Method for producing gigabar-level maritime work steel forge piece through slab ingot and large ring forge piece
Through flat ingot forging technology, heating and heat treatment are controlled, the problems of many fire times and poor performance of round ingot forging are solved, and the high performance and low crack characteristics of Gipa-grade marine steel forgings are achieved.
Patent Information
- Application Number
- CN202411348020.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-06
AI Technical Summary
In the existing forging technology, round ingots are used to forge ring forging, resulting in many forging fires and poor performance. Especially under large specifications, poor heat dissipation conditions and slow cooling speed, which can easily cause segregation and affect product performance.
Flat ingots are used for forging, and the heating temperature and time are controlled through heating, square, pre-upsetting, rounding, material separation, upsetting, punching, reaming and heat treatment, reducing the forging fire times, and pre-prepared heat treatment and performance Heat treatment improves the performance of steel forgings.
The reduction of forging fires is achieved, ensuring the high yield strength and elongation of Jipa-grade marine steel forgings, reducing crack sensitivity, and improving the comprehensive performance of the product.
Smart Images

Figure CN119076885A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of forging, and in particular to a method for producing GPa-grade marine steel forgings from flat ingots and large-scale ring forgings. Background Art
[0002] With the development of marine engineering and shipbuilding industry, higher requirements are put forward for steel materials. These steels are not only required to have high strength and high toughness, but also good plasticity, impact toughness, weldability and corrosion resistance to cope with the harsh marine environment.
[0003] At present, steel for ships and marine engineering can meet most of the demand, but some high-grade special steels still rely on imports. These steels have high strength, ultra-low temperature toughness, high crack arrest and other properties, strict production process, and high development difficulty. From a global perspective, the main grades of high-strength steel for offshore platforms include yield strength 355, 420, 460, 500, 550, 620, 690MPa, etc., and the requirement for low-temperature performance is at least -40J, or even -60J. In the research on offshore platform steel, a series of high-strength steel plates resistant to seawater corrosion and low temperature have been developed, and the strength level has reached 1000MPa.
[0004] In the existing forging technology, round ingots are often used to forge ring forgings. This production process requires multiple forgings to form a forging blank. Large-sized round ingots are prone to serious segregation due to poor heat dissipation conditions, slow cooling speed, and long condensation time during solidification, which has an adverse effect on product performance.
[0005] Therefore, there is an urgent need for a preparation method that not only ensures the performance of the resulting marine engineering steel, but also reduces the number of forging times and improves production efficiency. Summary of the invention
[0006] In view of the above analysis, the present invention aims to provide a method for producing GPa-grade marine steel forgings from flat ingots and large ring forgings, so as to solve the problems of multiple firing times and poor performance in the existing methods.
[0007] In one aspect, the present invention provides a method for producing GPa-grade marine steel forgings from a flat ingot, comprising the following steps:
[0008] S1: Forging heating, heating the flat ingot;
[0009] S2: Use upper flat anvil and lower flat anvil to forge the flat ingot into a square shape; square it into a width of B × thickness of H × length of L;
[0010] S3: After returning to the original position, remove the waste material at the nozzle end and the riser end;
[0011] S4: performing overall pre-upsetting to obtain a blank;
[0012] S5: rounding the obtained blank by using an upper flat anvil and a lower V anvil, and performing a material separation process;
[0013] S6: upsetting and punching again;
[0014] S7: After punching, the hole is expanded and leveled;
[0015] S8: Expand the hole of the horse bar to produce the finished product;
[0016] S9: After forging, heat treatment is carried out, including preliminary heat treatment and performance heat treatment, to produce GPa-grade marine steel forgings.
[0017] Further, in step S1, heating is performed at 600-800°C for a holding time of ≥7h, and then heating is performed to 1200-1220°C for a holding time of 7-12h.
[0018] Further, in step S2, after normalization, B / H=2-2.5.
[0019] Further, in step S4, the initial forging temperature is 1200-1220°C, the final forging temperature is ≥850°C, and the overall reduction is 500-800 mm.
[0020] Furthermore, in steps S6 and S7, the initial forging temperature is controlled at 1150-1220°C, and the final forging temperature is controlled at ≥850°C.
[0021] Furthermore, in step S5, after the material is divided, 1.8≤L / D≤2.3 of the blank.
[0022] Furthermore, in step S8, the initial forging temperature is 1100-1200°C, the holding time is 4-8h, and the final forging temperature is ≥800°C.
[0023] Furthermore, the preliminary heat treatment is one supercooling, two annealing and tempering, keeping at 600-650°C, stopping the furnace and cooling to 200-250°C, the first annealing temperature is 840-900°C, the second annealing temperature is 810-850°C, and the tempering temperature is 620-640°C.
[0024] Furthermore, the performance heat treatment is quenching and tempering, the quenching temperature is 800-850°C, the cooling method is water immersion cooling, and the tempering temperature is 570-620°C.
[0025] On the other hand, the present invention provides a large ring forging, which is prepared by the method of the present invention.
[0026] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0027] 1. The method provided by the present invention is used to produce GPa-grade marine engineering steel forgings using flat ingots, and the preparation process includes controlled heating, squaring, pre-upsetting, rounding, material division, upsetting, punching, hole expansion and heat treatment. The method provided has a small number of overall forging reheating times, less than 6 times, and the obtained GPa-grade marine engineering steel has no cracks.
[0028] 2. In the present invention, during the squaring and rounding process, the initial forging temperature is controlled at 1200-1220°C, and the final forging temperature is controlled at ≥850°C. The amount of precipitates is relatively small, the deformation resistance is small during the preparation process, and the crack sensitivity is reduced, so as to ensure that no cracks or few cracks are generated during the forging process.
[0029] 3. The heat treatment of the present invention adopts preliminary heat treatment and performance heat treatment, wherein the preliminary heat treatment is one supercooling, two annealing and tempering, and the performance heat treatment adopts quenching and tempering. After heat treatment, the yield strength of the GPa-grade marine steel forging obtained is above 1080MPa, the elongation is above 18%, and the cross-sectional shrinkage is above 64%.
[0030] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.
[0032] Figure 1 This is a metallographic photograph of the test results of Example 1;
[0033] Figure 2 This is a metallographic photograph of Example 1 magnified 500 times. DETAILED DESCRIPTION
[0034] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.
[0035] With the development of marine engineering and shipbuilding industry, higher requirements are put forward for steel materials. At present, the main grades of high-strength steel for offshore platforms include yield strength 355, 420, 460, 500, 550, 620, 690MPa, etc., and the requirement for low-temperature performance is at least -40J, or even -60J. In the research of offshore platform steel, a series of high-strength steel plates resistant to seawater corrosion and low temperature have been developed, and the strength level has reached 980MPa.
[0036] However, in the process of preparing forgings, round ingots are often used to forge ring forgings. This production process requires multiple forgings to form forging blanks. Large-sized round ingots are prone to severe segregation due to poor heat dissipation conditions, slow cooling speed, and long condensation time during solidification, which has an adverse effect on product performance.
[0037] Therefore, the present invention provides a method for producing GPa-grade marine steel forgings from a flat ingot, comprising the following steps:
[0038] S1: Forging heating, heating the flat ingot;
[0039] S2: Use upper flat anvil and lower flat anvil to forge the flat ingot into a square shape; square it into a width of B × thickness of H × length of L;
[0040] S3: After returning to the original position, remove the waste material at the nozzle end and the riser end;
[0041] S4: performing overall pre-upsetting to obtain a blank;
[0042] S5: rounding the obtained blank by using an upper flat anvil and a lower V anvil, and performing a material separation process;
[0043] S6: upsetting and punching again;
[0044] S7: After punching, the hole is expanded and leveled;
[0045] S8: Expand the hole of the horse bar to produce the finished product;
[0046] S9: After forging, heat treatment is carried out, including preliminary heat treatment and performance heat treatment, to produce GPa-grade marine steel forgings.
[0047] Compared with the prior art, the method provided by the present invention uses flat ingots to produce GPa-grade marine engineering steel forgings, and the preparation process includes controlled heating, squaring, pre-upsetting, rounding, material division, upsetting, punching, hole expansion and heat treatment, etc. The method provided has fewer overall forging reheating times, and the obtained GPa-grade marine engineering steel forgings are free of cracks.
[0048] Specifically, the chemical composition of the slab is calculated by weight percentage as follows: C: 0.08%-0.13%, Cu: 0.40%-0.60%, V: 0.12%-0.18%, Ni: 7.20%-8.00%, Cr: 0.45%-0.75%, P≤0.015%, S≤0.010%, Mo: 0.50%-0.8%, and the balance is Fe.
[0049] It should be noted that under the above composition ratio, the forgings prepared by using the flat ingot have higher performance. However, from the composition information, it can be seen that the alloy content of the flat ingot is high, especially the Ni content, and the forging temperature range is narrow; in addition, due to the influence of the segregation and precipitates of the flat ingot, the forgeability is poor, the hot crack sensitivity is strong, and forging cracking is very easy to occur; the work hardening is serious, the deformation resistance is large; the organization is highly hereditary, so the overall forging difficulty is relatively large.
[0050] Specifically, in step S1, the material is heated in a furnace at 600-800°C for a holding time of ≥7 hours, and then heated to 1200-1220°C for a holding time of 7-12 hours.
[0051] It should be noted that alloy composition is one of the important factors affecting the thermal conductivity of materials. The alloy composition of the GPa-grade marine engineering steel mentioned in the present invention is relatively high. During the heating process, especially in the low temperature stage, it is advisable to heat up slowly, and the heating rate is ≤40°C / hour. At the same time, the step heating method is more conducive to reducing the temperature difference between the surface and the core of the billet during the heating process, reducing temperature stress and tissue stress.
[0052] The step heating method first heats to 600-800°C at a heating rate of ≤40°C / hour for insulation, and the insulation time must be greater than 7h, and then heats to 1200-1220°C at high power and insulation for 7-12h, and then forging is performed.
[0053] Specifically, in step S2, after normalization, B / H=2-2.5.
[0054] It should be noted that the specifications of the flat square steel ingot (referred to as flat ingot) are length L×width B×thickness H=3520mm×2000mm×700mm, and the ratio of width to thickness is 2.86. Moreover, the flat square steel ingot includes the arc-closing end (sprue end) and the arc-starting end (riser end). In order to avoid confusion between the arc-closing end (sprue end) and the arc-starting end (riser end) of the flat square steel ingot after high-temperature heating, obvious markings should be used to distinguish them before entering the furnace.
[0055] After heating, the flat ingot needs to be squared in order to fully break up the columnar crystals, improve the macro segregation, change the cast structure into the forged structure, make the forgings have a reasonable fiber direction distribution, improve the plasticity, impact toughness, fatigue strength, etc., and obtain excellent comprehensive performance. After squared, control B / H = 2 ~ 2.5.
[0056] During square forging, the arc end (gate end) of the ingot is flattened first. The quality of the ingot at the gate end is relatively poor, and cracks are particularly prone to occur even when forged in a high-temperature zone. Therefore, the ingot must be forged with a light hammer first, and the initial reduction should be controlled within 80 mm. As the cast structure in the ingot gradually breaks, the reduction can be gradually increased.
[0057] In addition, since the height and width of the steel ingot are relatively large, the position of the flat ingot must be adjusted at all times when squaring it to ensure that the side surface is always parallel to the pressing direction of the hydraulic press to avoid the defect of a concave center.
[0058] Specifically, in steps S2 and S4, the initial forging temperature is controlled at 1200-1220°C, and the final forging temperature is controlled at ≥850°C.
[0059] It should be noted that the initial forging temperature is controlled within 1200-1220°C, mainly due to the segregation of the core of the steel ingot. A large amount of low-melting-point materials gather in the core. During the plastic deformation process, a large amount of deformation heat will be generated inside the forging billet, making the core more prone to "overheating" and "overburning", resulting in a sharp decrease in plasticity.
[0060] The final forging temperature is controlled to be ≥850℃, mainly based on two considerations: (1) From the constant strain rate hot compression test, it is known that when the temperature is lower than 900℃, the deformation resistance increases sharply; the strain rate is 0.01s -1 The peak stress at 1000°C is about 91 MPa, but the strain rate is 0.01s -1 , the peak stress at 900°C is about 138Mpa, which is about 1.5 times that at 1000°C. Therefore, the lower the temperature, the greater the deformation resistance, so the final forging temperature is controlled above 850°C in the present invention.
[0061] (2) From the phase equilibrium diagram, it can be seen that M(C,N) begins to precipitate when cooled to 850℃ and exists stably. The maximum precipitation amount (0.33%) is at 629℃. M(C,N) is the carbide (V,Mo)C of V and Mo. M6C begins to precipitate when cooled to 690℃. The maximum precipitation amount at 290℃ is 0.46%. M6C is a carbide rich in Mo and Fe. 23 C6, the maximum precipitation amount at 310℃ is 1.05%, M 23 C6 is a carbide rich in Cr, Fe, and Mo. G phase begins to precipitate when cooled to 481°C, and the maximum precipitation amount is 2.01% at 250°C. It is an intermetallic silicon compound rich in Ni, Mn, Si, and Fe. Cu-rich phase begins to precipitate when cooled to 418°C, and the maximum precipitation amount is 0.19% at 280°C. The thermoplasticity and deformation ability of the precipitated phase are significantly different from those of the matrix. The increase of precipitates will lead to a decrease in plasticity, greater deformation resistance, and strong crack sensitivity.
[0062] Specifically, in step S5, the L / D of the blank after material separation satisfies 1.8≤L / D≤2.3.
[0063] It should be noted that the material should be divided after squaring to control the L / D ratio of the material billet after division to avoid breakage during subsequent rounding and upsetting.
[0064] Specifically, in step S4, the initial forging temperature is 1200-1220°C, the final forging temperature is ≥850°C, and the overall reduction is 500-800mm.
[0065] It should be noted that during the upsetting process, the pressing speed (below 30mm / s) and the pressing amount should be controlled, and the pressing amount for each time should be controlled (200-300mm). If the shape of the blank is not good after upsetting and there is a risk of local breakage, the shape should be repaired in time, and the upsetting forging ratio should be ≥1.8.
[0066] Punching should be done on both sides as much as possible. Before punching, if the temperature of the blank is lower than 1150℃, it is recommended to return the blank to the furnace for heating. When punching at low temperature, it is very easy to cause tearing on the end face of the blank.
[0067] In addition, if cracks appear, the direction of crack cleaning is the main deformation direction. The grooves produced by crack cleaning must not be 90° to each other, and cleaning must not be performed perpendicular to the direction of crack extension, otherwise it is easy to cause folding defects.
[0068] Specifically, in step S7, the initial forging temperature is controlled at 1150-1220°C, and the final forging temperature is controlled at ≥850°C.
[0069] Specifically, in step S8, the initial forging temperature is 1100-1200°C, the holding time is 4-8h, and the final forging temperature is ≥800°C.
[0070] It should be noted that for the flattening fire, a 600mm upper flat anvil and a rotary table are used for double-sided flattening, and the auxiliary tool is preheated to 300℃. Asbestos cloth is laid on the rotary table to delay the temperature drop of the end surface. The flattening reduction needs to be dynamically adjusted according to the temperature of the billet with 900℃ as the limit. If it is higher than 900℃, large reduction can be used for forging; if it is lower than 900℃, small reduction can be used for forging.
[0071] The forging ratio of the finished product of the horse bar expansion fire is 1.5 to 2. Considering that the deformation amount of one fire can be completed in one fire, avoid small forging ratio deformation in the final forging fire.
[0072] Specifically, the preliminary heat treatment is one supercooling, two annealing and tempering. First, the forging is kept at 600-650℃ (the holding time can be calculated according to 50mm / H), and the annealing heat treatment is carried out after the furnace is stopped and cooled to 200-250℃. The first annealing temperature is 840-900℃, and the second annealing temperature is 810-860℃; after the annealing is completed, the tempering heat treatment is carried out, and the tempering temperature is 620-640℃. The cooling method is furnace cooling.
[0073] It should be noted that forgings are subjected to post-forging heat treatment after forging. The purpose of post-forging heat treatment (also known as preliminary heat treatment) is to adjust and improve the coarse grain structure formed during the forging process, reduce the chemical composition and structural inhomogeneity inside the forging, and improve the ultrasonic flaw detection performance of the forging.
[0074] After the forgings are preparatory heat treated, rough machining is carried out to improve the surface quality of the forgings and reduce the effective thickness of the forgings, in preparation for the execution of performance heat treatment.
[0075] Forging performance heat treatment is a heat treatment carried out to ensure that the forgings finally achieve their required performance.
[0076] Specifically, the performance heat treatment adopts quenching and tempering, the quenching temperature is 800-850°C, the cooling method is water immersion cooling, and the tempering temperature is 570-620°C.
[0077] It should be noted that, by adopting the preparation method of the present invention, after preliminary heat treatment and performance heat treatment, the yield strength of the obtained GPa-grade marine steel forgings is above 1080 MPa, the elongation is above 18%, and the cross-sectional shrinkage is above 64%.
[0078] The present invention also provides a large ring forging, which is prepared by the method of the present invention.
[0079] In order to more clearly describe the present invention, it is further illustrated by the following examples and comparative examples.
[0080] Example 1
[0081] A production process for flange forgings comprises the following steps:
[0082] Step 1): After smelting, pouring and solidification, a flat ingot is obtained, the size of which is length L×width B×thickness H=3520mm×2000mm×700mm, and the ratio of width to thickness is 2.86. Forging heating, the heating furnace temperature is 700°C, the material is waited for 7h, and then the temperature is increased to 1220°C at a power heating rate, and the temperature is kept for ≥7h;
[0083] Step 2): After step 1), take out of the furnace for forging and square drawing to B (width) × H (thickness) = 1700mm × 750mm; forge the nozzle side first when square drawing;
[0084] Step 3): After step 2), the nozzle and riser ends are cut by gas cutting, the nozzle is cut off by 330mm, and the riser is cut off by 100mm: then the furnace is returned to heat to 1220℃, and the holding time is ≥5H;
[0085] Step 4): Pre-upset the whole piece to H=3000mm; round it to Ф1050mm×~L=5300mm. Then return it to the furnace and heat it to 1220℃, with a holding time of ≥7h;
[0086] Step 5): Return to the roundness to Ф920×~L=7000, cut the material φ920mm×1550mm for forging ultra-high strength steel flange forgings; then return to the furnace to heat to 1220℃, and keep warm for ≥5h; control the pressing amount each time to 80-150mm.
[0087] Step 6): Upsetting Punch holes of Ф500 on both sides; then return to the furnace and heat to 1150℃;
[0088] Step 7): After step 6), take the steel out of the furnace for pre-expansion and leveling of the horse bar. Step 7) is divided into 1-2 fire forging. When leveling, lay asbestos cloth on the turntable and adopt a double-sided leveling scheme. Then return to the furnace and heat to 1100℃, and keep warm for ≥4h;
[0089] Step 8): Expand the hole of the horse bar to produce the finished product;
[0090] Step 9): Post-forging heat treatment and performance heat treatment
[0091] After forging, the forging is heat treated once and then cooled at 600-650℃, then cooled to 200-250℃ and kept at this temperature for 8h. During annealing, the first annealing temperature is 850℃ and the holding time is 6h, and the second annealing temperature is 830℃ and the holding time is 6h. During tempering heat treatment, the tempering temperature is 630℃ and the holding time is 12h. The cooling method is furnace cooling.
[0092] The quenching temperature of performance heat treatment is 810℃×4h, and water cooling is performed after quenching; the tempering temperature is 600℃, and the holding time is 6h.
[0093] After production according to the above process, the overall forging number is 6.
[0094] Comparative Example 1
[0095] The preparation process of Comparative Example 1 is substantially the same as that of Example 1, comprising the following steps:
[0096] Step 1): After smelting, pouring and solidification, a flat ingot is obtained, the size of which is length L×width B×thickness H=3520mm×2000mm×700mm, and the ratio of width to thickness is 2.86. Forging heating, the heating furnace temperature is 700°C, the material is waited for 7h, and then the temperature is increased to 1220°C at a power heating rate, and the temperature is kept for ≥7h;
[0097] Step 2): After step 1), take it out of the furnace for forging and square it to B (width) × H (thickness) = 1700mm × 750mm; when square it, forge the nozzle side first;
[0098] Step 3): After step 2), the nozzle and riser ends are cut by gas cutting, the nozzle is cut off by 330mm, and the riser is cut off by 100mm: then the furnace is returned to heat to 1220℃, and the holding time is ≥5h;
[0099] Step 4): Return to roundness to Ф1050mm×~L=5300mm. During the rounding process, the upper and lower flat anvils need to be used to repeatedly trim the shape to reduce the side concave center. Then return to the furnace and heat to 1220℃, and the heat preservation time is ≥7h;
[0100] Step 5): Return to the roundness to Ф920×~L=7000, cut the material φ920mm×1550mm for forging ultra-high strength steel flange forgings; then return to the furnace to heat to 1220℃, and keep warm for ≥5h; control the pressing amount each time to 80-150mm.
[0101] Step 6): Upsetting Punch holes of Ф500 on both sides; then return to the furnace and heat to 1150℃;
[0102] Step 7): After step 6), take the steel out of the furnace for pre-expansion and leveling of the horse bar. Step 7) is divided into 1-2 fire forging. When leveling, lay asbestos cloth on the turntable and adopt a double-sided leveling scheme. Then return to the furnace and heat to 1100℃, and keep warm for ≥4h;
[0103] Step 8): Expand the hole of the horse bar to produce the finished product
[0104] Step 9): Post-forging heat treatment and performance heat treatment
[0105] After forging, the forging is heat treated once and then cooled at 600-650℃, then cooled to 200-250℃ and kept at this temperature for 8h. During annealing, the first annealing temperature is 850℃ and the holding time is 6h, and the second annealing temperature is 830℃ and the holding time is 6h. During tempering heat treatment, the tempering temperature is 630℃ and the holding time is 12h. The cooling method is furnace cooling.
[0106] The quenching temperature of performance heat treatment is 810℃×4h, and water cooling is performed after quenching; the tempering temperature is 600℃, and the holding time is 6h.
[0107] After production according to the above process, the overall forging number is about 9.
[0108] After forging, the forging is heat treated once and then cooled at 600-650℃, then cooled to 200-250℃ and kept at this temperature for 8h. During annealing, the first annealing temperature is 850℃ and the holding time is 6h, and the second annealing temperature is 830℃ and the holding time is 6h. During tempering heat treatment, the tempering temperature is 630℃ and the holding time is 12h. The cooling method is furnace cooling.
[0109] The quenching temperature of performance heat treatment is 810℃×4h, and water cooling is performed after quenching; the tempering temperature is 580℃, and the holding time is 7h.
[0110] Comparative Example 2
[0111] The preparation process of Comparative Example 2 is substantially the same as that of Example 1, except that in step 9) of Comparative Example 2: post-forging heat treatment and performance heat treatment
[0112] After forging, the forging is heat treated once and then cooled at 600-650℃, then cooled to 200-250℃ and kept at this temperature for 8h. During annealing, the first annealing temperature is 850℃ and the holding time is 6h, and the second annealing temperature is 830℃ and the holding time is 6h. During tempering heat treatment, the tempering temperature is 630℃ and the holding time is 12h. The cooling method is furnace cooling.
[0113] The quenching temperature of performance heat treatment is 830℃×3h, and water cooling is performed after quenching; the tempering temperature is 510℃, and the holding time is 4h.
[0114] Performance Testing
[0115] The above embodiments and comparative examples were subjected to production capacity statistics and performance tests, mainly including yield strength, elongation, cross-sectional shrinkage, etc. The performance test results are shown in Table 1.
[0116] Table 1 Performance test results
[0117]
[0118] In combination with Example 1 and Comparative Examples 1-2 and Table 1, the method provided in Example 1 of the present invention is adopted to produce and prepare GPa-grade marine engineering steel forgings using flat ingots, and the preparation process includes controlled heating, squaring, pre-upsetting, rounding, material division, upsetting, punching, hole expansion and heat treatment. The method provided has a small number of overall forging reheating times, less than 6 times, and the obtained GPa-grade marine engineering steel forgings are free of cracks. After heat treatment, the yield strength of the obtained GPa-grade marine engineering steel forgings is above 1080MPa, the elongation is above 18%, and the cross-sectional shrinkage is above 64%.
[0119] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A method for producing GPa-grade marine steel forgings from flat ingots, characterized in that: The following steps are involved: S1: Forging heating, heating the flat ingot; S2: Use upper flat anvil and lower flat anvil to forge and square the flat ingot; square it to width B×thickness H×length L; S3: After returning to the original position, remove the waste material at the nozzle end and the riser end; S4: performing overall pre-upsetting to obtain a blank; S5: rounding the obtained blank by using an upper flat anvil and a lower V anvil, and performing a material separation process; S6: upsetting and punching again; S7: After punching, the hole is expanded and leveled; S8: Expand the hole of the horse bar to produce the finished product; S9: After forging, heat treatment is carried out, including preliminary heat treatment and performance heat treatment, to produce GPa-grade marine steel forgings.
2. The method for producing GPa-grade marine steel forgings from flat ingots according to claim 1, characterized in that: In step S1, heating is performed at 600-800°C for a holding time of ≥7 hours, and then heating is performed to 1200-1220°C for a holding time of 7-12 hours.
3. The method for producing GPa-grade marine steel forgings from flat ingots according to claim 1, characterized in that: In step S2, after normalization, B / H=2~2.
5.
4. The method for producing GPa-grade marine steel forgings from flat ingots according to claim 1, characterized in that: In step S4, the initial forging temperature is 1200-1220°C, the final forging temperature is ≥850°C, and the overall reduction is 500-800 mm.
5. The method for producing GPa-grade marine steel forgings from flat ingots according to claim 1, characterized in that: In steps S6 and S7, the initial forging temperature is controlled at 1150-1220°C, and the final forging temperature is controlled at ≥850°C.
6. The method for producing GPa-grade marine steel forgings from flat ingots according to claim 1, characterized in that: In step S5, after the material is divided, 1.8≤L / D≤2.3 of the blank.
7. The method for producing GPa-grade marine steel forgings from flat ingots according to claim 1, characterized in that: In step S8, the initial forging temperature is 1100-1200°C, the holding time is 4-8h, and the final forging temperature is ≥800°C.
8. The method for producing GPa-grade marine steel forgings from flat ingots according to claim 1, characterized in that: The preliminary heat treatment includes one supercooling, two annealing and tempering, keeping at 600-650°C, stopping the furnace and cooling to 200-250°C, the first annealing temperature is 840-900°C, the second annealing temperature is 810-850°C, and the tempering temperature is 620-640°C.
9. The method for producing GPa-grade marine steel forgings from flat ingots according to claim 1, characterized in that: The performance heat treatment includes quenching and tempering, the quenching temperature is 800-850°C, the cooling method is water immersion cooling, and the tempering temperature is 570-620°C.
10. A large ring forging, characterized in that: The method is prepared by any one of claims 1 to 9.
Citation Information
Patent Citations
Forging process of large forged ring
CN102513780A
Improved 9% Ni steel suitable for ultra-thick section and preparation method thereof
CN112708826A
Forging method of high-torque-density offshore wind power forged steel part
CN116463480A