Production process for synthesizing mica from artificial lens

Through high-temperature melting and ultrasonic stripping and refinement processes, combined with the preparation of potassium fluorosilicate, the problem of high energy consumption in the artificial mica crushing process and poor fluidity of potassium fluorosilicate is solved, achieving high-efficiency, low-energy consumption mica production and high quality Preparation of potassium fluorosilicate.

CN118724006AInactive Publication Date: 2024-10-01JIANGSU SONGSHENG MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410929495.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing artificial mica crushing process has problems such as high energy consumption, low efficiency and complex processes. At the same time, potassium fluorosilicate on the market has poor fluidity and is easy to agglomerate, which cannot meet the quality requirements of synthetic mica.

Method used

Flake mica is produced by melting raw materials such as molybdenum tailings, potassium carbonate, potassium feldspar, magnesium oxide, alumina, montmorillonite, silicon dioxide and sodium fluorosilicate at high temperatures, and then uses ultrasonic peeling to refine it. The process combines sodium citrate as a grinding aid to achieve damage-free ultra-fine grinding; at the same time, through the reaction of sodium chloride melt leaching potassium feldspar and fluosilicate solution, potassium fluosilicate with suitable particle size and good fluidity is prepared.

Benefits of technology

It achieves efficient production of artificial crystal mica, reduces costs and energy consumption, improves grinding efficiency, ensures the smoothness and particle thickness ratio of the mica surface, meets the demand for high-quality mica, and effectively utilizes molybdenum tailings resources.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a production process of mica synthesized from artificial crystals. The mica is prepared from the following raw materials: molybdenum tailings, potassium carbonate, potassium feldspar, magnesium oxide, aluminum oxide, montmorillonite, silicon dioxide, sodium fluosilicate, potassium fluosilicate and the like. The used molybdenum tailings are industrial waste residues, so that the production cost of the mica synthesized by the artificial crystal is reduced, resources are saved, and economic benefits are improved; sodium citrate is used for assisting grinding, so that the dispersity is improved, and the production efficiency is improved; ultrasonic waves are used for stripping and refining, the surface of the synthetic mica is not damaged, energy consumption is low, consumed time is short, the surface of the mica is smooth, and the grain thickness ratio is large. The synthesized potassium fluosilicate improves the development and utilization rate of insoluble sylvite resources in the production process of synthesizing mica by the artificial lens; and through a feeding mode of simultaneously adding main reaction materials, the solution concentration, the stirring speed, the reaction temperature and the reaction time are controlled, so that the potassium fluosilicate which is proper in particle size, good in flowability and free of caking after long-term storage is obtained, and the quality of the mica synthesized by the artificial lens is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of synthetic mica, and in particular to a production process of artificial crystal synthetic mica. Background Art

[0002] Artificial mica is synthesized from a variety of chemical raw materials at high temperatures. Due to its high temperature resistance, high insulation, and complete crystal surface, it is widely used in pearlescent mica substrates, cosmetic fillers, high temperature resistant coatings, insulation materials, plastic reinforcement materials, etc. 2 The new surface consumes a lot of energy, so it is one of the most difficult minerals to grind. At present, the domestic mica crushing process commonly uses wheel mills, sand mills, and stirred mills, which mainly crush mica through the impact, friction and shearing of the grinding medium. The mica flake particles produced by grinding have many types of particle sizes and a wide particle size distribution. During continuous production, water must be added to the grinding trough continuously. After grinding to a certain fineness, the mica slurry must be diluted. The process is complicated and wastes energy. At the same time, the friction mechanical action will scratch the surface of the mica sheet and affect its optical effect. Therefore, it is necessary to develop a new method for exfoliating and refining artificial synthetic mica. Ultrafine grinding is a necessary processing technology for powder raw materials such as modern chemical industry, electronics, light industry, ceramics, metallurgy, and composite materials. However, grinding is a high-energy consumption and low-efficiency process. Therefore, it is an important research topic to effectively control the grinding balance, reduce the grinding limit, and delay the formation of "agglomeration" by adding grinding aids.

[0003] Molybdenum tailings are waste residues produced when mining molybdenum ore. Its discharge and accumulation not only consumes manpower, material and financial resources, but also occupies land and pollutes the environment. Its comprehensive utilization is not ideal. Soluble potassium salt resources are in short supply, and the development of insoluble potassium salt resources is one of the future development directions. Potassium feldspar is one of the representatives of insoluble potassium salts, with large reserves and wide distribution. It is urgent to develop a suitable extraction method to rationally utilize the potassium salt resources. The production process of artificial synthetic mica requires that the raw material potassium fluorosilicate has good fluidity, low moisture and no agglomeration. The mainstream potassium fluorosilicate products on the market are powder products with fine particle size, but poor fluidity, agglomeration and large dust during use, which cannot meet the quality requirements of synthetic mica users. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a production process of artificial crystal synthetic mica.

[0005] The purpose of the present invention can be achieved through the following technical solutions: The artificial crystal synthetic mica is prepared by the following steps: Step S1: crush the molybdenum tailings, pass through a 40-mesh sieve, and then put them into a magnetic field screening machine, screen them for 45-60 minutes under the condition of a magnetic moment of 130-140 mm, and obtain the iron-removed molybdenum tailings; the amount of molybdenum tailings used is 80-120 g; During the reaction process of step S1, the molybdenum tailings are treated to remove iron to avoid adverse effects on the color of the synthetic mica.

[0006] Step S2: The iron-removed molybdenum tailings, potassium carbonate, potassium feldspar, magnesium oxide, aluminum oxide, montmorillonite, silicon dioxide, sodium fluorosilicate and potassium fluorosilicate are placed in a mechanical mixer and mixed for 1-1.5 hours, the feeding temperature is 1200°C, the melting temperature is 1460°C, and the temperature is kept for 2 hours, and then the temperature is reduced to 1250°C at a cooling rate of 2-3°C / min, and after being kept for 2 hours, the mixture is sealed and cooled to room temperature with the furnace, and the mixing is continued for 30 minutes. min to obtain flaky synthetic mica; the dosage ratio of molybdenum tailings, potassium carbonate, potassium feldspar, magnesium oxide, aluminum oxide, montmorillonite, silicon dioxide, sodium fluorosilicate and potassium fluorosilicate is 40-60g: 1.9-2.7g: 0.9-1.3g: 8.5-13.1g: 4.7-7.1g: 14.9-23.1g: 5.9-16.4g: 2.8-2.9g: 13.1-13.4g; During the reaction process of step S2, the iron-removed molybdenum tailings, potassium carbonate, potassium feldspar, magnesium oxide, aluminum oxide, montmorillonite, silicon dioxide, sodium fluorosilicate and potassium fluorosilicate react to fully utilize the molybdenum tailings resources, partially replace silicon dioxide with them, participate in the synthesis reaction, and obtain flaky synthetic mica.

[0007] Step S3: adding flaky synthetic mica to water, mixing for 15-20 minutes to obtain a suspension, adding ethanol and sodium citrate to the suspension, mixing for 20-30 minutes, and then placing it in an ultrasonic device I for 15-20 minutes, and then placing it in an ultrasonic device II for 40-60 minutes to obtain artificial crystal synthetic mica; the frequency of the ultrasonic device I is 20kHz, the power is 260W, and the frequency of the ultrasonic device II is 20kHz, and the power is 300W; the amount ratio of the flaky synthetic mica, water, ethanol, and sodium citrate is 18.7g:100mL:50-60mL:0.01-0.02g, and the volume fraction of ethanol is 95%; During the reaction process of step S3, sodium citrate grinding aid is used. Sodium citrate is adsorbed on the surface of synthetic mica to reduce surface free energy and penetrate into microcracks to split. Sodium citrate also reduces the viscosity of the suspension, improves the dispersibility during ultrafine grinding, and greatly improves the grinding efficiency. After two ultrasonic actions of different powers, the synthetic mica is stripped and refined. During the stripping and refinement process, the volume crushing generated by the ultrasonic microjet plays a leading role in large-particle mica, and the surface crushing generated by the ultrasonic cavitation shock wave plays a leading role in small-particle mica. This non-destructive crushing process has the characteristics of low energy consumption, short action time, smooth mica surface and large particle thickness ratio.

[0008] The potassium fluorosilicate is prepared by the following steps: Step A1: After potassium feldspar and sodium chloride are crushed respectively to obtain potassium feldspar particles and sodium chloride powder, the potassium feldspar particles and the sodium chloride powder are mixed and stirred for 20-30 minutes, and then put into an alumina crucible and heated in a high-temperature furnace at 850-950° C. for melting and leaching without stirring in the crucible. After 3.5-4 hours, the crucible is taken out, cooled and water is added to obtain a potassium feldspar leaching solution; the dosage ratio of potassium feldspar particles, sodium chloride powder and water is 100g:100g:210-230mL; the potassium concentration in the potassium feldspar leaching solution is 0.30-0.33mol / L; During the reaction of step A1, NaCl reacts with KAlSi3O8 in potassium feldspar to generate KCl and NaAlSi3O8. During leaching, potassium in the solid phase is replaced by sodium and melted into the liquid phase. As the reaction proceeds, the potassium in the solid phase becomes less and less, while the potassium in the liquid phase becomes more and more, and finally a balance is reached. At this time, the potassium melting rate is the largest, thereby obtaining a potassium feldspar leachate.

[0009] Step A2: adding the fluorosilicic acid solution and the potassium feldspar leaching solution to a synthesis tank simultaneously and slowly, and then adding a growth agent potassium sulfate, stirring the synthesis tank at a stirring speed of 120 r / min and stirring at 50-55° C. for 1.5-2 hours to obtain a slurry, and then filtering and washing the slurry, and drying it at 100° C. for 4-6 hours to obtain potassium fluorosilicate; the dosage ratio of the fluorosilicic acid solution, the potassium feldspar leaching solution and the potassium sulfate is 100 mL: 190-200 mL: 0.15-0.25 g, and the concentration of the fluorosilicic acid solution is 0.25-0.30 mol / L; During the reaction process of step A2, fluorosilicic acid in the fluorosilicic acid solution reacts with potassium ions in the potassium feldspar leachate to generate potassium fluorosilicate; by adding the fluorosilicic acid solution and the potassium feldspar leachate at the same time and adding an extender potassium sulfate, potassium fluorosilicate with suitable particle size, good fluidity and no agglomeration during long-term storage is obtained.

[0010] Beneficial effects of the present invention: the artificial crystal synthetic mica of the present invention comprises raw materials such as molybdenum tailings, potassium carbonate, potassium feldspar, magnesium oxide, aluminum oxide, montmorillonite, silicon dioxide, sodium fluorosilicate and potassium fluorosilicate. In the process of synthesizing artificial crystal synthetic mica, molybdenum tailings are reasonably and effectively utilized, and industrial waste residues are fully utilized to prepare artificial crystal synthetic mica, which can reduce costs, save resources, and improve the comprehensive utilization of molybdenum tailings, so that the production process of artificial crystal synthetic mica has higher economic benefits; in addition, in the preparation process of artificial crystal synthetic mica, sodium citrate is also used to aid grinding, which not only reduces the surface free energy of synthetic mica, but also improves dispersibility and improves grinding efficiency, thereby improving the production efficiency of artificial crystal synthetic mica; at the same time, ultrasonic waves are used for exfoliation and refinement, which does not damage the surface of synthetic mica, and has the advantages of low energy consumption, short time consumption, smooth surface of mica and large particle thickness ratio.

[0011] In the preparation process of potassium fluorosilicate, sodium chloride is first used to melt-leach potassium feldspar to obtain a potassium feldspar leaching solution, so that insoluble potassium salt resources in the potassium feldspar can be utilized, thereby improving the development and utilization rate of insoluble potassium salt resources in artificial crystal synthetic mica; then, by simultaneously adding two main reaction materials of a fluorosilicic acid solution and a potassium feldspar leaching solution, adding a growth agent potassium sulfate, and controlling appropriate solution concentration, stirring speed, reaction temperature and time, potassium fluorosilicate with appropriate particle size, good fluidity and no agglomeration during long-term storage is obtained, thereby meeting the property requirements of the current artificial crystal synthetic mica production process for potassium fluorosilicate and improving the quality of artificial crystal synthetic mica. DETAILED DESCRIPTION

[0012] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0013] Example 1: Potassium fluorosilicate, prepared by the following steps: Step A1: After potassium feldspar and sodium chloride are crushed respectively to obtain potassium feldspar particles and sodium chloride powder, the potassium feldspar particles and sodium chloride powder are mixed and stirred for 20 minutes, and then put into an alumina crucible and heated in a high-temperature furnace at 850° C. for melting and leaching without stirring in the crucible. After 3.5 hours, the crucible is taken out, cooled and water is added to obtain a potassium feldspar leaching solution; the dosage ratio of potassium feldspar particles, sodium chloride powder and water is 100g:100g:210mL; the potassium concentration in the potassium feldspar leaching solution is 0.30mol / L; Step A2: Fluorosilicic acid solution and potassium feldspar leaching solution are slowly added to a synthesis tank at the same time, and then potassium sulfate is added as an extender. The synthesis tank is stirred at a speed of 120 r / min and stirred at 50° C. for 1.5 hours to obtain a slurry. The slurry is then filtered, washed, and dried at 100° C. for 4 hours to obtain potassium fluorosilicate. The dosage ratio of the fluosilicic acid solution, the potassium feldspar leaching solution and the potassium sulfate is 100 mL: 190 mL: 0.15 g, and the concentration of the fluosilicic acid solution is 0.25 mol / L.

[0014] Example 2: Potassium fluorosilicate, prepared by the following steps: Step A1: After potassium feldspar and sodium chloride are crushed respectively to obtain potassium feldspar particles and sodium chloride powder, the potassium feldspar particles and sodium chloride powder are mixed and stirred for 25 minutes, and then put into an alumina crucible and heated in a high-temperature furnace at 850-950° C. for melting and leaching without stirring in the crucible. After 3.7 hours, the crucible is taken out, cooled and water is added to obtain a potassium feldspar leaching solution; the dosage ratio of potassium feldspar particles, sodium chloride powder and water is 100g:100g:220mL; the potassium concentration in the potassium feldspar leaching solution is 0.31mol / L; Step A2: Fluorosilicic acid solution and potassium feldspar leaching solution are slowly added to a synthesis tank at the same time, and then potassium sulfate is added as an extender. The synthesis tank is stirred at a stirring speed of 120 r / min and stirred at 52° C. for 1.7 hours to obtain a slurry. The slurry is then filtered, washed, and dried at 100° C. for 5 hours to obtain potassium fluorosilicate. The dosage ratio of the fluosilicic acid solution, the potassium feldspar leaching solution and the potassium sulfate is 100 mL: 195 mL: 0.20 g, and the concentration of the fluosilicic acid solution is 0.27 mol / L.

[0015] Example 3: Potassium fluorosilicate is prepared by the following steps: Step A1: After potassium feldspar and sodium chloride are crushed respectively to obtain potassium feldspar particles and sodium chloride powder, the potassium feldspar particles and the sodium chloride powder are mixed and stirred for 30 minutes, and then put into an alumina crucible and heated in a high-temperature furnace at 950° C. for melting and leaching without stirring in the crucible. After 4 hours, the crucible is taken out, cooled and water is added to obtain a potassium feldspar leaching solution; the dosage ratio of potassium feldspar particles, sodium chloride powder and water is 100g:100g:230mL; the potassium concentration in the potassium feldspar leaching solution is 0.33mol / L; Step A2: Slowly add the fluorosilicic acid solution and the potassium feldspar leaching solution into the synthesis tank at the same time, then add the growth agent potassium sulfate, stir the synthesis tank at a stirring speed of 120r / min, and stir at 55°C for 2h to obtain a slurry, then filter and wash the slurry, and dry it at 100°C for 6h to obtain potassium fluorosilicate; the dosage ratio of the fluorosilicic acid solution, the potassium feldspar leaching solution and the potassium sulfate is 100mL:200mL:0.25g, and the concentration of the fluorosilicic acid solution is 0.30mol / L.

[0016] Embodiment 4: The artificial crystal synthetic mica is prepared by the following steps: Step S1: crush the molybdenum tailings, pass them through a 40-mesh sieve, and then put them into a magnetic field screening machine and screen them for 45 minutes under the condition of a magnetic moment of 130 mm to obtain the iron-removed molybdenum tailings; the amount of molybdenum tailings used is 80 g; Step S2: adding the iron-removed molybdenum tailings, potassium carbonate, potassium feldspar, magnesium oxide, aluminum oxide, montmorillonite, silicon dioxide, sodium fluorosilicate and the potassium fluorosilicate obtained in Example 1 into a mechanical mixer and mixing for 1 hour, with the feeding temperature being 1200° C., the melting temperature being 1460° C., and keeping the temperature for 2 hours, then cooling to 1250° C. at a cooling rate of 2° C. / min, keeping the temperature for 2 hours, sealing with a cover, cooling to room temperature with the furnace, and continuing to mix for 30 minutes to obtain flaky synthetic mica; the amount ratio of the iron-removed molybdenum tailings, potassium carbonate, potassium feldspar, magnesium oxide, aluminum oxide, montmorillonite, silicon dioxide, sodium fluorosilicate and potassium fluorosilicate is 40g:2.7g:1.3g:13.1g:7.1g:23.1g:16.4g:2.9g:13.4g; Step S3: adding flaky synthetic mica to water, mixing for 15 minutes to obtain a suspension, adding ethanol and sodium citrate to the suspension, mixing for 20 minutes, placing it in an ultrasonic device I for 15 minutes, and then placing it in an ultrasonic device II for 40 minutes to obtain artificial crystal synthetic mica; the frequency of the ultrasonic device I is 20kHz, the power is 260W, the frequency of the ultrasonic device II is 20kHz, and the power is 300W; the amount ratio of the flaky synthetic mica, water, ethanol, and sodium citrate is 18.7g:100mL:50mL:0.01g, and the volume fraction of ethanol is 95%.

[0017] Embodiment 5: The artificial crystal synthetic mica is prepared by the following steps: Step S1: crush the molybdenum tailings, pass them through a 40-mesh sieve, and then put them into a magnetic field screening machine and screen them for 50 minutes under the condition of a magnetic moment of 130 mm to obtain the iron-removed molybdenum tailings; the amount of the molybdenum tailings used is 90 g; Step S2: adding the iron-removed molybdenum tailings, potassium carbonate, potassium feldspar, magnesium oxide, aluminum oxide, montmorillonite, silicon dioxide, sodium fluorosilicate and the potassium fluorosilicate obtained in Example 2 into a mechanical mixer and mixing for 1.2 hours, with the feeding temperature being 1200° C., the melting temperature being 1460° C., and keeping the temperature for 2 hours, then cooling to 1250° C. at a cooling rate of 2° C. / min, keeping the temperature for 2 hours, sealing with a cover, cooling to room temperature with the furnace, and continuing to mix for 30 minutes to obtain flaky synthetic mica; the amount ratio of the iron-removed molybdenum tailings, potassium carbonate, potassium feldspar, magnesium oxide, aluminum oxide, montmorillonite, silicon dioxide, sodium fluorosilicate and potassium fluorosilicate is 50g:2.3g:1.1g:10.8g:5.9g:19.0g:11.1g:2.85g:13.2g; Step S3: adding flaky synthetic mica to water, mixing for 17 minutes to obtain a suspension, adding ethanol and sodium citrate to the suspension, mixing for 25 minutes, placing it in an ultrasonic device I for 17 minutes, and then placing it in an ultrasonic device II for 50 minutes to obtain artificial crystal synthetic mica; the frequency of the ultrasonic device I is 20kHz, the power is 260W, the frequency of the ultrasonic device II is 20kHz, and the power is 300W; the amount ratio of the flaky synthetic mica, water, ethanol, and sodium citrate is 18.7g:100mL:55mL:0.015g, and the volume fraction of ethanol is 95%.

[0018] Example 6: The artificial crystal synthetic mica is prepared by the following steps: Step S1: crush the molybdenum tailings, pass them through a 40-mesh sieve, and then put them into a magnetic field screening machine and screen them for 60 minutes under the condition of a magnetic moment of 140 mm to obtain the iron-removed molybdenum tailings; the amount of molybdenum tailings used is 120 g; Step S2: adding the iron-removed molybdenum tailings, potassium carbonate, potassium feldspar, magnesium oxide, aluminum oxide, montmorillonite, silicon dioxide, sodium fluorosilicate and the potassium fluorosilicate obtained in Example 3 into a mechanical mixer and mixing for 1.5 hours, with the feeding temperature being 1200° C., the melting temperature being 1460° C., and keeping the temperature for 2 hours, then cooling to 1250° C. at a cooling rate of 3° C. / min, keeping the temperature for 2 hours, sealing with a cover, cooling to room temperature with the furnace, and continuing to mix for 30 minutes to obtain flaky synthetic mica; the amount ratio of the iron-removed molybdenum tailings, potassium carbonate, potassium feldspar, magnesium oxide, aluminum oxide, montmorillonite, silicon dioxide, sodium fluorosilicate and potassium fluorosilicate is 60g:1.9g:0.9g:8.5g:4.7g:14.9g:5.9g:2.8g:13.1g; Step S3: adding flaky synthetic mica to water, mixing for 20 minutes to obtain a suspension, adding ethanol and sodium citrate to the suspension, mixing for 30 minutes, placing it in an ultrasonic device I for 20 minutes, and then placing it in an ultrasonic device II for 60 minutes to obtain artificial crystal synthetic mica; the frequency of the ultrasonic device I is 20kHz, the power is 260W, the frequency of the ultrasonic device II is 20kHz, and the power is 300W; the amount ratio of the flaky synthetic mica, water, ethanol, and sodium citrate is 18.7g:100mL:60mL:0.02g, and the volume fraction of ethanol is 95%.

[0019] Comparative Example 1 This comparative example is commercially available artificial crystal synthetic mica.

[0020] Comparative Example 2 Compared with Example 6, the potassium fluorosilicate was replaced with commercially available potassium fluorosilicate, and the other procedures were exactly the same as Example 6 to obtain artificial crystal synthetic mica.

[0021] Comparative Example 3 Compared with Example 6, the ultrasonic exfoliation and refinement method is replaced by a wheel mill mechanical crushing method, and the rest is exactly the same as Example 6 to obtain artificial crystal synthetic mica.

[0022] The artificial crystal synthetic mica prepared by the present invention is further tested for its effect, and the test results are as follows.

[0023] In order to test the artificial crystal synthetic mica prepared by the present invention, the performance was measured according to relevant standards, and the results are shown in Table 1.

[0024] Table 1: Example 4 Example 5 Example 6 Comparative Example 1 Comparative Example 2 Comparative Example 3 +4 mesh content% 82 85 88 75 87 85 -16 mesh content% 4 4 2 5 3 4 Impurity content% ≤1.2 ≤1.2 ≤1 5~10 ≤1 ≤1.1 Coarse whiteness % 82 82 85 72 84 83 Average diameter-thickness ratio 94 95 97 85 96 95 Powder physical indicators Soft, elastic and skin-friendly Soft, elastic and skin-friendly Soft, elastic and skin-friendly The chips are small, brittle and not tough The feel is good, soft, elastic and skin-friendly The feel is good, soft, elastic and skin-friendly Tensile strength (MPa) 135 145 150 100 148 146 According to the data in Table 1, compared with Example 1, Example 4, Example 5 and Example 6, it can be seen that the artificial crystal synthetic mica prepared by the present invention has excellent qualities such as very few impurity crystals, large crystals, good smoothness, flexibility and elasticity, and high tensile strength compared with commercially available artificial crystal synthetic mica; compared with Example 2, Example 6 shows that the artificial crystal synthetic mica prepared by using synthetic potassium fluorosilicate with suitable particle size, good fluidity and no agglomeration during long-term storage is of better quality; compared with Comparative Example 3, Example 6 shows that the artificial crystal synthetic mica obtained by using ultrasonic exfoliation and refinement method has better smoothness and a larger particle thickness ratio than mechanical crushing.

[0025] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A production process of artificial crystal synthetic mica, characterized by: The steps include: Step S1: crushing the molybdenum tailings, passing through a 40-mesh sieve, and then placing them in a magnetic field screening machine, screening them for 45-60 minutes under a magnetic moment of 130-140 mm to obtain iron-removed molybdenum tailings; Step S2: adding the iron-removed molybdenum tailings, potassium carbonate, potassium feldspar, magnesium oxide, aluminum oxide, montmorillonite, silicon dioxide, sodium fluorosilicate and potassium fluorosilicate into a mechanical mixer and mixing for 1-1.5 hours, with the feeding temperature being 1200° C., the melting temperature being 1460° C., and keeping the temperature for 2 hours, and then cooling the temperature to 1250° C. at a cooling rate of 2-3° C. / min, keeping the temperature for 2 hours, sealing the mixture, cooling it to room temperature with the furnace, and continuing to mix for 30 minutes to obtain flaky synthetic mica; Step S3: adding flaky synthetic mica into water, mixing for 15-20 minutes to obtain a suspension, adding ethanol and sodium citrate into the suspension, mixing for 20-30 minutes, placing it into an ultrasonic device I for 15-20 minutes, and then placing it into an ultrasonic device II for 40-60 minutes to obtain artificial crystal synthetic mica.

2. The production process of artificial crystal synthetic mica according to claim 1, characterized in that: The potassium fluorosilicate is prepared by the following steps: Step A1: potassium feldspar particles are mixed with sodium chloride powder and stirred for 20-30 minutes, then placed in an alumina crucible and heated in a high-temperature furnace at 850-950° C. for melting and leaching without stirring in the crucible. After 3.5-4 hours, the crucible is taken out, cooled and water is added to obtain a potassium feldspar leaching solution; Step A2: Slowly add the fluorosilicic acid solution and the potassium feldspar leaching solution into the synthesis tank at the same time, and then add potassium sulfate. The stirring speed of the synthesis tank is 120r / min, and the stirring is carried out at 50-55°C for 1.5-2h to obtain a slurry. The slurry is then filtered, washed, and dried at 100°C for 4-6h to obtain potassium fluorosilicate.

3. The production process of artificial crystal synthetic mica according to claim 1, characterized in that: In step S1, the amount of molybdenum tailings used is 80-120g.

4. The production process of artificial crystal synthetic mica according to claim 1, characterized in that: In step S2, the usage ratio of the molybdenum tailings for iron removal, potassium carbonate, potassium feldspar, magnesium oxide, aluminum oxide, montmorillonite, silicon dioxide, sodium fluorosilicate and potassium fluorosilicate is 40-60g: 1.9-2.7g: 0.9-1.3g: 8.5-13.1g: 4.7-7.1g: 14.9-23.1g: 5.9-16.4g: 2.8-2.9g: 13.1-13.4g.

5. The production process of artificial crystal synthetic mica according to claim 1, characterized in that: In step S3, the frequency of ultrasonic device I is 20kHz, the power is 260W, the frequency of ultrasonic device II is 20kHz, the power is 300W; the dosage ratio of flaky synthetic mica, water, ethanol, and sodium citrate is 18.7g:100mL:50-60mL:0.01-0.02g, and the volume fraction of ethanol is 95%.

6. The production process of artificial crystal synthetic mica according to claim 2, characterized in that: In step A1, the dosage ratio of potassium feldspar particles, sodium chloride powder and water is 100g:100g:210-230mL; the potassium concentration in the potassium feldspar leaching solution is 0.30-0.33mol / L.

7. The production process of artificial crystal synthetic mica according to claim 2, characterized in that: In step A2, the usage ratio of the fluorosilicic acid solution, the potassium feldspar leaching solution and the potassium sulfate is 100 mL: 190-200 mL: 0.15-0.25 g, and the concentration of the fluorosilicic acid solution is 0.25-0.30 mol / L.