A high-temperature magnesium oxide powder additive and magnesium powder preparation method and application

The composite granulation technology of nano-magnesium oxide and other materials coated with refired magnesium oxide, which solves the problem of unstable insulation performance and insufficient leakage current in heating pipes, and achieves efficient improvement of the performance of electrical magnesium oxide materials and extends the performance of the extended service life.

CN118724033BActive Publication Date: 2024-11-01FENGCHENG FENGHUA MAGNESIUM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411219784.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-01
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

Magnesium oxide has problems such as unstable insulation performance, insufficient leakage current and insufficient water resistance in heating pipes, resulting in safety hazards and short service life.

Method used

Nanomagnesium oxide, boron nitride, polyether ether ketone, cetriamyl bromide, stearamide propyldimethylbenzyl ammonium chloride, kaolin, alumina and silica were used to granulate and be mixed. Cook magnesium oxide for coating to form high-temperature magnesium oxide powder additives to improve its water resistance, insulation and current leakage resistance.

Benefits of technology

It significantly improves the water resistance, insulation and current leakage resistance of electrical magnesium oxide materials. The product quality is uniform, the thermal shock resistance is good, it is not easy to crack, and has a long service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to a high-temperature magnesium oxide powder additive and a magnesium powder preparation method and application, belonging to the technical field of magnesium oxide refractory electrical insulating materials, wherein the additive is prepared from nano magnesium oxide, boron nitride, polyetheretherketone, cetrimonium bromide, stearamidopropyl dimethyl benzyl ammonium chloride, kaolin, aluminum oxide, silicon dioxide and bisphenol A epoxy resin; wherein aluminum oxide, silicon dioxide, kaolin and bisphenol A epoxy resin are subjected to briquetting, baking, crushing and granulation to prepare component A; nano magnesium oxide, boron nitride, polyetheretherketone, stearamidopropyl dimethyl benzyl ammonium chloride, kaolin and bisphenol A epoxy resin are subjected to briquetting, baking, crushing and granulation to prepare component B; component A, component B and cetrimonium bromide are mixed to obtain the additive. The additive is used to coat heavy-burned magnesium oxide, which can greatly improve the water resistance, insulation and anti-current leakage performance of electrical magnesium oxide materials, and the product quality is uniform, the thermal shock resistance is good, it is not easy to break down, and the service life is long.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of magnesium oxide fire-resistant electrical insulating materials, and in particular relates to a high-temperature magnesium oxide powder additive and a magnesium powder preparation method and application. Background Art

[0002] In modern industry and daily life, heating tubes are widely used in various fields as a common heating equipment. As a key electrical material in heating tubes, magnesium oxide is mainly used as a refractory insulating material in electric heating equipment, especially as a filler in electric heating tubes. Its performance and characteristics play a vital role in the working efficiency, safety and service life of heating tubes. First of all, it must have good thermal conductivity at the working temperature so that heat can be quickly transferred to the surface of the tube, so that the resistance wire is closer to the temperature of the tube wall, thereby improving thermal efficiency. Secondly, it should have excellent insulation properties to ensure that it can effectively prevent current leakage in complex environments such as high temperature and ensure safe use. In addition, it must have a certain particle size, generally in a round shape. This shape is conducive to improving the filling density and fluidity, facilitating processing, and is not easy to damage the heating wire during processing.

[0003] There are many methods for preparing magnesium oxide, the most common ones are as follows:

[0004] 1. Magnesite calcination method: Magnesite is calcined at high temperature to decompose carbon dioxide to obtain magnesium oxide. This method has a wide range of raw materials, but the purity of the obtained magnesium oxide is relatively low.

[0005] 2. Brine ammonia method: brine is used as raw material, and ammonia water is added to cause precipitation reaction to generate magnesium hydroxide, which is then calcined to obtain magnesium oxide. The magnesium oxide prepared by this method has a higher purity, but the process is relatively complicated.

[0006] 3. Dolomite carbonization method: First, calcine and decompose the dolomite, then use carbon dioxide for carbonization, and finally thermally decompose it to obtain magnesium oxide. This method has a low cost, but the product quality is greatly affected by the raw materials.

[0007] Due to the limitations of raw materials and processes, although magnesium oxide has important applications in heating tubes, there are still some problems to be solved:

[0008] (1) Decreased stability of insulation performance: Under high temperature and complex environment, the insulation performance of magnesium oxide may decrease, thereby increasing the risk of leakage and short circuit.

[0009] (2) Insufficient protection against leakage current: The heating tube will experience frequent temperature changes during operation. Under high temperature conditions, there is a risk of leakage current and even safety accidents.

[0010] (3) Insufficient water resistance: Under the conditions of liquid heating, magnesium oxide is easily corroded by water and other liquids, reducing its stability in use.

[0011] In order to improve the performance of magnesium oxide as an electrical material for heating tubes, some additives are usually added, such as boron compounds, metal oxides, insulating chemicals, etc., to prevent leakage current, improve thermal conductivity, enhance insulation performance, improve thermal shock resistance, etc. However, it is difficult to improve the characteristics of magnesium oxide powder itself by simply mixing and adding various ingredients. The improvement in performance is still limited and it is difficult to meet the ever-increasing performance requirements of heating tubes for electrical grade magnesium oxide powder. Summary of the invention

[0012] The existing magnesium oxide has the above-mentioned various performance deficiencies due to the limitations of raw materials and processes, and it is difficult to improve the characteristics of the magnesium oxide powder itself even with additives. The performance improvement is still limited, and it is difficult to meet the ever-increasing performance requirements of electrical grade magnesium oxide powder for heating tubes. The present invention provides a high-temperature magnesium oxide powder additive and a method for preparing and using magnesium powder. The additive is prepared by mixing nano-magnesium oxide, boron nitride, polyetheretherketone, cetrimonium bromide, stearamidopropyl dimethylbenzyl ammonium chloride, kaolin, alumina, silicon dioxide and bisphenol A epoxy resin through composite granulation. The additive is used to coat modified heavy-burned magnesium oxide, which can greatly improve the water resistance, insulation and anti-current leakage performance of electrical magnesium oxide materials, and the product quality is uniform, thermal shock resistance is good, not easy to crack, and has a long service life. The specific technical scheme is as follows:

[0013] A high-temperature magnesium oxide powder additive, the additive is made of the following raw materials in parts by mass: 10 to 15 parts of nano magnesium oxide, 20 to 25 parts of boron nitride, 1 to 3 parts of polyetheretherketone, 0.3 to 0.5 parts of cetrimonium bromide, 0.5 to 1 parts of stearamidopropyl dimethylbenzyl ammonium chloride, 20 to 25 parts of kaolin, 5 to 8 parts of aluminum oxide, 6 to 10 parts of silicon dioxide and 5 to 8 parts of bisphenol A epoxy resin;

[0014] The preparation method of the additive comprises the following steps:

[0015] S1: Alumina, silicon dioxide, 50% by mass of kaolin, and 50% by mass of bisphenol A epoxy resin are mixed, briquetted, baked at 350°C to 400°C for 1h to 2h, cooled, and crushed to obtain granulated material I; granulated material I is dry-milled for 30min to 40min, then a ball milling aid is added to wet-mill for 5min to 8min, and after drying, component A is obtained;

[0016] S2: Nano magnesium oxide, boron nitride, polyetheretherketone, stearamidopropyl dimethylbenzyl ammonium chloride, 50% by weight of kaolin, and 50% by weight of bisphenol A epoxy resin are mixed, briquetted, baked at 300°C to 320°C for 1h to 2h, cooled, crushed, dry-milled for 30min to 40min, then a ball milling aid is added for wet-milling for 5min to 8min, and dried to obtain component B;

[0017] S3: Mix component A, component B and cetrimide according to parts by mass to obtain an additive.

[0018] In the above technical solution, the nano magnesium oxide is dead-burned magnesium oxide with a particle size of nanometers; the dead-burned magnesium oxide is obtained by calcining magnesite at 1700°C to 1900°C for 8h to 10h, crushing and classifying.

[0019] In the above technical solution, the particle size of boron nitride is nanometer level.

[0020] In the above technical solution, the particle size of polyetheretherketone is nanometer level.

[0021] In the above technical solution, the median particle size of cetrimonium bromide is less than 30 μm.

[0022] In the above technical solution, the median particle size of stearamidopropyl dimethylbenzyl ammonium chloride is less than 10 μm.

[0023] In the above technical solution, the median particle size of kaolin is less than 10 μm.

[0024] In the above technical solution, the median particle size of aluminum oxide is less than 15 μm.

[0025] In the above technical solution, the median particle size of silicon dioxide is less than 15 μm.

[0026] In the above technical solution, the median particle size of the bisphenol A epoxy resin is less than 2 μm.

[0027] In S1 of the above technical solution, the median particle size of the crushed material is 20 μm to 30 μm.

[0028] In S2 of the above technical solution, the median particle size of the crushed material is 10 μm to 15 μm.

[0029] In the above technical solution, the mass ratio of the components of the ball milling aid is hot water: stearyl trimethyl ammonium chloride: polyvinyl alcohol = 100: (5-8): (3-5), and the temperature of the hot water is 60°C to 80°C.

[0030] In S1 of the above technical solution, the amount of ball milling aid added is 8% to 12% of the mass of granulated material I.

[0031] In S2 of the above technical solution, the amount of ball milling aid added is 6% to 10% of the mass of granulated material II.

[0032] A method for preparing high-temperature magnesium oxide powder, using the above-mentioned high-temperature magnesium oxide powder additive, the preparation method comprises the following steps:

[0033] According to the mass ratio, dead-burned magnesium oxide: additive: thermosetting resin = (100-120): (5-8): (3-5), the dead-burned magnesium oxide, additive and thermosetting resin are mixed, dry ball milled for 40-50 minutes, modified at 260-280°C for 2-3 hours to obtain dead-burned magnesium oxide coated with additives and thermosetting resin, cooled, broken up, sieved, and the sieved material is taken to obtain high-temperature magnesium oxide powder.

[0034] In the preparation method of the above-mentioned high-temperature magnesium oxide powder, the dead-burned magnesium oxide is obtained by calcining dolomite at 1700°C to 1900°C for 8h to 10h; the particle size classification of the dead-burned magnesium oxide is 60 mesh>particle size ≥80 mesh, accounting for 10 to 20 parts by mass, 80 mesh>particle size ≥100 mesh, accounting for 30 to 40 parts by mass, 100 mesh>particle size ≥250 mesh, accounting for 25 to 35 parts by mass, 250 mesh>particle size ≥325 mesh, accounting for 5 to 10 parts by mass, and 325 mesh>particle size, accounting for 1 to 5 parts by mass; the thermosetting resin is phenolic resin or epoxy resin, and the median particle size of the thermosetting resin is less than 2μm.

[0035] In the above-mentioned method for preparing high-temperature magnesium oxide powder, the modified stirring speed is 80 rpm to 120 rpm.

[0036] In the above-mentioned preparation method of high-temperature magnesium oxide powder, the mesh number of the sieve is 60 meshes.

[0037] The high-temperature magnesium oxide powder is used to prepare heating tubes.

[0038] The high-temperature magnesium oxide powder additive and magnesium powder preparation method and application provided by the present invention have the following beneficial effects compared with the prior art:

[0039] 1. The additive of the present invention is prepared by mixing nano magnesium oxide, boron nitride, polyetheretherketone, cetrimide, stearamidopropyl dimethylbenzyl ammonium chloride, kaolin, aluminum oxide, silicon dioxide and bisphenol A epoxy resin through composite granulation. The additive is used to coat modified dead-burned magnesium oxide, which can greatly improve the water resistance, insulation and anti-current leakage performance of electrical magnesium oxide materials. The product has uniform quality, good thermal shock resistance, not easy to crack, high hot pressure resistance, not easy to break down, and long service life.

[0040] 2. Component A in the additive is prepared by pressing alumina, silica, kaolin and bisphenol A epoxy resin into blocks, baking at 350℃~400℃, and crushing and granulating. The pressing and granulating of alumina, silica, kaolin and bisphenol A epoxy resin can achieve a good combination of alumina, silica and kaolin, and change the characteristics of the granulated particles. Among them, alumina improves the insulation and thermal conductivity of the granulated particles; silica improves the strength of the granulated particles, reduces the expansion rate, and reduces the hygroscopicity; kaolin can improve the fire retardancy of the granulated particles. At the same time, kaolin and bisphenol A epoxy resin are used together to have a good pressing and molding effect, so that the components are more closely combined after the pressing and baking, and then after crushing, a good granulation effect can be achieved. The baking temperature is designed according to the temperature resistance characteristics of each component.

[0041] In addition, after crushing, dry ball milling is carried out for 30 minutes to 40 minutes, which can well arrange the morphology of the granulated particles, making them more round, increasing the tap density of the material, and increasing the filling density and fluidity. When the heating tube is prepared later, the strength is better and the thermal shock resistance is good; the hot pressure resistance is high and it is not easy to be punctured.

[0042] 3. Component B in the additive is prepared by pressing nano magnesium oxide, boron nitride, polyetheretherketone, stearamidopropyl dimethylbenzyl ammonium chloride, kaolin and bisphenol A epoxy resin into blocks, baking at 300℃~320℃, and crushing and granulating. The composite granulation particles with excellent properties can be obtained by composite granulation of various components. Among them, nano magnesium oxide has the function of improving the high temperature resistance of composite granulated particles, and boron nitride has the function of improving the insulation, thermal conductivity and chemical corrosion resistance of composite granulated particles; polyetheretherketone can improve the insulation, water resistance and current leakage resistance of composite granulated particles, as well as improve the hardness, impact resistance, creep resistance, corrosion resistance and flame retardancy of granulated particles, improve hot pressure resistance and make them not easy to break down; stearamidopropyl dimethyl benzyl ammonium chloride has the function of improving the insulation and current leakage resistance of granulated particles, and stearamidopropyl dimethyl benzyl ammonium chloride has the function of promoting mixing homogeneity, preventing uneven dispersion of nano magnesium oxide and nano boron nitride, leading to uneven thermal stress, poor thermal shock resistance, cracking of heating tubes and other problems. Kaolin can improve fire retardancy, and kaolin is used in combination with bisphenol A epoxy resin, which has a good briquetting effect, so that the components are more closely combined after briquetting and then can achieve a good granulation effect after crushing. The baking temperature is designed according to the temperature resistance characteristics of each component.

[0043] In addition, after crushing, dry ball milling is carried out for 30 minutes to 40 minutes, which can well arrange the morphology of the granulated particles, making them more round, increasing the tap density of the material, and increasing the filling density and fluidity. When the heating tube is prepared later, the strength is better and the thermal shock resistance is good; the hot pressure resistance is high and it is not easy to be punctured.

[0044] Fourth, the present invention granulates component A and component B separately according to the temperature resistance characteristics of different components, so as to realize baking granulation at different temperatures. Separate granulation can ensure that the types of components of the granulated particles are not too many, and prevent uneven mixing caused by too many components, which makes it difficult to achieve a granulation effect with good homogeneity and high firmness.

[0045] 5. Component A, component B and cetrimonium bromide are mixed to obtain an additive. Adding cetrimonium bromide has the effect of improving the insulation and anti-current leakage of the material, and improving the hot withstand voltage. In addition, cetrimonium bromide plays an antistatic and dispersing role. When the subsequent additives coat the dead-burned magnesium oxide, the cetrimonium bromide component can improve the coating effect and promote more uniform coating modification mixing and surface adhesion.

[0046] 6. Modify at 260℃~280℃ for 2h~3h to obtain dead-burned magnesium oxide coated with additives and thermosetting resin. Coating modification can reduce the amount of additives and ensure the high content of dead-burned magnesium oxide; and the additives are coated on the surface of dead-burned magnesium oxide particles to form modified particles with core-shell structure, which can change the original characteristics of dead-burned magnesium oxide particles. The modified dead-burned magnesium oxide particles have excellent performance in electrical products. The design of the modification temperature and the modified stirring speed is designed according to the characteristics of each component in the additive.

[0047] 7. The present invention also designs the particle size distribution of dead-burned magnesium oxide to be 60 mesh> particle size ≥ 80 mesh, accounting for 10 to 20 parts by mass, 80 mesh> particle size ≥ 100 mesh, accounting for 30 to 40 parts by mass, 100 mesh> particle size ≥ 250 mesh, accounting for 25 to 35 parts by mass, 250 mesh> particle size ≥ 325 mesh, accounting for 5 to 10 parts by mass, and 325 mesh> particle size, accounting for 1 to 5 parts by mass. The particle size distribution, combined with the surface coating modification treatment of the additive, is used to prepare the heating tube, which has good mechanical properties, high strength, good thermal shock resistance, high hot pressure resistance, and is not easy to break down.

[0048] 8. The additive of the present invention contains polyetheretherketone, cetrimide bromide, and stearamidopropyl dimethylbenzyl ammonium chloride at the same time; and component A and component B are designed to be granulated in advance, and then mixed with cetrimide bromide to prepare the additive; the additive is used to coat and modify the dead-burned magnesium oxide, and an electrical magnesium oxide material with greatly improved performance can be obtained, thereby realizing the preparation of high-quality electrical magnesium oxide materials, and having good practical value.

[0049] 9. The present invention designs granulation material I and granulation material II to be wet ball milled. Wet ball milling can promote the morphology of the granules to be smoother, and can condense the ultrafine powder produced by dry ball milling, so that it can agglomerate large particles and reduce the output of ultrafine powder, which helps to increase the tap density of the material, and then can increase the compaction density of the material, improve the insulation and anti-current leakage performance; in addition, the ball milling aid component can promote the mixing of component A and component B to achieve good homogeneity, and improve the homogeneous quality of the material; in the subsequent preparation of high-temperature magnesium oxide powder, the stearyl trimethyl ammonium chloride and polyvinyl alcohol in the ball milling aid participate in the modification, which helps to improve the homogeneity and coating effect, the quality uniformity is good, and the modified coating film is more firm, further improving the insulation and anti-current leakage performance. DETAILED DESCRIPTION

[0050] The present invention is further described below in conjunction with specific implementation cases, but the present invention is not limited to these embodiments.

[0051] Example 1

[0052] A high-temperature magnesium oxide powder additive, the additive is made of the following raw materials in parts by mass: 12 parts of nano magnesium oxide, 23 parts of boron nitride, 2 parts of polyetheretherketone, 0.4 parts of cetrimonium bromide, 0.8 parts of stearamidopropyl dimethylbenzyl ammonium chloride, 22 parts of kaolin, 6.5 parts of aluminum oxide, 8 parts of silicon dioxide and 6.5 parts of bisphenol A epoxy resin;

[0053] Among them, nano magnesium oxide is dead-burned magnesium oxide with a particle size of nanometers; dead-burned magnesium oxide is dead-burned magnesium oxide obtained by calcining dolomite at 1800°C for 9 hours, crushing and grading; the particle size of boron nitride is nanometers; the particle size of polyetheretherketone is nanometers; the median particle size of cetrimonium bromide is 26.5μm; the median particle size of stearamidopropyl dimethylbenzyl ammonium chloride is 8.3μm; the median particle size of kaolin is 7.9μm; the median particle size of alumina is 13.2μm; the median particle size of silica is 12.6μm; the median particle size of bisphenol A epoxy resin is 1.4μm.

[0054] The preparation method of the additive comprises the following steps:

[0055] S1: Alumina, silica, 50% by mass of kaolin, and 50% by mass of bisphenol A epoxy resin were mixed, briquetted, baked at 380°C for 1.5 hours, cooled, and crushed into powder with a median particle size of 26.4 μm to obtain granulation material I; granulation material I was dry-milled for 35 minutes, and then 10% by mass of ball milling aid of granulation material I was added for wet ball milling for 6 minutes, and after drying, component A was obtained;

[0056] S2: Nano magnesium oxide, boron nitride, polyetheretherketone, stearamidopropyl dimethylbenzyl ammonium chloride, 50% by mass of kaolin, and 50% by mass of bisphenol A epoxy resin were mixed, briquetted, baked at 310°C for 1.5h, cooled, and crushed into powder with a median particle size of 12.5μm to obtain granulation material II; granulation material II was dry-milled for 35min, and then 8% by mass of ball milling aid of granulation material II was added for wet ball milling for 6min, and after drying, component B was obtained;

[0057] S3: Mix component A, component B and cetrimide according to parts by mass to obtain an additive.

[0058] The mass ratio of the components of the ball milling aid is hot water: stearyl trimethyl ammonium chloride: polyvinyl alcohol = 100: 6.5: 4, and the temperature of the hot water is 70°C.

[0059] A method for preparing high-temperature magnesium oxide powder, using the above-mentioned high-temperature magnesium oxide powder additive, the preparation method comprises the following steps:

[0060] According to the mass ratio of dead-burned magnesium oxide: additive: thermosetting resin = 110:7:4, the dead-burned magnesium oxide, additive and phenolic resin with a median particle size of 1.6 μm are mixed, dry ball milled for 45 minutes, modified at 270°C for 2.5 hours, and the modified stirring speed is 100 rpm to obtain dead-burned magnesium oxide coated with additives and thermosetting resin, cooled, broken up, passed through a 60-mesh sieve, and the sieve under the sieve is taken to obtain high-temperature magnesium oxide powder;

[0061] Among them, the dead-burned magnesium oxide is the dead-burned magnesium oxide obtained by calcining magnesite at 1800°C for 9 hours; the particle size grading of the dead-burned magnesium oxide is as follows: 60 mesh>particle size ≥80 mesh accounts for 15 parts by mass, 80 mesh>particle size ≥100 mesh accounts for 35 parts by mass, 100 mesh>particle size ≥250 mesh accounts for 30 parts by mass, 250 mesh>particle size ≥325 mesh accounts for 7 parts by mass, and 325 mesh>particle size accounts for 3 parts by mass.

[0062] The high-temperature magnesium oxide powder of this embodiment is used to prepare a heating tube.

[0063] Example 2

[0064] A high-temperature magnesium oxide powder additive, the additive is made of the following raw materials in parts by mass: 10 parts of nano magnesium oxide, 20 parts of boron nitride, 1 part of polyetheretherketone, 0.3 parts of cetrimonium bromide, 0.5 parts of stearamidopropyl dimethylbenzyl ammonium chloride, 20 parts of kaolin, 5 parts of aluminum oxide, 6 parts of silicon dioxide and 5 parts of bisphenol A epoxy resin;

[0065] Among them, nano magnesium oxide is dead-burned magnesium oxide with a particle size of nanometers; dead-burned magnesium oxide is dead-burned magnesium oxide obtained by calcining dolomite at 1700°C for 8 hours, crushing and grading; the particle size of boron nitride is nanometers; the particle size of polyetheretherketone is nanometers; the median particle size of cetrimonium bromide is 18.6μm; the median particle size of stearamidopropyl dimethylbenzyl ammonium chloride is 7.5μm; the median particle size of kaolin is 6.4μm; the median particle size of alumina is 14.1μm; the median particle size of silica is 12.7μm; the median particle size of bisphenol A epoxy resin is 1.3μm.

[0066] The preparation method of the additive comprises the following steps:

[0067] S1: Alumina, silicon dioxide, 50% by mass of kaolin, and 50% by mass of bisphenol A epoxy resin were mixed, briquetted, baked at 350°C for 1 hour, cooled, and crushed into powder with a median particle size of 20.0 μm to obtain granulation material I; granulation material I was dry-milled for 30 minutes, and then 8% by mass of ball milling aid of granulation material I was added for wet ball milling for 5 minutes, and after drying, component A was obtained;

[0068] S2: Nano magnesium oxide, boron nitride, polyetheretherketone, stearamidopropyl dimethylbenzyl ammonium chloride, 50% by mass of kaolin, and 50% by mass of bisphenol A epoxy resin are mixed, briquetted, baked at 300°C for 1h, cooled, and crushed into powder with a median particle size of 11.3μm to obtain granulation material II; granulation material II is dry-milled for 30min, and then 6% by mass of ball milling aid of granulation material II is added for wet ball milling for 5min, and after drying, component B is obtained;

[0069] S3: Mix component A, component B and cetrimide according to parts by mass to obtain an additive.

[0070] The mass ratio of the components of the ball milling aid is hot water: stearyl trimethyl ammonium chloride: polyvinyl alcohol = 100:5:3, and the temperature of the hot water is 60°C.

[0071] A method for preparing high-temperature magnesium oxide powder, using the above-mentioned high-temperature magnesium oxide powder additive, the preparation method comprises the following steps:

[0072] According to the mass ratio of dead-burned magnesium oxide: additive: thermosetting resin = 100:5:3, the dead-burned magnesium oxide, additive and epoxy resin with a median particle size of 1.8 μm are mixed, dry ball milled for 40 minutes, modified at 260°C for 2 hours, and the modified stirring speed is 80 rpm to obtain dead-burned magnesium oxide coated with additives and thermosetting resin, cooled, broken up, passed through a 60-mesh sieve, and the sieve under the sieve is taken to obtain high-temperature magnesium oxide powder;

[0073] Among them, the dead-burned magnesium oxide is the dead-burned magnesium oxide obtained by calcining magnesite at 1700°C for 8 hours; the particle size grading of the dead-burned magnesium oxide is as follows: 60 mesh>particle size ≥80 mesh accounts for 10 parts by mass, 80 mesh>particle size ≥100 mesh accounts for 30 parts by mass, 100 mesh>particle size ≥250 mesh accounts for 25 parts by mass, 250 mesh>particle size ≥325 mesh accounts for 5 parts by mass, and 325 mesh>particle size accounts for 1 part by mass.

[0074] The high-temperature magnesium oxide powder of this embodiment is used to prepare a heating tube.

[0075] Example 3

[0076] A high-temperature magnesium oxide powder additive, the additive is made of the following raw materials in parts by mass: 11 parts of nano magnesium oxide, 21 parts of boron nitride, 1.5 parts of polyetheretherketone, 0.35 parts of cetrimonium bromide, 0.6 parts of stearamidopropyl dimethylbenzyl ammonium chloride, 21 parts of kaolin, 6 parts of aluminum oxide, 7 parts of silicon dioxide and 6 parts of bisphenol A epoxy resin;

[0077] Among them, nano magnesium oxide is dead-burned magnesium oxide with a nanometer particle size; dead-burned magnesium oxide is dead-burned magnesium oxide obtained by calcining dolomite at 1750°C for 8.5 hours, crushing and grading; the particle size of boron nitride is nanometer-scale; the particle size of polyetheretherketone is nanometer-scale; the median particle size of cetrimonium bromide is 15.0μm; the median particle size of stearamidopropyl dimethylbenzyl ammonium chloride is 7.3μm; the median particle size of kaolin is 5.4μm; the median particle size of alumina is 8.7μm; the median particle size of silicon dioxide is 9.8μm; the median particle size of bisphenol A epoxy resin is 0.9μm.

[0078] The preparation method of the additive comprises the following steps:

[0079] S1: Alumina, silicon dioxide, 50% by mass of kaolin, and 50% by mass of bisphenol A epoxy resin were mixed, briquetted, baked at 360°C for 1 hour, cooled, and crushed into powder with a median particle size of 22.4 μm to obtain granulation material I; granulation material I was dry-milled for 30 minutes, and then 9% by mass of ball milling aid of granulation material I was added for wet ball milling for 6 minutes, and after drying, component A was obtained;

[0080] S2: Nano magnesium oxide, boron nitride, polyetheretherketone, stearamidopropyl dimethylbenzyl ammonium chloride, 50% by mass of kaolin, and 50% by mass of bisphenol A epoxy resin are mixed, briquetted, baked at 305°C for 1 hour, cooled, and crushed into a powder with a median particle size of 10.0 μm to obtain granulation material II; granulation material II is dry-milled for 30 minutes, and then 7% by mass of ball milling aid of granulation material II is added for wet ball milling for 6 minutes, and after drying, component B is obtained;

[0081] S3: Mix component A, component B and cetrimide according to parts by mass to obtain an additive.

[0082] The mass ratio of the components of the ball milling aid is hot water: stearyl trimethyl ammonium chloride: polyvinyl alcohol = 100:6:3.5, and the temperature of the hot water is 65°C.

[0083] A method for preparing high-temperature magnesium oxide powder, using the above-mentioned high-temperature magnesium oxide powder additive, the preparation method comprises the following steps:

[0084] According to the mass ratio of dead-burned magnesium oxide: additive: thermosetting resin = 105:6:3.5, the dead-burned magnesium oxide, additive and phenolic resin with a median particle size of 1.7 μm are mixed, dry ball milled for 40 minutes, modified at 265°C for 2 hours, and the modified stirring speed is 90 rpm to obtain dead-burned magnesium oxide coated with additives and thermosetting resin, cooled, broken up, passed through a 60-mesh sieve, and the sieve under the sieve is taken to obtain high-temperature magnesium oxide powder;

[0085] Among them, the dead-burned magnesium oxide is the dead-burned magnesium oxide obtained by calcining magnesite at 1750°C for 8.5 hours; the particle size grading of the dead-burned magnesium oxide is as follows: 60 mesh>particle size ≥80 mesh accounts for 12 parts by mass, 80 mesh>particle size ≥100 mesh accounts for 32 parts by mass, 100 mesh>particle size ≥250 mesh accounts for 28 parts by mass, 250 mesh>particle size ≥325 mesh accounts for 6 parts by mass, and 325 mesh>particle size accounts for 2 parts by mass.

[0086] The high-temperature magnesium oxide powder of this embodiment is used to prepare a heating tube.

[0087] Example 4

[0088] A high-temperature magnesium oxide powder additive, the additive is made of the following raw materials in parts by mass: 14 parts of nano magnesium oxide, 24 parts of boron nitride, 2.5 parts of polyetheretherketone, 0.45 parts of cetrimonium bromide, 0.8 parts of stearamidopropyl dimethylbenzyl ammonium chloride, 24 parts of kaolin, 7 parts of aluminum oxide, 9 parts of silicon dioxide and 7 parts of bisphenol A epoxy resin;

[0089] Among them, nano magnesium oxide is dead-burned magnesium oxide with a particle size of nanometers; dead-burned magnesium oxide is dead-burned magnesium oxide obtained by calcining dolomite at 1850°C for 9.5 hours, crushing and grading; the particle size of boron nitride is nanometers; the particle size of polyetheretherketone is nanometers; the median particle size of cetrimonium bromide is 28.4μm; the median particle size of stearamidopropyl dimethylbenzyl ammonium chloride is 9.1μm; the median particle size of kaolin is 8.1μm; the median particle size of alumina is 13.2μm; the median particle size of silicon dioxide is 12.7μm; the median particle size of bisphenol A epoxy resin is 1.9μm.

[0090] The preparation method of the additive comprises the following steps:

[0091] S1: Alumina, silicon dioxide, 50% by mass of kaolin, and 50% by mass of bisphenol A epoxy resin were mixed, briquetted, baked at 390°C for 2h, cooled, and crushed into powder with a median particle size of 30.0μm to obtain granulation material I; granulation material I was dry-milled for 40min, and then 10% by mass of ball milling aid of granulation material I was added for wet ball milling for 7min, and after drying, component A was obtained;

[0092] S2: Nano magnesium oxide, boron nitride, polyetheretherketone, stearamidopropyl dimethylbenzyl ammonium chloride, 50% by mass of kaolin, and 50% by mass of bisphenol A epoxy resin are mixed, briquette, baked at 315°C for 2h, cooled, and crushed into a powder with a median particle size of 14.2μm to obtain granulation material II; granulation material II is dry ball-milled for 40min, and then 9% by mass of ball milling aid of granulation material II is added for wet ball milling for 7min, and after drying, component B is obtained;

[0093] S3: Mix component A, component B and cetrimide according to parts by mass to obtain an additive.

[0094] The mass ratio of the components of the ball milling aid is hot water: stearyl trimethyl ammonium chloride: polyvinyl alcohol = 100:7:4.5, and the temperature of the hot water is 75°C.

[0095] A method for preparing high-temperature magnesium oxide powder, using the above-mentioned high-temperature magnesium oxide powder additive, the preparation method comprises the following steps:

[0096] According to the mass ratio of dead-burned magnesium oxide: additive: thermosetting resin = 115:7:4.5, the dead-burned magnesium oxide, additive and epoxy resin with a median particle size of 1.3 μm are mixed, dry ball milled for 50 minutes, modified at 275°C for 3 hours, and the modified stirring speed is 110 rpm to obtain dead-burned magnesium oxide coated with additives and thermosetting resin, cooled, broken up, passed through a 60-mesh sieve, and the sieve under the sieve is taken to obtain high-temperature magnesium oxide powder;

[0097] Among them, the dead-burned magnesium oxide is the dead-burned magnesium oxide obtained by calcining magnesite at 1850°C for 9.5 hours; the particle size grading of the dead-burned magnesium oxide is as follows: 60 mesh>particle size ≥80 mesh accounts for 18 parts by mass, 80 mesh>particle size ≥100 mesh accounts for 38 parts by mass, 100 mesh>particle size ≥250 mesh accounts for 32 parts by mass, 250 mesh>particle size ≥325 mesh accounts for 8 parts by mass, and 325 mesh>particle size accounts for 4 parts by mass.

[0098] The high-temperature magnesium oxide powder of this embodiment is used to prepare a heating tube.

[0099] Example 5

[0100] A high-temperature magnesium oxide powder additive, the additive is made of the following raw materials in parts by mass: 15 parts of nano magnesium oxide, 25 parts of boron nitride, 3 parts of polyetheretherketone, 0.5 parts of cetrimonium bromide, 1 part of stearamidopropyl dimethylbenzyl ammonium chloride, 25 parts of kaolin, 8 parts of aluminum oxide, 10 parts of silicon dioxide and 8 parts of bisphenol A epoxy resin;

[0101] Among them, nano magnesium oxide is dead-burned magnesium oxide with a particle size of nanometers; dead-burned magnesium oxide is dead-burned magnesium oxide obtained by calcining dolomite at 1900°C for 10 hours, crushing and grading; the particle size of boron nitride is nanometers; the particle size of polyetheretherketone is nanometers; the median particle size of cetrimonium bromide is 17.5μm; the median particle size of stearamidopropyl dimethylbenzyl ammonium chloride is 9.2μm; the median particle size of kaolin is 8.1μm; the median particle size of alumina is 14.7μm; the median particle size of silica is 14.1μm; the median particle size of bisphenol A epoxy resin is 1.2μm.

[0102] The preparation method of the additive comprises the following steps:

[0103] S1: Alumina, silica, 50% by mass of kaolin and 50% by mass of bisphenol A epoxy resin were mixed, briquetted, baked at 400°C for 2h, cooled, and crushed into powder with a median particle size of 24.7μm to obtain granulation material I; granulation material I was dry-milled for 40min, and then 12% by mass of ball milling aid of granulation material I was added for wet ball milling for 8min, and after drying, component A was obtained;

[0104] S2: Nano magnesium oxide, boron nitride, polyetheretherketone, stearamidopropyl dimethylbenzyl ammonium chloride, 50% by mass of kaolin, and 50% by mass of bisphenol A epoxy resin are mixed, briquette, baked at 320°C for 2h, cooled, and crushed into a powder with a median particle size of 15.0μm to obtain granulation material II; granulation material II is dry ball-milled for 40min, and then 10% by mass of ball milling aid of granulation material II is added for wet ball milling for 8min, and after drying, component B is obtained;

[0105] S3: Mix component A, component B and cetrimide according to parts by mass to obtain an additive.

[0106] The mass ratio of the components of the ball milling aid is hot water: stearyl trimethyl ammonium chloride: polyvinyl alcohol = 100:8:5, and the temperature of the hot water is 80°C.

[0107] A method for preparing high-temperature magnesium oxide powder, using the above-mentioned high-temperature magnesium oxide powder additive, the preparation method comprises the following steps:

[0108] According to the mass ratio of dead-burned magnesium oxide: additive: thermosetting resin = 120:8:5, the dead-burned magnesium oxide with a particle size of 100 mesh, the additive and the phenolic resin with a median particle size of 1.6 μm are mixed, dry ball milled for 50 minutes, modified at 280°C for 3 hours, and the modified stirring speed is 120 rpm to obtain the dead-burned magnesium oxide coated with the additive and the thermosetting resin, cooled, broken up, passed through a 60-mesh sieve, and the sieve under the sieve is taken to obtain high-temperature magnesium oxide powder;

[0109] Among them, the dead-burned magnesium oxide is the dead-burned magnesium oxide obtained by calcining magnesite at 1900°C for 10 hours; the particle size grading of the dead-burned magnesium oxide is as follows: 60 mesh>particle size ≥80 mesh accounts for 20 parts by mass, 80 mesh>particle size ≥100 mesh accounts for 40 parts by mass, 100 mesh>particle size ≥250 mesh accounts for 35 parts by mass, 250 mesh>particle size ≥325 mesh accounts for 10 parts by mass, and 325 mesh>particle size accounts for 5 parts by mass.

[0110] The high-temperature magnesium oxide powder of this embodiment is used to prepare a heating tube.

[0111] Comparative Example 1

[0112] No stearamidopropyl dimethylbenzyl ammonium chloride is added to the additive, that is, component B does not contain stearamidopropyl dimethylbenzyl ammonium chloride; other parameters and methods are the same as in Example 1.

[0113] Comparative Example 2

[0114] No granulation material is prepared, that is, component A and component B are not prepared. Nano magnesium oxide, boron nitride, polyetheretherketone, cetrimonium bromide, stearamidopropyl dimethylbenzylammonium chloride, kaolin, aluminum oxide, silicon dioxide and bisphenol A epoxy resin are directly mixed to obtain an additive; other parameters and methods are the same as in Example 1.

[0115] Comparative Example 3

[0116] In the additive, polyetheretherketone, cetrimonium bromide and stearamidopropyl dimethylbenzyl ammonium chloride are not added, that is, component B does not contain polyetheretherketone and stearamidopropyl dimethylbenzyl ammonium chloride; S3, mixing component A and component B to obtain an additive; other parameters and methods are the same as in Example 1.

[0117] Comparative Example 4

[0118] In the preparation method of high-temperature magnesium oxide powder, the additive does not coat and modify the dead-burned magnesium oxide, and the dead-burned magnesium oxide is directly mixed with the additive to obtain the high-temperature magnesium oxide powder; other parameters and methods are the same as in Example 1.

[0119] Comparative Example 5

[0120] No polyetheretherketone, cetrimonium bromide, or stearamidopropyl dimethylbenzyl ammonium chloride is added to the additive, that is, component B does not contain polyetheretherketone or stearamidopropyl dimethylbenzyl ammonium chloride; S3, mixing component A and component B to obtain the additive; in the preparation method of high-temperature magnesium oxide powder, the additive does not coat and modify the dead-burned magnesium oxide, and the dead-burned magnesium oxide is directly mixed with the additive to obtain the high-temperature magnesium oxide powder; other parameters and methods are the same as those in Example 1.

[0121] Comparative Example 6

[0122] In S1 and S2, wet ball milling is not performed, and no ball milling aid is added. Other parameters and methods are the same as those in Example 1.

[0123] According to the test method of "Electrical Grade Magnesium Oxide" JB / T 8508, the performance of the high temperature magnesium oxide powder prepared in the above embodiments and comparative examples was tested, wherein the leakage current was 9W / cm 2 The test results are shown in Table 1 below.

[0124] Table 1 Performance test results

[0125]

[0126] It can be seen from the above results that the high temperature magnesium oxide powder prepared by Examples 1 to 5 has excellent performance, low moisture absorption rate, low water resistance rate, good insulation, effective reduction of current leakage, improvement of hot withstand voltage, and is not easy to break down. As shown in the comparison of the results of Comparative Example 1, stearamidopropyl dimethyl benzyl ammonium chloride is used in additives, which can improve insulation, reduce current leakage, and improve withstand voltage. As shown in the comparison of the results of Comparative Example 2, no pre-granulation treatment is performed, and each component is directly mixed and used as an additive. The product is poor in terms of moisture absorption rate, water resistance rate, insulation, current leakage, hot withstand voltage, etc., indicating that component A and component B are pre-granulated, which helps to improve the overall performance of the product. From the comparison of the results of comparative example 3, it can be seen that without adding polyetheretherketone, cetrimonium bromide, and stearamidopropyl dimethylbenzyl ammonium chloride, the product's moisture absorption rate, anti-hydration rate, insulation and anti-current leakage performance are seriously affected. The use of polyetheretherketone, cetrimonium bromide and stearamidopropyl dimethylbenzyl ammonium chloride can greatly improve the product's moisture absorption rate, anti-hydration rate, insulation and anti-current leakage performance, high hot withstand voltage, and not easy to break down. From the comparison of the results of comparative example 4, it can be seen that the additive does not coat and modify the dead-burned magnesium oxide, the dead-burned magnesium oxide particles themselves do not have good performance changes, and the additive is mixed in small amounts. The product prepared after simple mixing has unsatisfactory performance indicators. From the comparison of the results of comparative example 5, it can be seen that polyetheretherketone, cetrimonium bromide, and stearamidopropyl dimethylbenzyl ammonium chloride are not added during the addition, and the additive does not coat and modify the dead-burned magnesium oxide, and the various performance indicators of the obtained product are greatly reduced. From the comparison of the results of Comparative Example 6, it can be seen that wet ball milling can promote the morphology of the granular material to be smoother, and can condense the ultrafine powder produced by dry ball milling, so that it can agglomerate large particles and reduce the output of ultrafine powder, which helps to increase the tap density of the material, and then can increase the compaction density of the material, improve the insulation and anti-current leakage performance; in addition, the ball milling aid component can promote the mixing of component A and component B to achieve good homogeneity, and improve the homogeneous quality of the material; in the subsequent preparation of high-temperature magnesium oxide powder, the stearyl trimethyl ammonium chloride and polyvinyl alcohol in the ball milling aid participate in the modification, which helps to improve the homogeneity and coating effect, the quality uniformity is good, and the modified coating film is more firm, further improving the insulation and anti-current leakage performance.

Claims

1. A high temperature magnesium oxide powder additive, characterized in that: The additive is made of the following raw materials in parts by mass: 10 to 15 parts of nano magnesium oxide, 20 to 25 parts of boron nitride, 1 to 3 parts of polyetheretherketone, 0.3 to 0.5 parts of cetrimonium bromide, 0.5 to 1 parts of stearamidopropyl dimethylbenzyl ammonium chloride, 20 to 25 parts of kaolin, 5 to 8 parts of aluminum oxide, 6 to 10 parts of silicon dioxide and 5 to 8 parts of bisphenol A epoxy resin; The preparation method of the additive comprises the following steps: S1: Alumina, silicon dioxide, 50% by mass of kaolin and 50% by mass of bisphenol A epoxy resin are mixed, briquetted, baked at 350°C to 400°C for 1h to 2h, cooled, and crushed to obtain granulation material I; granulation material I is dry-milled for 30min to 40min, and then 8% to 12% by mass of ball milling aid is added to wet-mill for 5min to 8min, and after drying, component A is obtained; S2: Nano magnesium oxide, boron nitride, polyetheretherketone, stearamidopropyl dimethylbenzyl ammonium chloride, 50% by mass of kaolin, and 50% by mass of bisphenol A epoxy resin are mixed, briquetted, baked at 300°C to 320°C for 1h to 2h, cooled, and crushed to obtain granulation material II; granulation material II is dry-milled for 30min to 40min, and then 6% to 10% by mass of ball milling aid of granulation material II is added for wet ball milling for 5min to 8min, and after drying, component B is obtained; S3: Mixing component A, component B and cetrimide according to parts by mass to obtain an additive; The mass ratio of the components of the ball milling aid is hot water: stearyl trimethyl ammonium chloride: polyvinyl alcohol = 100: (5-8): (3-5), and the temperature of the hot water is 60°C to 80°C.

2. A high temperature magnesium oxide powder additive according to claim 1, characterized in that: The nano magnesium oxide is dead-burned magnesium oxide with a nanometer particle size; the dead-burned magnesium oxide is obtained by calcining magnesite at 1700° C. to 1900° C. for 8 h to 10 h, crushing and classifying.

3. A high temperature magnesium oxide powder additive according to claim 1, characterized in that: The particle size of the boron nitride is nanometer-scale; the particle size of the polyetheretherketone is nanometer-scale; the median particle size of the cetrimonium bromide is less than 30 μm; the median particle size of the stearamidopropyl dimethylbenzyl ammonium chloride is less than 10 μm; the median particle size of the kaolin is less than 10 μm; the median particle size of the alumina is less than 15 μm; the median particle size of the silicon dioxide is less than 15 μm; and the median particle size of the bisphenol A epoxy resin is less than 2 μm.

4. A high temperature magnesium oxide powder additive according to claim 1, characterized in that: In S1, the median particle size of the pulverized material is 20 μm to 30 μm.

5. The high temperature magnesium oxide powder additive according to claim 1, characterized in that: In S2, the median particle size of the pulverized material is 10 μm to 15 μm.

6. A method for preparing high-temperature magnesium oxide powder, using a high-temperature magnesium oxide powder additive according to claim 1, characterized in that: The preparation method comprises the following steps: According to the mass ratio, dead-burned magnesium oxide: additive: thermosetting resin = (100-120): (5-8): (3-5), the dead-burned magnesium oxide, additive and thermosetting resin are mixed, dry ball milled for 40-50 minutes, modified at 260-280°C for 2-3 hours to obtain dead-burned magnesium oxide coated with additives and thermosetting resin, cooled, broken up, sieved, and the sieved material is taken to obtain high-temperature magnesium oxide powder.

7. The method for preparing high temperature magnesium oxide powder according to claim 6, characterized in that: The dead-burned magnesia is obtained by calcining magnesite at 1700°C to 1900°C for 8h to 10h. The particle size of the dead-burned magnesia is 60 mesh> particle size ≥ 80 mesh, accounting for 10 to 20 parts by mass, 80 mesh> particle size ≥ 100 mesh, accounting for 30 to 40 parts by mass, 100 mesh> particle size ≥ 250 mesh, accounting for 25 to 35 parts by mass, 250 mesh> particle size ≥ 325 mesh, accounting for 5 to 10 parts by mass, and 325 mesh> particle size, accounting for 1 to 5 parts by mass. The thermosetting resin is phenolic resin or epoxy resin, and the median particle size of the thermosetting resin is less than 2μm.

8. The method for preparing high temperature magnesium oxide powder according to claim 6, characterized in that: The modified stirring speed is 80 rpm to 120 rpm; the sieving mesh number is 60 meshes.

9. An application of high temperature magnesium oxide powder, the high temperature magnesium oxide powder prepared by the preparation method of high temperature magnesium oxide powder according to claim 6, characterized in that: High temperature magnesium oxide powder is used to prepare heating tubes.