Accurate butt joint and combined welding method for large marine motor shaft forgings

Through segmented assembly and precision welding technology, the problems of large marine motor shaft weight and high energy consumption are solved, the motor shaft is lightweight, energy-saving and efficient, and dynamic balance and safety are ensured.

CN118720668AActive Publication Date: 2024-10-01BAODING HEAVY IND CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411180233.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-10-01
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The large marine motor shaft has a large weight, high energy consumption during operation, and is difficult to weld, which can easily lead to unstable dynamic balance and safety hazards.

Method used

It adopts a segmented assembly design, achieves precise docking through interference fit and heating blanket technology, and combines carbon dioxide gas shielded welding and submerged arc welding technology to perform inner hole and outer circle welding to ensure wall thickness uniformity and strength.

Benefits of technology

It greatly reduces the weight of the motor shaft by about 55%, while reducing energy consumption, improving the dynamic balance and safety of the motor shaft, and extending the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720668A_ABST
    Figure CN118720668A_ABST
Patent Text Reader

Abstract

The invention relates to an accurate butt joint and combined welding method for large marine motor shaft forgings, which not only can greatly reduce the self weight of a motor shaft (the weight reduction rate is about 55%), but also can greatly reduce the energy consumption during operation to achieve the purposes of saving energy and improving efficiency. The iron core and the short shaft are provided with spigots in a connection area; the iron core spigot is placed upwards, after the iron core spigot meets the set magnitude of interference, the short shaft is vertically lifted, the shaft head faces upwards, the short shaft spigot faces downwards, and after the iron core spigot is vertically placed to the iron core spigot, the heating blanket on the outer circle of the iron core is detached to clamp the short shaft spigot; after the interference fit is completed, a plurality of reinforcing ribs are additionally arranged at the interface; the short-shaft iron core assembly is horizontally placed on an electric roller carrier, and after welding in an inner hole is completed, the electric blanket stops heating, but is not disassembled, and is slowly cooled; after the inner hole is welded, the reinforcing ribs are removed, and an outer circle groove is machined through a machine tool; the short-shaft iron core assembly is placed on the roller carrier again, the outer circle is welded in a submerged-arc welding mode, and after welding is completed, the outer circle is wrapped with an electric blanket and slowly cooled; and after welding is completed, subsequent finish machining and subsequent screw bolt assembling procedures of the propeller shaft are carried out.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for accurately butting and combining welding large-scale marine motor shaft forgings, which can not only greatly reduce the weight of the motor shaft itself (weight reduction rate is about 55%), but also greatly reduce energy consumption during operation, thereby achieving the purpose of energy saving and efficiency improvement, and belongs to the field of manufacturing large-scale marine motor shaft forgings. Background Art

[0002] At present, the motor shaft of large marine motors is designed to be integrally forged, and the finished product is a solid forging. The disadvantages are: first, the weight is heavy, the energy consumption is high during operation; second, the manufacturing cost is high. Summary of the invention

[0003] Design purpose: To avoid the shortcomings of the background technology, a method for precise docking and combined welding of large marine motor shaft forgings is designed, which can not only significantly reduce the weight of the motor shaft itself (weight reduction rate is about 55%), but also significantly reduce energy consumption during operation, so as to achieve the purpose of energy saving and efficiency improvement.

[0004] Design scheme: In order to achieve the above design objectives. In the manufacturing process design of the present invention: the motor shaft design adopts segmented assembly, which consists of three parts: propeller shaft, short shaft and iron core. The propeller shaft and the iron core are fixedly connected by bolts, and the short shaft and the iron core are connected by combined welding ( Figure 1 ). The difficulty in manufacturing is that due to the large size of the short shaft and the iron core, the concentricity after matching is extremely difficult to control. Conventional stacking and welding splicing are likely to cause large deviations in straightness after assembly, resulting in uneven wall thickness after fine machining of the outer circle. In actual application, the marine motor shaft is a high-speed rotating moving part. If the wall thickness is uneven, it will cause uneven distribution of centrifugal force during high-speed rotation and unstable dynamic balance, which will reduce the service life of the marine motor shaft and even cause serious safety accidents. Secondly, the main difficulty in welding is that the marine motor shaft is a large forging with a minimum wall thickness of 90mm. The welding of the short shaft and the iron core is difficult. If single-side groove welding of the outer circle is used, there will be a risk of welding failure or cracks at the bottom of the inner hole, which will greatly reduce the overall strength of the motor shaft.

[0005] To this end, this method 1) uses interference fit to achieve precise docking and positioning, and sets stoppers on the core and short shaft in the connection area; 2) The core stopper is placed upward, and the outer circle is wrapped with a heating blanket. After the stoppers of the short shaft and the core meet the set interference, the short shaft is lifted vertically, with the shaft head facing upward and the stopper of the short shaft facing downward, and is placed vertically on the stopper of the core. The heating blanket on the outer circle of the core is removed, and the stopper of the core is cooled and contracted naturally, and the stopper of the short shaft is clamped; 3) After the interference fit is completed, add multiple reinforcing ribs at the interface; 4) After the reinforcement rib welding is completed, the short shaft core assembly is placed horizontally on the electric roller frame, ready for welding in the inner hole. The groove depth at the inner hole stop is one-third to two-fifths of the wall thickness, the groove angle is 45°-62°, and the roller speed is 1 turn / 20min~1 turn / 30min; 5) The inner hole welding adopts carbon dioxide gas shielded welding (FCAW), and the inner hole is welded in a circular manner. Before welding, a heating blanket is used to wrap the entire circle of the reinforcement rib position. The preheating temperature is 80-100℃, and the roller speed is adjusted according to the welding speed of the inner hole. The inner hole welding position is always kept flat. The interlayer control during welding is ≤250℃. After welding, the electric heating blanket stops heating, but is not removed and slowly cooled; 6) After the inner hole welding is completed, remove the reinforcement ribs, and the outer circle groove is machined by machine tools; 7) The outer hole groove depth corresponding to the motor shaft wall thickness is greater than two-thirds of the motor shaft wall thickness, the groove angle is 55°-72°, and the roller speed is 1 turn / 10min~1 turn / 15min; 8) External circle welding: The short shaft core assembly is placed on the roller frame again, and the outer circle is welded by submerged arc welding (SAW). Before welding, a heating blanket is used to locally heat the outer circle groove position, the preheating temperature is 100℃, and the insulation time is 3h. The roller speed is adjusted according to the welding speed of the outer circle, and the welding position is always kept flat. The interlayer control during welding is ≤250℃. After welding, it is wrapped with an electric heating blanket and slowly cooled; after welding, the machining amount of the outer circle is uniform to ensure the uniformity of the wall thickness, so that the dynamic balance of the motor shaft during high-speed rotation meets the requirements. 9) After welding is completed, subsequent fine processing and subsequent bolt assembly process with the propeller shaft are carried out.

[0006] Compared with the background technology, the weight of the motor shaft is reduced by about 55% in the present invention, thereby significantly reducing energy consumption during operation and achieving the purpose of energy saving and efficiency improvement. BRIEF DESCRIPTION OF THE DRAWINGS

[0007] Figure 1 This is a schematic diagram of the motor shaft being assembled in sections.

[0008] Figure 2 yes Figure 1 Schematic diagram of the size outline of the joint.

[0009] Figure 3 It is a schematic diagram of the vertical coordination of the short shaft and the iron core.

[0010] Figure 4 It is a schematic diagram of the reinforcement rib.

[0011] Figure 5 Schematic diagram of the roller bracket.

[0012] Figure 6 It is a schematic diagram of the inner hole groove.

[0013] Figure 7 It is a schematic diagram of external cylindrical groove processing.

[0014] Figure 8 It is a schematic diagram of background technology. DETAILED DESCRIPTION

[0015] See attached Figure 1-7 A precise docking and combined welding method for large marine motor shaft forgings. 1. Accurate docking positioning, using interference fit to achieve accurate docking, the core and short shaft are set with stoppers in the connection area, the corresponding size ( Figure 2 ): According to the commonly used motor shaft sizes, the stop size and interference requirements are set as shown in Table 1: Table 1 Seam size and interference

[0016] 2. Place the core with the stop facing upwards and wrap the outer circle with a heating blanket. For different thicknesses T, heating rates, heating temperatures and holding times, see Table 2. After the short shaft and the core stop meet the interference fit in Table 1, lift the short shaft vertically with the shaft head facing upwards and the short shaft stop facing downwards ( Figure 3 ), after vertically placing it on the core stop, remove the heating blanket on the outer circle of the core, allow the core stop to cool and shrink naturally, and tighten the short shaft stop to achieve the purpose of interference fit.

[0017] Table 2 Correspondence between wall thickness, heating rate and heating time

[0018] 3. After the interference fit is completed, in order to ensure the straightness of the short shaft and the iron core after fitting, 4 reinforcing ribs are added at the interface ( Figure 4 ), and also ensure that when the inner hole welding is implemented, the overall deformation will not be caused by welding stress.

[0019] 4. After the reinforcement welding is completed, the short shaft core assembly is placed horizontally on the electric roller frame ( Figure 5 ), prepare to implement welding in the inner hole, groove depth at the inner hole stop, groove angle diagram ( Figure 6 ); The inner hole groove depth, angle and roller speed corresponding to the motor shaft wall thickness are shown in Table 3; Table 3 Inner hole groove design parameters

[0020] 5. Inner hole welding: The inner hole is welded by carbon dioxide gas shielded welding (FCAW). The inner hole is welded in a circular manner. Before welding, a heating blanket is used to wrap the entire circle of the reinforcement position. The preheating temperature is 80-100℃. The roller speed is adjusted according to the welding speed of the inner hole. The inner hole welding position is always kept flat. The interlayer temperature during welding is controlled at ≤250℃. After welding, the electric heating blanket stops heating, but is not removed and slowly cooled. The welding materials and welding parameters are detailed in Tables 4 and 5; Table 4 Inner hole welding materials

[0021] Table 5 Inner hole welding parameters

[0022] 6. After the inner hole is welded, the reinforcing ribs are removed and the outer cylindrical groove is machined by machine tools. Schematic diagram of groove processing depth ( Figure 7 ); The outer hole groove depth, angle and roller speed corresponding to the motor shaft wall thickness are shown in Table 6; Table 6 External groove design parameters

[0023] 7. External cylindrical welding: Re-place the short shaft core assembly on the roller frame, and weld the external cylindrical part by submerged arc welding (SAW). Before welding, use a heating blanket to locally heat the external cylindrical groove position. The preheating temperature is 100°C, and the holding time is 3h. The roller speed is adjusted according to the welding speed of the external cylindrical part. The welding position is always kept flat. The interlayer temperature during welding is controlled at ≤250°C. After welding, wrap it with an electric heating blanket and cool it slowly. For details of welding materials and welding parameters, see Table 7 and Table 8; Table 7 External cylindrical welding materials

[0024] Table 8 External round welding parameters

[0025] 8. After welding is completed, subsequent finishing and subsequent bolt assembly process with the propeller shaft will be carried out.

[0026] It should be understood that although the above embodiments provide a relatively detailed textual description of the design ideas of the present invention, these textual descriptions are only simple textual descriptions of the design ideas of the present invention, rather than limitations on the design ideas of the present invention. Any combination, addition or modification that does not exceed the design ideas of the present invention shall fall within the protection scope of the present invention.

Claims

1. A method for precise docking and combined welding of large marine motor shaft forgings, characterized by: 1) Adopt interference fit to achieve precise docking and positioning, and set stoppers in the connection area of ​​the core and short shaft; 2) Place the core with the stop facing upwards and wrap the outer circle with a heating blanket. After the short shaft and the core stop meet the set interference, lift the short shaft vertically with the shaft head facing upwards and the short shaft stop facing downwards. Place it vertically on the core stop, remove the heating blanket on the outer circle of the core, and allow the core stop to cool and shrink naturally, and tighten the short shaft stop; 3) After the interference fit is completed, add multiple reinforcing ribs at the interface; 4) After the reinforcement welding is completed, the short shaft core assembly is placed horizontally on the electric roller frame, ready for welding in the inner hole. The groove depth at the inner hole stop is one-third to two-fifths of the wall thickness, the groove angle is 45°-62°, and the roller speed is 1 revolution / 20min~1 revolution / 30min; 5) Carbon dioxide gas shielded welding (FCAW) is used for inner hole welding. The inner hole is welded in a circular pattern. Before welding, a heating blanket is used to wrap the entire circle of the reinforcement position. The preheating temperature is 80-100°C. The roller speed is adjusted according to the welding speed of the inner hole. The inner hole welding position is always kept flat. The interlayer temperature during welding is controlled at ≤250°C. After welding is completed, the electric heating blanket stops heating, but is not removed and slowly cooled; 6) After the inner hole welding is completed, remove the reinforcement ribs and process the outer groove through the machine tool; 7) The groove depth of the outer hole corresponding to the motor shaft wall thickness is greater than two-thirds of the motor shaft wall thickness, the groove angle is 55°-72°, and the roller speed is 1 revolution / 10min~1 revolution / 15min; 8) External cylindrical welding: Re-place the short-axis core assembly on the roller frame, and weld the external cylindrical part by submerged arc welding (SAW). Before welding, use a heating blanket to locally heat the external cylindrical groove position. The preheating temperature is 100°C, and the insulation time is 3 hours. The roller speed is adjusted according to the welding speed of the external cylindrical part. The welding position is always kept flat. The interlayer temperature during welding is controlled at ≤250°C. After welding, wrap it with an electric blanket and cool it slowly. 9) After welding is completed, subsequent finishing and subsequent bolt assembly process with the propeller shaft will be carried out.

Citation Information

Patent Citations

  • Processing method of hollow shaft with small orifices and large inner holes

    CN101947721A

  • Multi-section hollow shaft butt joint method

    CN107855730A

  • Precise assembling and welding method for pipeline parts

    CN115255939A

  • Butt welding of inclined steel tubes

    JP2001018065A

  • Method for producing welded steel tube

    JP2006281313A