After annealing the steel substrate to be plated, the substrate is dip-plated in a plating solution to obtain a dip-plated steel substrate; the plating solution comprises, by mass percentage: Si: 8-11%; Fe: 1-4%; the rest is Al and unavoidable impurities;

[0268] Cooling the dip-plated steel substrate to 570°C to 650°C at a rate of 2 to 20°C / s, and maintaining the temperature at 570°C to 650°C for 1 to 20 seconds to obtain primary cold dip-plated steel;

[0269] The primary cold-dip plated steel is placed in a temperature regulating device and, under the condition of heated gas, is continuously cooled to 300°C at an average cooling rate of 5-25°C / s, and the holding time is 2-30 seconds to obtain a secondary cold-dip plated steel; the temperature of the temperature regulating device is 300°C-570°C; the temperature of the heated gas is ≥100°C, and the total suspended particles in the gas are ≤0.2mg / m3;

[0270] The second cold-dip plated steel is cooled to room temperature to obtain pre-coated plated steel.

[0271] Note 12. The method for preparing aluminum-silicon steel according to Note 11 is characterized in that the dip-plated steel substrate is cooled to 570°C at a rate of 2 to 15°C / s and maintained at 570°C for 1 to 10 seconds to obtain initial cold-dip-plated steel.

[0272] Note 13. The method for preparing aluminum-silicon-coated steel according to Note 11 is characterized in that the primary cold-dip coated steel is cooled to 300°C at an average cooling rate of 5 to 20°C / s, and the holding time is 2 to 20 seconds to obtain the secondary cold-dip coated steel.

[0273] Note 14. The method for preparing aluminum-silicon steel according to any one of Notes 11 to 13 is characterized in that the annealing temperature in the annealing step of the steel substrate to be plated is 700 to 850°C, and the annealing time is 1 to 20 minutes; the temperature of the steel substrate to be plated after annealing entering the immersion bath is 600 to 700°C.

[0274] Note 15. A pre-coated steel, characterized in that the pre-coated steel is obtained by cold rolling and / or skin-passing of aluminum-silicon-coated steel; the pre-coated steel comprises a steel substrate and a skin-pass coating disposed on the steel substrate; the skin-pass coating is obtained by one of cold rolling and / or skin-passing;

[0275] The smooth coating layer comprises an intermediate layer and an aluminum silicon coating layer; the nominal thickness of the aluminum silicon coating layer is 10 μm to 33 μm; the aluminum silicon coating layer contains 5 to 40% of an AlSi phase and 0.1 to 15% of an AlSiFe phase, and the dispersion index of the AlSi phase and the AlSiFe phase in the aluminum silicon coating layer is ≥0.05;

[0276] The mass fraction of silicon in the AlSi phase is 30-50%; the mass fraction of iron in the AlSiFe phase is 10-35%, and the mass fraction of silicon is 3-15%.

[0277] Note 16. A hot-formed component, characterized in that it comprises a steel substrate and a component coating; the component coating is produced by mutual diffusion between the steel substrate and the aluminum-silicon pre-coating layer during the hot-forming process;

[0278] The component coating comprises an interdiffusion layer, a first intermediate layer, a first Al-rich intermetallic compound layer, a second intermediate layer and a second Al-rich intermetallic compound layer stacked in sequence; the interdiffusion layer is located at the innermost side of the component coating;

[0279] The first Al-rich intermetallic compound layer is a discontinuous structure, accounting for ≤80% of the length of the layer; the second Al-rich intermetallic compound layer is a quasi-continuous structure, accounting for ≥20% of the continuous length of the layer.

[0280] Note 17. The hot-formed component according to Note 16 is characterized in that the proportion of the first Al-rich intermetallic compound layer to the length of the layer is 1-50%; and the proportion of the second Al-rich intermetallic compound layer to the continuous length of the layer is ≥50%.

[0281] Note 18. The hot-formed component according to Note 17 is characterized in that the second Al-rich intermetallic compound layer accounts for 50 to 90% of the continuous length of the layer.

[0282] Supplement 19. The hot-formed component according to any one of Supplements 16 to 18, characterized in that the component plating further includes a surface layer located outside the second Al-rich intermetallic compound layer.

[0283] Note 20. The hot-formed component according to Note 19, characterized in that the average grain size of the first intermediate layer, the second intermediate layer, and the surface layer is less than or equal to 30 μm.

[0284] Note 21. The hot-formed component according to Note 20, characterized in that the average grain size of the first intermediate layer and the second intermediate layer is less than or equal to 25 μm.

[0285] Note 22. The hot-formed component according to Note 21, characterized in that the average grain size of the first intermediate layer and the second intermediate layer is less than or equal to 15 μm.

[0286] Note 23. The hot-formed component according to any one of Notes 16 to 18, characterized in that the total thickness of the coating layer of the component is 5 μm to 60 μm.

[0287] Note 24. The hot-formed component according to Note 23 is characterized in that the total thickness of the component coating is 20 μm to 55 μm.

[0288] Note 25. The hot-formed component according to Note 24 is characterized in that the total thickness of the component coating is 26 μm to 50 μm.

[0289] Note 26. The hot-formed component according to Note 25 is characterized in that the total thickness of the component coating is 30 μm to 50 μm.

[0290] Note 27. A hot-formed component, characterized in that it comprises a steel substrate and a component coating; the component coating is produced by mutual diffusion between the steel substrate and the aluminum-silicon pre-coating layer during the hot-forming process;

[0291] The component coating has at least four Si concentration peaks along the thickness direction.

[0292] Supplementary note 28. The hot-formed component according to Supplementary note 27, characterized in that the at least four Si concentration peaks include a first Si concentration peak, a second Si concentration peak, a third Si concentration peak and a fourth Si concentration peak from the component coating surface to the steel substrate;

[0293] The distance between the first Si concentration peak and the surface of the component coating is ≥0.25 μm.

[0294] Note 29. The hot-formed component according to Note 28 is characterized in that the distance between the first Si concentration peak and the component coating surface is ≥0.45 μm.

[0295] Note 30. The hot-formed component according to Note 29 is characterized in that the distance between the first Si concentration peak and the component coating surface is ≥0.75 μm.

[0296] Note 31. The hot-formed component according to Note 30 is characterized in that the distance between the first Si concentration peak and the component coating surface is ≥1.5 μm.

[0297] Note 32. The hot-formed component according to Note 27 is characterized in that, after deducting the background from the at least four Si concentration peaks, the concentration value of the minimum peak among them is ≥ 0.01%.

[0298] Note 33. The thermoformed component according to Note 32, characterized in that the concentration value of the minimum peak value is ≥ 0.025%.

[0299] Note 34. The thermoformed component according to Note 33, characterized in that the concentration value of the minimum peak value is ≥ 0.05%.

[0300] Note 35. The thermoformed component according to Note 34, characterized in that the concentration value of the minimum peak value is ≥ 0.25%.

[0301] Note 36. A production process for a thermoformed component, characterized in that it comprises the following steps:

[0302] The aluminum-silicon-coated steel described in any one of Appendix 1 to 10 or the pre-coated steel described in Appendix 15 is heated to the austenite range, the holding temperature range is 880 to 950°C, and the holding time is 3 to 15 minutes; the heating atmosphere is air, and the dew point is ≤ 0°C;

[0303] The steel plate after insulation is cooled, and the heated steel plate is taken out and deformed by pressing with a mold within 10 seconds, and cooled to below 200°C at the same time.

[0304] Note 37. A motor vehicle, characterized by comprising the hot formed component according to any one of Notes 16 to 35.

Claims

1. A kind of aluminum-plated silicon steel, characterized in that: It comprises a steel substrate and a pre-plating layer arranged on the steel substrate; the pre-plating layer comprises an intermediate layer and an aluminum-silicon coating layer; The aluminum silicon coating includes aluminum flowers; the nominal thickness of the aluminum silicon coating is 10 to 33 μm, and the aluminum flowers meet the requirements of mm. 2 The condition that the coordinate points formed by the aluminum flower area in units of μm and the aluminum flower convexity in units of μm are located in the first convex pentagon, and the first convex pentagon is surrounded by five points (2, 3), (150, 3), (350, 7), (350, 35), and (2, 35); The convexity of the aluminum flower is the difference between the three-point average value of the maximum coating thickness near the center of the aluminum flower and the three-point average value of the minimum coating thickness near the edge of the aluminum flower.

2. The aluminum-coated silicon steel according to claim 1, characterized in that: The aluminum silicon coating includes aluminum flowers; the nominal thickness of the aluminum silicon coating is 19 to 33 μm, and the aluminum flowers meet the requirements of mm. 2 The coordinate points formed by the aluminum flower area in units and the aluminum flower convexity in units of μm are located within the second convex pentagon, and the second convex pentagon is surrounded by five points: (4, 5), (170, 5), (400, 12), (400, 40), and (4, 40).

3. The aluminum-coated silicon steel according to claim 1, characterized in that: The aluminum-silicon coating includes aluminum flowers; the nominal thickness of the aluminum-silicon coating is 10 to 20 μm, and the aluminum flowers satisfy the conditions that the coordinate points formed by the aluminum flower boundary length per unit area in units of 1 / mm and the aluminum flower convexity in units of μm are located within a third convex pentagon, and the third convex pentagon is surrounded by five points: (0.1, 7), (0.17, 3), (10, 3), (10, 35), and (0.1, 35).

4. The aluminum-coated silicon steel according to claim 1, characterized in that: The aluminum-silicon coating includes aluminum flowers; the nominal thickness of the aluminum-silicon coating is 19 to 33 μm, and the aluminum flowers satisfy the conditions that the coordinate points formed by the aluminum flower boundary length per unit area in units of 1 / mm and the aluminum flower convexity in units of μm are located within the fourth convex pentagon, and the fourth convex pentagon is surrounded by five points: (0.08, 12), (0.16, 5), (8, 5), (8, 40), and (0.08, 40).

5. A method for preparing aluminum-plated silicon steel according to any one of claims 1 to 4, characterized in that: The following steps are involved: After annealing the steel substrate to be plated, the substrate is dip-plated in a plating solution to obtain a dip-plated steel substrate; the plating solution comprises, by mass percentage, 8 to 11% Si; 1 to 4% Fe; and the remainder is Al and unavoidable impurities; Cooling the dip-plated steel substrate to 570°C to 650°C at a rate of 2 to 20°C / s, and maintaining the temperature at 570°C to 650°C for 1 to 20 seconds to obtain primary cold dip-plated steel; The primary cold-dip plated steel is placed in a temperature regulating device and, under the condition of heated gas, is continuously cooled to 300°C at an average cooling rate of 5-25°C / s, and the holding time is 2-30 seconds to obtain a secondary cold-dip plated steel; the temperature of the temperature regulating device is 300°C-570°C; the temperature of the heated gas is ≥100°C, and the total suspended particulate matter in the gas is ≤0.2mg / m 3 ; The second cold-dip plated steel is cooled to room temperature to obtain pre-coated plated steel.

6. The method for preparing aluminum-plated silicon steel according to claim 5, characterized in that: The dip-plated steel substrate is cooled to 570° C. at a rate of 2 to 15° C. / s, and maintained at 570° C. for 1 to 10 seconds to obtain the initially cold-dip-plated steel.

7. The method for preparing aluminum-plated silicon steel according to claim 5, characterized in that: The primary cold-dip plated steel is cooled to 300° C. at an average cooling rate of 5 to 20° C. / s, and the heat preservation time is 2 to 20 seconds to obtain the secondary cold-dip plated steel.

8. The method for preparing aluminum-coated silicon steel according to any one of claims 5 to 7, characterized in that: The annealing temperature in the annealing step of the steel substrate to be plated is 700-850°C, and the annealing time is 1-20 minutes; the temperature of the annealed steel substrate entering the immersion plating solution is 600-700°C.

9. A pre-coated steel, characterized in that: The pre-coated steel is obtained by cold rolling and / or skin-passing the aluminum-silicon steel according to any one of claims 1 to 4; the pre-coated steel comprises a steel substrate and a skin-pass coating disposed on the steel substrate; the skin-pass coating is obtained by cold rolling and / or skin-passing; The polished coating comprises an intermediate layer and an aluminum silicon coating; the nominal thickness of the aluminum silicon coating is 10 μm to 33 μm; the aluminum silicon coating contains 5 to 40% of an Al-Si phase and 0.1 to 15% of an Al-Si-Fe phase, and the dispersion index of the Al-Si phase and the Al-Si-Fe phase in the aluminum silicon coating is ≥0.05; The dispersion index is: within the range of 20×100 square microns of the aluminum-silicon coating, each uniform-sized and significantly discontinuous Al-Si phase and Al-Si-Fe phase is simplified as a particle at the geometric center, or a single Al-Si phase and Al-Si-Fe phase with an area of ​​≥1 square micron is simplified as a particle, and the proportion of non-obtuse triangles in multiple triangles formed by connecting three adjacent particles; The mass fraction of silicon in the Al-Si phase is 30-50%; the mass fraction of iron in the Al-Si-Fe phase is 10-35%, and the mass fraction of silicon is 3-15%.

10. A production process for a thermoformed component, characterized in that: The following steps are involved: The aluminum-silicon-coated steel according to any one of claims 1 to 4 or the pre-coated steel according to claim 9 is heated to the austenite range, the holding temperature range is 880 to 950°C, and the holding time is 3 to 15 minutes; the heating atmosphere is air, and the dew point is ≤ 0°C; The steel plate after insulation is cooled, and the heated steel plate is taken out and deformed by pressing with a mold within 10 seconds, and cooled to below 200°C at the same time.

Citation Information

Patent Citations

  • Production process of hot-dip aluminum-silicon plated steel plate

    CN111549307A

  • Aluminum-free aluminum-silicon-plated steel plate and preparation process and application thereof

    CN111621706A

  • Machining method and welding method of steel blank with aluminum-silicon coating

    CN113333948A

  • Method for producing aluminum-plated silicon steel strip with high surface quality

    CN113802079A

  • High-surface-quality aluminum alloy coated steel plate and manufacturing method thereof

    CN115161519A