Regeneration method of lithium cobalt oxide positive electrode material, lithium cobalt oxide positive electrode material and application
By extracting lithium sulfate and cobalt sulfate through low-temperature roasting and water leaching, combined with carbonate precipitation and calcination steps, the efficient recovery and regeneration of lithium cobalt oxide cathode materials was successfully achieved, solving the environmental problem of lithium cobalt oxide materials in used lithium-ion batteries. pollution and resource waste issues, and improve material performance and stability.
Patent Information
- Application Number
- CN202410715687.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The recycling technology of lithium cobalt oxide cathode materials in used lithium-ion batteries has problems of environmental pollution and resource waste, and it is difficult to effectively recover and regenerate efficient lithium cobalt oxide materials with existing technology.
The mixture of lithium cobalt oxide black powder and sulfate is processed using low-temperature roasting and water leaching methods. Lithium sulfate and cobalt sulfate are generated through low-temperature roasting, followed by water leaching to remove floating matter, and carbonate precipitation is added to extract cobalt and lithium. Finally, The regenerated lithium cobalt oxide cathode material is obtained by calcination, and the material stability is improved by doping with aluminum oxide.
It achieves efficient recovery and regeneration of lithium cobalt oxide cathode materials, shortens the material regeneration process, improves material performance, avoids environmental pollution, and uses aluminum scrap residue to enhance material stability.
Smart Images

Figure CN118724077A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery recycling, and in particular to a regeneration method for a lithium cobalt oxide positive electrode material, a lithium cobalt oxide positive electrode material and applications thereof. Background Art
[0002] In recent years, with the increasing demand for energy, lithium-ion batteries (LIBs) with high energy density and long service life have been widely used. Among the many positive electrode materials for lithium-ion batteries, LiCoO 2 Due to its advantages such as simple synthesis process, high initial coulombic efficiency, good cycle stability, stable charge and discharge voltage, high voltage platform and volume energy density, it is widely used in the field of digital electronic products. 2 The widespread use of LiCoO also means that there is more waste 2 Battery production. Waste LiCoO 2 Toxic metal elements and organic matter in batteries can pollute soil, air, and even groundwater, causing serious environmental problems and harming human health. At the same time, waste cobalt oxide lithium-ion batteries contain rich valuable metal elements. 2 Battery material recycling is of special significance to alleviate the serious shortage of cobalt resources in my country. Therefore, developing a reasonable and efficient recycling method for lithium cobalt oxide positive electrode materials in waste batteries has great potential economic value.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] The purpose of the present invention is to provide a regeneration method for lithium cobalt oxide positive electrode materials, lithium cobalt oxide positive electrode materials and applications, and to recycle elements in waste lithium cobalt oxide batteries to prepare lithium cobalt oxide positive electrode materials with good stability and suitable for higher voltages.
[0005] The present invention is achieved in that:
[0006] In a first aspect, the present invention provides a method for regenerating a lithium cobalt oxide positive electrode material, comprising:
[0007] Low-temperature roasting, in the presence of oxygen, roasting a mixture of lithium cobalt oxide black powder and sulfate to obtain a roasted material containing lithium sulfate and cobalt sulfate; the sulfate is selected from at least one of ammonium sulfate and ammonium hydrogen sulfate;
[0008] Water leaching, mixing the roasted material with water to obtain a water leaching slurry, stirring and standing the water leaching slurry in turn to obtain a water leaching liquid, and removing floating objects on the upper layer of the water leaching liquid to obtain a leachate;
[0009] Extracting lithium and cobalt, adding carbonate to the leaching solution to precipitate cobalt and lithium, and then performing solid-liquid separation to obtain a precipitate;
[0010] Calcination: calcining the precipitate to obtain a regenerated lithium cobalt oxide positive electrode material.
[0011] In some embodiments, the low temperature calcination temperature is 300°C-550°C, and the time is 0.5h-12h;
[0012] And / or, the molar ratio of lithium cobaltate to sulfate in the mixture is 1:(0.5-3);
[0013] And / or, the mixture is ground and mixed before being subjected to low temperature roasting.
[0014] In some embodiments, the stirring step is performed for 30 min to 1 h, and the stirring speed is 150 rpm to 300 rpm;
[0015] And / or, the standing time is 1h-24h;
[0016] And / or, the mass ratio of the calcined material to water in the water-impregnated slurry is 1:(1-3).
[0017] In some embodiments, in the lithium-cobalt extraction step, the molar amount of carbonate in the carbonate n (Na 2 CO 3 )=(1-1.25)n(Li + )+(2-2.5)n(Co 2+ );
[0018] And / or, the carbonate is selected from at least one of sodium carbonate and potassium carbonate.
[0019] In some embodiments, the calcination step is performed at a temperature of 700° C. to 1000° C. for a time of 0.5 h to 12 h.
[0020] In some embodiments, the method for preparing the lithium cobalt oxide black powder comprises: placing the lithium cobalt oxide positive electrode sheet in a crushing device for crushing and peeling, and then sieving through a 150-250 mesh standard sieve, and the sieved material is the lithium cobalt oxide black powder.
[0021] In a second aspect, the present invention provides a lithium cobalt oxide positive electrode material obtained by the regeneration method described in any one of the aforementioned embodiments.
[0022] In some embodiments, the positive electrode material comprises lithium cobalt oxide and aluminum oxide doped in the lithium cobalt oxide, and the aluminum content in the lithium cobalt oxide positive electrode material is 0.1 wt %-0.5 wt %.
[0023] In a third aspect, the present invention provides a positive electrode plate, comprising a lithium cobalt oxide positive electrode material prepared by the method described in any one of the aforementioned embodiments or a lithium cobalt oxide positive electrode material described in the aforementioned embodiments.
[0024] In a fourth aspect, the present invention provides a lithium-ion battery, comprising the positive electrode sheet described in the aforementioned embodiment.
[0025] The present invention has the following beneficial effects:
[0026] Since waste lithium cobalt oxide positive electrode materials contain a large amount of heavy metals, irregular discharge will cause ecological pollution and environmental damage to the environment. The present invention has obvious advantages in terms of economy and sustainable development in recycling and regenerating lithium cobalt oxide positive electrode materials.
[0027] The present invention realizes efficient and selective extraction of lithium cobalt through low-temperature roasting and water leaching, greatly shortens the material regeneration process, removes carbon and SP after cracking, and improves the performance of lithium cobalt oxide.
[0028] The present invention takes advantage of the disadvantage of residual aluminum chips generated during the stripping of the pole piece, and a small amount of Al(OH) 3 Converted to Al 2 O 3 , for the generated LiCoO 2 The formation of coated doping makes the regenerated lithium cobalt oxide positive electrode material more stable and realizes the rational utilization of aluminum chip waste. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0030] Figure 1 This is a flow chart of Embodiment 1 of the present invention;
[0031] Figure 2 This is a SEM image of the lithium cobalt oxide black powder in Example 1 of the present invention;
[0032] Figure 3 This is a SEM image of the regenerated lithium cobalt oxide in Example 1 of the present invention;
[0033] Figure 4 This is the EDS image of the regenerated lithium cobalt oxide in Example 1 of the present invention. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0035] The present invention provides a method for regenerating a lithium cobalt oxide positive electrode material, comprising:
[0036] Low-temperature roasting, in the presence of oxygen, roasting a mixture of lithium cobalt oxide black powder and sulfate to obtain a roasted material containing lithium sulfate and cobalt sulfate; the sulfate is selected from at least one of ammonium sulfate and ammonium hydrogen sulfate;
[0037] Water leaching, mixing the roasted material with water to obtain a water leaching slurry, stirring and standing the water leaching slurry in turn to obtain a water leaching liquid, and removing floating objects on the upper layer of the water leaching liquid to obtain a leachate;
[0038] Extracting lithium and cobalt, adding carbonate to the leaching solution to precipitate cobalt and lithium, and then performing solid-liquid separation to obtain a precipitate;
[0039] Calcination: calcining the precipitate to obtain a regenerated lithium cobalt oxide positive electrode material.
[0040] In a method for regenerating a lithium cobalt oxide positive electrode material provided by an embodiment of the present invention, a mixture of lithium cobalt oxide black powder and sulfate is subjected to low-temperature roasting to decompose the sulfate, and the generated sulfate radical reacts with cobalt and lithium to generate cobalt sulfate and lithium sulfate, so that the cobalt and lithium can be transferred to the leaching solution in a subsequent water leaching step. The low-temperature roasting is performed under an aerobic condition such as an air atmosphere, and lithium is more easily sulfated to form sulfate. At the same time, since there is some residual aluminum in the lithium cobalt oxide black powder, a trace amount of aluminum reacts with sulfate radicals to generate aluminum sulfate, which can be transferred to the leaching solution with the cobalt and lithium in the subsequent water leaching step. In addition, there is still a binder remaining in the lithium cobalt oxide black powder, and the binder will crack during the low-temperature roasting process. The cracking products of the binder will affect the performance of the regenerated lithium cobalt oxide positive electrode material. Therefore, in the subsequent water immersion step, the water immersion slurry is first stirred to accelerate the leaching of lithium salt, cobalt salt and aluminum salt. After stirring, it is allowed to stand so that the cracking products of the binder and the conductive agent in the black powder will gradually float up, and then the floating objects are skimmed off to remove most of the cracking products and conductive agents to improve the performance of the regenerated lithium cobalt oxide positive electrode material.
[0041] It should be noted that, in the embodiment of the present invention, the sulfate is selected from at least one of ammonium sulfate and ammonium bisulfate, the leaching solution obtained after water immersion is acidic, with a pH between 3-5, and carbonate is added to the leaching solution to precipitate lithium cobalt. On the one hand, the ammonia generated by the decomposition of ammonium sulfate and ammonium bisulfate can escape, and less residue remains in the regenerated lithium cobalt oxide positive electrode material. On the other hand, the decomposition of ammonium sulfate and ammonium bisulfate will produce ammonia and sulfuric acid, and sulfuric acid can react with lithium cobalt oxide and aluminum to dissolve cobalt, lithium and aluminum. At the same time, the decomposition of sulfate and the reaction of sulfuric acid with lithium cobalt oxide and aluminum will produce gas, which promotes the forward movement of the reaction equilibrium, promotes the reaction, and is conducive to the dissolution of cobalt, lithium and aluminum.
[0042] In an embodiment of the present invention, carbonate is added to the leachate to precipitate lithium and cobalt. At the same time, trace amounts of aluminum present in the leachate can also be converted into aluminum hydroxide and precipitated to obtain a precipitate containing lithium carbonate, cobalt carbonate, and aluminum hydroxide. In some embodiments, the precipitate is ground and mixed before calcination to promote uniform distribution of the components in the precipitate; in some embodiments, the precipitate is dried before calcination.
[0043] In the embodiment of the present invention, since there is a small amount of aluminum hydroxide in the precipitate, aluminum hydroxide is calcined to generate aluminum oxide, which can be used to dope and coat lithium cobalt oxide to improve the stability of the regenerated lithium cobalt oxide positive electrode material.
[0044] In some embodiments, the temperature of the low-temperature roasting is 300°C-550°C, and the time is 0.5h-12h. Specifically, the temperature of the low-temperature roasting can be 300°C, 350°C, 400°C, 450°C, 500°C, 550°C or any value between 300°C-550°C, and the time of the low-temperature roasting can be 0.5h, 1h, 2h, 4h, 0.5h, 6h, 8h, 10h, 12h or any value between 0.5h-12h. When the low-temperature roasting temperature is lower than 300°C, ammonium sulfate and ammonium bisulfate are difficult to decompose; ammonium sulfate roasting of lithium cobalt oxide at an appropriate temperature can ensure the formation of lithium sulfate that is easily soluble and leached and cobalt sulfate that is easily separated; if the temperature is too high, ammonium sulfate or ammonium bisulfate will decompose too quickly at high temperature, and will escape and run away before reacting with lithium cobalt oxide in time, which is not conducive to the separation of lithium and cobalt, and will reduce the yield of valuable elements in the subsequent processing process.
[0045] In some embodiments, the molar ratio of lithium cobalt oxide to sulfate in the mixture is 1:(0.5-3), specifically, it can be 1:0.5, 1:1, 1:2, 1:3 or any value between 1:(0.5-3). The main component in the black powder that reacts with sulfate is lithium cobalt oxide, and there is a trace amount of aluminum. In order to make the lithium cobalt oxide and sulfate react more fully, some embodiments can add sulfate according to the stoichiometric ratio of lithium cobalt oxide and sulfate, and the sulfate can also be added in a slightly excess amount compared to the stoichiometric ratio.
[0046] In some embodiments, the mixture is ground and mixed before low-temperature calcination to improve the uniformity of the mixture, which is beneficial for a more complete reaction between the lithium cobalt oxide black powder and the ammonium sulfate salt.
[0047] In some embodiments, the stirring step is performed for 30 min to 1 h, and the stirring speed is 150 rpm to 300 rpm. Specifically, the stirring step can be performed for 30 min, 40 min, 50 min, 1 h, or any value between 30 min and 1 h; the stirring step can be performed for 150 rpm, 200 rpm, 250 rpm, 300 rpm, or any value between 150 rpm and 300 rpm. If the stirring time is too short, the amorphous carbon and SP produced after the cracking of the binder cannot be effectively dispersed and separated, affecting the purity of the precipitate; if the stirring speed is too low, similarly, the amorphous carbon produced by the cracking of the binder cannot be effectively mechanically broken up by the stirring paddle, which is not conducive to the separation of amorphous carbon and SP from the precipitation product, affecting the purity of the precipitate.
[0048] In some embodiments, the standing time is 1h-24h, specifically 1h, 2h, 5h, 10h, 15h, 20h, 24h or any value between 1h-24h. The standing time is sufficient to allow the small molecule organic matter and the conductive agent generated by the decomposition of the binder to fully float up and be easily removed. If the standing time is not sufficient or is too short, the small molecule organic matter and the conductive agent generated by the decomposition of the binder will exist in the leachate, thereby affecting the stability of the regenerated lithium cobalt oxide positive electrode material.
[0049] In some embodiments, the mass ratio of the calcined material to water in the water-immersion slurry is 1:(1-3), specifically, it can be 1:1, 1:2, 1:3 or any value between 1:(1-3). Within the scope of the embodiment of the present invention, increasing the water content in the water-immersion slurry is beneficial to improving the leaching rate, but if the water content is too high, the wastewater treatment volume is large, and due to the large amount of water, only the lower solubility will also cause a large element loss.
[0050] In some embodiments, in the lithium-cobalt extraction step, the molar amount of carbonate in the carbonate n (Na 2 CO 3 )=(1-1.25)n(Li + )+(2-2.5)n(Co 2+ ); Excessive addition of carbonate can promote Li + and Co 2+ and Al 3+ The precipitation is more complete.
[0051] In some embodiments, the carbonate is selected from at least one of sodium carbonate and potassium carbonate. Sodium carbonate and potassium carbonate react with sulfate in the leachate to generate sodium sulfate or potassium sulfate, which has high solubility in water and is beneficial to reducing the amount of impurities in the regenerated lithium cobalt oxide positive electrode material.
[0052] In some embodiments, the temperature of the calcination step is 700°C-1000°C, and the time is 0.5h-12h. Specifically, the temperature of the calcination step can be 700°C, 700°C, 700°C, 1000°C, or any value between 700°C-1000°C; the time of the calcination step can be 0.5h, 1h, 3h, 6h, 9h, 12h, or any value between 0.5h-12h. Under this condition, aluminum can be well coated and doped into the lithium cobalt oxide particles.
[0053] In some embodiments, the preparation method of the lithium cobalt oxide black powder includes: placing the lithium cobalt oxide positive electrode sheet in a crushing device for crushing and peeling, and then sieving it through a 150-250 mesh standard sieve, the material under the sieve is the lithium cobalt oxide black powder, and the material on the sieve is aluminum foil, etc., and the lithium cobalt oxide black powder is separated by sieving.
[0054] An embodiment of the present invention further provides a lithium cobalt oxide positive electrode material obtained by the regeneration method described in any one of the aforementioned embodiments.
[0055] In some embodiments, the lithium cobaltate and aluminum oxide doped in the lithium cobaltate are included, and the aluminum content in the lithium cobaltate positive electrode material is 0.1wt%-0.5wt%, specifically 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt% or any value between 0.1wt%-0.5wt%. The aluminum in the lithium cobaltate positive electrode material exists in the form of aluminum oxide. If the aluminum content is too high, it will affect the electrical properties such as the capacity of the regenerated lithium cobaltate positive electrode material.
[0056] An embodiment of the present invention further provides a positive electrode plate, comprising a lithium cobalt oxide positive electrode material prepared by the method described in any one of the aforementioned embodiments or a lithium cobalt oxide positive electrode material described in the aforementioned embodiments.
[0057] In the positive electrode sheet of the present invention, the positive electrode film layer generally comprises the positive electrode material and optionally a binder and optionally a conductive agent, and is generally formed by coating the positive electrode slurry, drying, and cold pressing. The positive electrode slurry is generally formed by dispersing the positive electrode material and optionally a conductive agent and optionally a binder in a solvent and stirring them uniformly. The solvent may be N-methylpyrrolidone (NMP).
[0058] In some optional embodiments, based on the total weight of the positive electrode film layer, the positive electrode film layer may contain 70wt%-97wt% of positive electrode material. Optionally, the weight proportion of the positive electrode material in the positive electrode film layer is 85%-97%, 90%-97%, or 95%-97%. By adjusting the proportion of the positive electrode material in the positive electrode film layer, the energy density and cycle life of the lithium-ion battery can be further improved.
[0059] In some embodiments, the binder of the positive electrode film layer may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and modified polymers thereof.
[0060] The conductive agent can improve the electronic conductivity of the positive electrode film layer. In some optional embodiments, based on the total weight of the positive electrode film layer, the positive electrode film layer may contain 2wt%-20wt% of the conductive agent. Optionally, the weight proportion of the conductive agent in the positive electrode film layer is 2%-10%, or 2%-5%.
[0061] In some embodiments, the conductive agent of the positive electrode film layer may include one or more of superconducting carbon, carbon black (such as SuperP, acetylene black, Ketjen black), carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0062] It should be noted that the composition or parameters of each positive electrode film layer given in the present invention refer to the composition or parameter range of the single-sided film layer of the positive electrode current collector. When the positive electrode film layer is arranged on two opposite surfaces of the positive electrode current collector, the composition or parameters of the positive electrode film layer on any one of the surfaces meet the requirements of the present invention, which is considered to fall within the protection scope of the present invention.
[0063] The present invention provides a lithium-ion battery, comprising the positive electrode sheet described in the above embodiment, and also comprising a negative electrode sheet, an electrolyte and a separator.
[0064] [Negative electrode]
[0065] The negative electrode plate of the present invention comprises a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector.
[0066] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is laminated on any one or both of the two opposite surfaces of the negative electrode current collector.
[0067] The negative electrode current collector may be made of a material with good electrical conductivity and mechanical strength to perform the functions of conducting and collecting current. In some embodiments, the negative electrode current collector may be made of copper foil.
[0068] In the negative electrode sheet of the present invention, the negative electrode film layer generally comprises a negative electrode active material and optionally a binder, optionally a conductive agent and other optional auxiliary agents. It is generally formed by coating a negative electrode slurry on a negative electrode current collector, drying, and cold pressing. The negative electrode slurry coating is generally formed by dispersing the negative electrode active material and optionally a conductive agent, optionally a binder, and optionally an auxiliary agent in a solvent and stirring evenly. The solvent may be N-methylpyrrolidone (NMP) or deionized water.
[0069] In some embodiments, the negative electrode active material may include one or more of artificial graphite, natural graphite, silicon-based materials, and tin-based materials. Alternatively, the negative electrode active material includes one or more of artificial graphite and natural graphite. Alternatively, the negative electrode active material includes artificial graphite.
[0070] In some embodiments, the conductive agent may include one or more of superconducting carbon, carbon black (eg, SuperP, acetylene black, Ketjen black, etc.), carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0071] In some embodiments, the binder may include one or more of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS).
[0072] In some embodiments, other optional auxiliary agents include, for example, a thickener (eg, sodium carboxymethyl cellulose CMC-Na), a PTC thermistor material, and the like.
[0073] [Electrolytes]
[0074] The electrolyte plays a role in conducting ions between the positive electrode and the negative electrode. The present invention has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be selected from an electrolyte. The electrolyte includes an electrolyte salt and a solvent.
[0075] In some embodiments, the electrolyte salt may be selected from lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium perchlorate (LiClO 4 ) lithium hexafluoroarsenate (LiAsF 6 ), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate 2 (LiPO 2 F), one or more of lithium difluorooxalate phosphate (LiDFOP) and lithium tetrafluorooxalate phosphate (LiTFOP).
[0076] In some embodiments, the solvent can be selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).
[0077] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high temperature performance, and additives that improve battery low temperature performance.
[0078] [Isolation film]
[0079] The separator is disposed between the positive electrode sheet and the negative electrode sheet to play a role of isolation. The lithium ion battery of the present invention has no particular restrictions on the type of separator, and any known porous structure separator for lithium ion batteries can be selected. For example, the separator can be selected from one or more of a glass fiber film, a non-woven film, a polyethylene film, a polypropylene film, a polyvinylidene fluoride film, and a multilayer composite film containing one or more of them.
[0080] The positive electrode sheet, the negative electrode sheet and the isolation film can be made into an electrode assembly through a lamination process or a winding process, so that the isolation film is placed between the positive electrode sheet and the negative electrode sheet to play an isolation role; the electrode assembly is placed in an outer package, the electrolyte is injected and sealed, and a lithium-ion battery can be obtained.
[0081] The outer packaging of the lithium-ion battery is used to encapsulate the electrode assembly and the electrolyte. In some embodiments, the outer packaging of the lithium-ion battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the lithium-ion battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.
[0082] The present invention has no particular limitation on the shape of the lithium-ion battery, which may be cylindrical, square or any other shape.
[0083] In some embodiments, lithium-ion batteries may be assembled into a battery module. The battery module may contain multiple lithium-ion batteries, and the specific number may be adjusted according to the application and capacity of the battery module.
[0084] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0085] The present invention provides an electrical device, comprising the lithium-ion battery described in the above embodiment.
[0086] The present invention also provides an electrical device, which includes at least one of the lithium-ion battery, battery module, or battery pack described in the present invention. The lithium-ion battery, battery module, or battery pack can be used as a power source for the device, or as an energy storage unit for the device. The device can be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc. The device can select a lithium-ion battery, a battery module, or a battery pack according to its use requirements.
[0087] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0088] Example 1
[0089] This embodiment provides a method for regenerating a lithium cobalt oxide positive electrode material. Figure 1 As shown, the specific steps include:
[0090] 1. Place the waste lithium cobalt oxide positive electrode sheet in a crushing device for crushing and peeling, and then screen it through a 200-mesh standard sieve. The black powder under the sieve is lithium cobalt oxide black powder. SEM shows Figure 2 As shown;
[0091] 2. Add ammonium sulfate (molar ratio LiCoO 2 :(NH 4 ) 2 SO 4 =2:1) after being fully ground, low-temperature calcination is carried out at 350°C for 2h in an air atmosphere to obtain a calcined material.
[0092] 3. Add 2 times the mass of water to the calcined material and stir for 45 minutes at a stirring speed of 200 rpm. Let it stand and soak for 2 hours. Skim off the carbon and SP produced by cracking on the upper layer of the solution to obtain an acidic leachate. Add sodium carbonate (Na2CO3) to the leachate. 2 CO 3)=n(Li + )+2n(Co 2+ ))A precipitate is formed.
[0093] 4. The precipitate was centrifugally dried and fully mixed in a high-speed mixer to obtain a lithium cobalt oxide precursor. After calcination at 800°C for 2h, a stable regenerated lithium cobalt oxide was obtained. Figure 3 As shown, the EDS test image is as follows Figure 4 As shown in Table 1, the content of each element in the regenerated lithium cobalt oxide is measured. Figure 3 and Figure 4 The regenerated lithium cobalt oxide has a regular shape, a relatively uniform particle size, a smooth surface and a uniform surface showing Al 2 O 3 The product forms an effective coating on lithium cobalt oxide.
[0094] Table 1. EDS test of the content of each element in the regenerated lithium cobalt oxide
[0095]
[0096] Embodiment 2:
[0097] This embodiment provides a method for regenerating a lithium cobalt oxide positive electrode material, which is different from Embodiment 1 mainly in that the amount of ammonium sulfate added and the calcination conditions are different, and specifically includes the following steps:
[0098] 1. Place the waste lithium cobalt oxide positive electrode sheet in a crushing device for crushing and peeling, and then screen it through a 200-mesh standard sieve. The black powder under the sieve is lithium cobalt oxide black powder;
[0099] 2. Add ammonium sulfate (molar ratio LiCoO 2 :(NH 4 ) 2 SO 4 =1:1) after being fully ground, low-temperature calcination is carried out at 350°C for 2h in an air atmosphere to obtain a calcined material.
[0100] 3. Add 2 times the mass of water to the calcined material and stir for 45 minutes at a stirring speed of 200 rpm. Let it stand and soak for 2 hours. Skim off the carbon and SP produced by cracking on the upper layer of the solution to obtain an acidic leachate. Add sodium carbonate (Na2CO3) to the leachate. 2 CO 3 )=n(Li + )+2n(Co 2+ ))A precipitate is formed.
[0101] 4. Each precipitate is centrifugally dried, and fully mixed in a high-speed mixer to obtain a lithium cobalt oxide precursor, which is then calcined at 900° C. for 2 h to obtain a stable regenerated lithium cobalt oxide.
[0102] Embodiment 3:
[0103] This embodiment provides a method for regenerating a lithium cobalt oxide positive electrode material, which is different from Embodiment 2 mainly in that the standing and soaking time is different, and specifically includes the following steps:
[0104] 1. Place the waste lithium cobalt oxide positive electrode sheet in a crushing device for crushing and peeling, and then screen it through a 200-mesh standard sieve. The black powder under the sieve is lithium cobalt oxide black powder;
[0105] 2. Add ammonium sulfate (molar ratio LiCoO 2 :(NH 4 ) 2 SO 4 =1:1) was fully ground and then calcined at low temperature. In air atmosphere, it was treated at 350°C for 2h to obtain calcined material 3. 2 times the mass of water was added to the calcined material and stirred for 45min at a stirring speed of 200rpm. The material was allowed to stand and soak for 4h. The carbon and SP produced by cracking on the upper layer of the solution were skimmed off to obtain a leachate. The leachate was acidic. Sodium carbonate (Na2CO3) was added to the leachate. 2 CO 3 )=n(Li + )+2n(Co 2+ ))A precipitate is formed.
[0106] 4. Each precipitate is centrifugally dried, and fully mixed in a high-speed mixer to obtain a lithium cobalt oxide precursor, which is then calcined at 900° C. for 2 h to obtain a stable regenerated lithium cobalt oxide.
[0107] Embodiment 4:
[0108] This embodiment provides a method for regenerating a lithium cobalt oxide positive electrode material, which specifically includes the following steps:
[0109] 1. Place the waste lithium cobalt oxide positive electrode sheet in a crushing device for crushing and peeling, and then screen it through a 200-mesh standard sieve. The black powder under the sieve is lithium cobalt oxide black powder;
[0110] 2. Add ammonium sulfate (molar ratio LiCoO 2 :(NH 4 ) 2 SO 4 =2:1) after being fully ground, low-temperature calcination is carried out at 300°C for 8h in an air atmosphere to obtain a calcined material.
[0111] 3. Add an equal amount of water to the calcined material and stir for 30 minutes at a stirring speed of 300 rpm. Let it stand for 1 hour and skim off the carbon and SP produced by cracking on the upper layer of the solution to obtain an acidic leachate. Add sodium carbonate (Na2CO3) to the leachate. 2 CO 3 )=1.25n(Li + )+2.5n(Co 2+ ))A precipitate is formed.
[0112] 4. The precipitate is centrifugally dried and fully mixed in a high-speed mixer to obtain a lithium cobalt oxide precursor, which is then calcined at 700° C. for 8 h to obtain stable regenerated lithium cobalt oxide.
[0113] Embodiment 5:
[0114] This embodiment provides a method for regenerating a lithium cobalt oxide positive electrode material, which specifically includes the following steps:
[0115] 1. Place the waste lithium cobalt oxide positive electrode sheet in a crushing device for crushing and peeling, and then screen it through a 200-mesh standard sieve. The black powder under the sieve is lithium cobalt oxide black powder;
[0116] 2. Add ammonium sulfate (molar ratio LiCoO 2 :(NH 4 ) 2 SO 4 =1:3) after being fully ground, low-temperature calcination is carried out, and treatment is carried out at 550°C for 1h in an air atmosphere to obtain a calcined material.
[0117] 3. Add 3 times the mass of water to the calcined material and stir for 60 minutes at a stirring speed of 150 rpm. Let it stand and soak for 10 hours. Skim off the carbon and SP produced by cracking on the upper layer of the solution to obtain an acidic leachate. Add sodium carbonate (Na2CO3) to the leachate. 2 CO 3 )=n(Li + )+2n(Co 2+ ))A precipitate is formed.
[0118] 4. The precipitate is centrifugally dried and fully mixed in a high-speed mixer to obtain a lithium cobalt oxide precursor, which is then calcined at 1000° C. for 1 h to obtain stable regenerated lithium cobalt oxide.
[0119] Comparative Example 1:
[0120] This comparative example provides a method for regenerating a lithium cobalt oxide positive electrode material, which specifically comprises the following steps:
[0121] 1. Cut the waste lithium cobalt oxide positive electrode into 2cm-7cm pieces with scissors, place them in a beaker, add NMP at a solid-liquid ratio of 1:3, stir the mixture with a blender for 40 minutes to fully shear the material, and then sieve it through a 200-mesh standard sieve. The black powder under the sieve is the required electrode powder;
[0122] 2. Place the sieved electrode powder in an oven and bake at 80°C for 24 hours in an air atmosphere until the material is completely dry;
[0123] 3. The dried material is put into a ball mill for ball milling. The crushed material is calcined at 800° C. for 2 h in an air atmosphere to obtain the recovered lithium cobalt oxide;
[0124] Comparative Example 2:
[0125] This comparative example provides a regeneration method for a lithium cobalt oxide positive electrode material, which is different from Example 1 mainly in that the atmosphere for low-temperature calcination is air, and the calcination is performed at 200° C. for 3 h.
[0126] Comparative Example 3:
[0127] This comparative example provides a regeneration method for a lithium cobalt oxide positive electrode material, which is different from Example 1 mainly in that the temperature of low-temperature calcination is 700°C.
[0128] Comparative Example 4:
[0129] This comparative example provides a method for regenerating a lithium cobalt oxide positive electrode material, which is different from Example 1 mainly in that in step 3, solid-liquid separation is directly performed after static immersion, and the carbon and SP produced by cracking the upper layer of the solution are not skimmed off.
[0130] Comparative Example 5:
[0131] This comparative example provides a regeneration method for a lithium cobalt oxide positive electrode material, which differs from Example 2 mainly in that the calcination temperature is reduced to 600°C.
[0132] Comparative Example 6:
[0133] This comparative example provides a method for regenerating a lithium cobalt oxide positive electrode material, which is different from Example 2 mainly in that in step 2, LiCoO 2 :(NH 4 ) 2 SO 4 =1:0.4.
[0134] Comparative Example 7:
[0135] This comparative example provides a method for regenerating a lithium cobalt oxide positive electrode material, which is different from Example 2 mainly in that in step 2 (NH 4 ) 2 SO 4Replace with SO 4 2- An equal molar amount of sodium sulfate.
[0136] Comparative Example 8:
[0137] This comparative example provides a method for regenerating a lithium cobalt oxide positive electrode material, which is different from Example 2 mainly in that stirring is performed for 10 minutes in step 3.
[0138] Comparative Example 9:
[0139] This comparative example provides a method for regenerating a lithium cobalt oxide positive electrode material, which is different from Example 2 mainly in that the stirring speed in step 3 is 100 ppm.
[0140] Comparative Example 10:
[0141] This comparative example provides a method for regenerating a lithium cobalt oxide positive electrode material, which is different from Example 2 mainly in that in step 3, the material is allowed to stand and soak for 0.5 h.
[0142] Electrochemical performance:
[0143] The lithium cobalt oxide positive electrode materials obtained in the embodiment and the comparative example are respectively prepared into lithium batteries. The preparation method of the lithium battery is as follows: the lithium cobalt oxide positive electrode material, polyvinylidene fluoride, and SP are evenly mixed, wherein the mass ratio of the lithium cobalt oxide positive electrode material, polyvinylidene fluoride, and SP is lithium cobalt oxide positive electrode material: polyvinylidene fluoride: SP = 90:5:5, and NMP (N-methylpyrrolidone) is added to the obtained mixture, stirred to form a slurry, coated on an aluminum foil, and dried at 80°C to form a positive electrode sheet. The prepared positive electrode sheet, graphite, electrolyte and diaphragm are used as raw materials and wound to form a soft-pack battery.
[0144] The performance of the obtained soft pack battery was tested by the following method:
[0145] (1) Cycle test: At 25°C, the soft pack battery was charged with a constant current (CC) at a rate of 1C until the voltage was 4.2V, and the current was cut off at a rate of 0.05C while the voltage was maintained at 4.2V in a constant voltage mode (CV). The battery was discharged with a constant current (CC) at a rate of 0.5C until the discharge voltage was 3.0V, and the capacity retention rate was calculated for 1000 cycles.
[0146] (2) Capacity test: The rate capacity was tested at 25°C and 4.2V / 0.1C charge and discharge conditions.
[0147] The test results are shown in Table 2. It can be seen from Table 2 that the initial capacity, first efficiency and capacity retention rate of the embodiment are better than those of the comparative example.
[0148] Table 2. Comparison of electrochemical performance of regenerated lithium cobalt oxide batteries prepared in various examples and comparative examples
[0149]
[0150] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for regenerating a lithium cobalt oxide positive electrode material, characterized in that: include: Low-temperature roasting: roasting the mixture of lithium cobalt oxide black powder and sulfate under oxygen conditions to obtain a roasted material containing lithium sulfate and cobalt sulfate; The sulfate is selected from at least one of ammonium sulfate and ammonium bisulfate; Water leaching, mixing the roasted material with water to obtain a water leaching slurry, stirring and standing the water leaching slurry in turn to obtain a water leaching liquid, and removing floating objects on the upper layer of the water leaching liquid to obtain a leachate; Extracting lithium and cobalt, adding carbonate to the leaching solution to precipitate cobalt and lithium, and then performing solid-liquid separation to obtain a precipitate; Calcination: calcining the precipitate to obtain a regenerated lithium cobalt oxide positive electrode material.
2. The method for regenerating a lithium cobalt oxide positive electrode material according to claim 1, characterized in that: The temperature of the low-temperature calcination is 300°C-550°C, and the time is 0.5h-12h; And / or, the molar ratio of lithium cobaltate to sulfate in the mixture is 1:(0.5-3); And / or, the mixture is ground and mixed before being subjected to low temperature roasting.
3. The regeneration method of lithium cobalt oxide positive electrode material according to claim 1, characterized in that: The stirring time is 30 min-1 h, and the stirring speed is 150 rpm-300 rpm; And / or, the standing time is 1h-24h; And / or, the mass ratio of the calcined material to water in the water-impregnated slurry is 1:(1-3).
4. The method for regenerating a lithium cobalt oxide positive electrode material according to claim 1, characterized in that: In the lithium cobalt extraction step, the molar amount of carbonate in the carbonate n(Na2CO3)=(1-1.25)n(Li + )+(2-2.5)n(Co 2+ ); And / or, the carbonate is selected from at least one of sodium carbonate and potassium carbonate.
5. The method for regenerating a lithium cobalt oxide positive electrode material according to claim 1, characterized in that: The temperature of the calcination step is 700° C.-1000° C., and the time is 0.5 h-12 h.
6. The method for regenerating a lithium cobalt oxide positive electrode material according to claim 1, characterized in that: The preparation method of the lithium cobalt oxide black powder comprises: placing the lithium cobalt oxide positive electrode sheet in a crushing device for crushing and peeling, and then sieving through a 150-250 mesh standard sieve, and the sieved material is the lithium cobalt oxide black powder.
7. A lithium cobalt oxide positive electrode material, characterized in that: Obtained by the regeneration method according to any one of claims 1 to 6.
8. The lithium cobalt oxide positive electrode material according to claim 7, characterized in that: The invention comprises lithium cobalt oxide and aluminum oxide doped in the lithium cobalt oxide, wherein the aluminum content in the lithium cobalt oxide positive electrode material is 0.1wt%-0.5wt%.
9. A positive electrode sheet, characterized in that: The invention comprises a lithium cobalt oxide positive electrode material prepared by the method according to any one of claims 1 to 6 or a lithium cobalt oxide positive electrode material according to claim 7 or 8.
10. A lithium ion battery, characterized in that: Including the positive electrode sheet as described in claim 9.
Citation Information
Patent Citations
Regeneration method of lithium ion battery anode material lithium cobalt oxide waste
CN104466293A
Method for purifying acid production tail gas by using waste lithium cobalt oxide and recycling cobalt and lithium
CN105742747A
Method for recovering cobalt and lithium from lithium cobalt oxide waste of lithium ion battery positive material
CN105742748A
Process for recovering nickel cobalt lithium manganate positive electrode material by taking waste lithium ion battery as raw material
CN108649291A
Method for recovering cobalt and lithium metals from waste lithium cobalt oxide battery
CN112095000A