Preparation method of flower-like nickel protoxide, method for preparing anode lithium supplement agent Li2NiO2 by adopting flower-like nickel protoxide and application of anode lithium supplement agent Li2NiO2
Preparing flower-like nickel oxide by precipitation method and calcining it with lithium source at high temperature solves the problems of slow reaction rate and complicated process in the preparation of Li2NiO2, achieves high-purity and high-efficiency Li2NiO2 preparation, and improves the electrochemical performance of lithium-ion batteries. and production efficiency.
Patent Information
- Application Number
- CN202410761174.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-01
AI Technical Summary
The existing Li2NiO2 preparation method has the problems of high calcination temperature, long time, complex process and slow reaction rate, which leads to reduced Coulombic efficiency of the first cycle of lithium-ion batteries and high material cost.
Flower-like nickel oxide is prepared by a precipitation method, and Ni(OH)2 is generated through hydrothermal reaction. The flower-like nickel oxide is then calcined in an air atmosphere. The flower-like nickel oxide is then mixed with a lithium source and calcined at high temperature in an inert atmosphere to produce high-quality nickel oxide. Pure Li2NiO2.
It increases the reaction rate of Li2NiO2, reduces the residual amount of nickel oxide and the amount of residual alkali on the surface, improves the electrochemical performance, simplifies the process flow, and is suitable for industrial production.
Smart Images

Figure CN118724088A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing flower-shaped nickelous oxide, a method for preparing a positive electrode lithium supplement Li2NiO2 by using the flower-shaped nickelous oxide and application thereof, belonging to the technical field of lithium ion batteries. Background Art
[0002] Lithium-ion batteries are widely used in mobile electronic devices, electric vehicles, energy storage and other fields. They are mainly composed of positive electrodes, negative electrodes, electrolytes, separators, etc. During the first charge and discharge stage of lithium-ion batteries, a solid electrolyte interface (SEI) will form at the interface of the negative electrode material of the battery, causing the loss of active lithium and resulting in a decrease in the coulombic efficiency of the battery's first cycle. To solve the problem of active lithium loss, the industry mainly uses "pre-lithiation" technology.
[0003] Positive lithium supplement Li2NiO2 is the main material used in the pre-lithiation technology of lithium-ion batteries. Chinese invention patent CN110218078A discloses a lithium supplement material Li2NiO2 and its preparation method and application. The invention uses Li2O and Ni2CO3 as raw materials, and obtains Li2NiO2 through ball milling, drying, low-temperature pre-sintering, ball milling, high-temperature sintering and other processes. At the same time, Chinese invention patent CN113571781B discloses a positive lithium supplement additive for lithium-ion batteries and its preparation method and lithium-ion batteries. The invention uses a composite lithium source and a nickel source, and obtains Li2NiO2 through mixing, high-temperature calcination, crushing and other steps. In addition, Chinese invention patent CN114122402A discloses a positive lithium supplement additive for lithium-ion batteries, a positive electrode sheet, its preparation method and use. The invention mixes a lithium source and a nickel source, and calcines at 500-700°C for 12-24h to obtain Li2NiO2.
[0004] In the published reports on the preparation of Li2NiO2, most of them only focus on the mixing process of nickel source and lithium source, calcination process, etc., and pay little attention to the properties of the nickel source of Li2NiO2 precursor; and the existing synthesis methods of Li2NiO2 have problems such as high calcination temperature, long calcination time, and complicated preparation process; obviously, the reaction rate of high-temperature reaction of nickel source and lithium source to generate Li2NiO2 is slow, which seriously restricts its industrial application. Studies have shown that the synthesis of Li2NiO2 is a liquid-solid or even solid-solid reaction. The nickel source (nickelous oxide) is a solid phase, and the lithium source (such as lithium hydroxide) is a liquid phase at the reaction temperature. As the reaction proceeds, lithium hydroxide is gradually dehydrated to form lithium oxide (solid state), so the later stage of the reaction is a solid-solid reaction. From the basic reaction engineering theory, we know that the reaction rates of liquid-solid and solid-solid reactions are usually slow, which is seriously restricted by the contact area (phase interface area) between the two phases and the mass transfer rate at the phase interface. Because the direct contact of the two reactants is a necessary condition for the reaction, the mass transfer rate in the solid phase is extremely slow, and the mass transfer rate in the liquid phase is not high. It can be seen that the existing NiO is a solid particle with a large particle size of about 400 nanometers, a small specific surface area, no pore structure, and a slow reaction rate. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for preparing flower-shaped nickelous oxide, which can effectively improve the reaction rate, produce Li2NiO2 with high purity, low residual nickelous oxide, small amount of residual alkali on the surface, and better electrochemical performance, a method for preparing positive electrode lithium supplement Li2NiO2 using the flower-shaped nickelous oxide, and its application.
[0006] In order to solve the above technical problems, the preparation method of flower-shaped nickelous oxide of the present invention comprises the following preparation steps:
[0007] (1) preparing a nickel soluble salt solution, a precipitant solution and a template solution, injecting the three solutions into a reaction kettle by a precipitation method, controlling the precipitation temperature at 20 to 40° C. and the precipitation pH value at 6 to 12, raising the temperature to between 60 and 150° C. after the feeding is completed, continuing the hydrothermal reaction for 4 to 24 hours, and then filtering, washing and drying to obtain Ni(OH)2;
[0008] (2) The dried Ni(OH)2 is placed in a calcining furnace and calcined at 250-500°C for 2-5 hours in an air atmosphere to obtain flower-shaped nickelous oxide.
[0009] The soluble salt of nickel in step (1) is one of nickelous sulfate, nickelous nitrate, nickelous chloride and nickelous acetate.
[0010] The precipitant in step (1) is one or more of NaOH, KOH, LiOH, ammonia water, urea and carbonate.
[0011] The template agent in step (1) is one or more surfactants selected from the group consisting of hexamethylenetetramine, 1,6-hexanediamine, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium bromide and the like.
[0012] The molar ratio of the soluble nickel salt of nickel to the template in step (1) is 1:0.05 to 1:2, OH - / Ni 2+ -ratio is greater than or equal to 2.0, the initial concentration of nickel salt is between 0.01 and 3.0 M, the hydrothermal reaction temperature is between 60 and 150 ° C, and the reaction time is between 4 and 24 hours.
[0013] The precipitation method in step (1) is one of the following: parallel flow precipitation method, forward addition method and reverse addition method.
[0014] The flower-like nickelous oxide is a secondary structure composed of thin nickelous oxide flakes (as petals), and the thickness of the nickelous oxide flakes is less than 50 nanometers. The flower-like nickelous oxide has a rich pore structure (pore volume 0.36-0.50 cm 3 / g, mesopore diameter between 10 and 17 nanometers) and high specific surface area (130 to 190 m 2 / g), the tap density of the flower-shaped nickelous oxide is 0.5-1.5 g / cm 3 .
[0015] A method for preparing a positive electrode lithium supplement Li2NiO2 using the above-mentioned flower-shaped nickelous oxide comprises the following steps:
[0016] (1) mixing flower-shaped nickelous oxide and a lithium source uniformly, wherein the molar ratio of lithium to nickel is 1.90:1 to 2.5:1;
[0017] (2) placing the mixed material in step (1) in a calcining furnace, and calcining it at a temperature of 550 to 750° C. for 8 to 16 hours under an inert atmosphere to obtain a positive electrode lithium supplement Li2NiO2.
[0018] The lithium source in step (1) is one of LiOH, LiOH·H2O and Li2CO3.
[0019] The prepared flower-like nickelous oxide is used as an active nickel source for the synthesis of lithium nickelate materials.
[0020] The advantages of the present invention are:
[0021] The invention adopts a precipitation method to react a nickel salt solution, a precipitant and a template agent to obtain Ni(OH)2, and then dries and calcines the Ni(OH)2 to obtain flower-shaped nickel oxide. The prepared flower-shaped nickel oxide of micron-sized (1-4 microns in diameter) is composed of thin flakes of about 50 nanometers in thickness. The flower-shaped nickel oxide has a rich pore structure and a high specific surface area. The high specific surface area (130-190 m 2 / g) increases the contact area between the lithium source and nickelous oxide, and the rich pore structure (pore volume is 0.36~0.50cm 3 / g, and the mesopore diameter is between 10 and 17 nanometers) is conducive to the diffusion of lithium source from the main phase to the phase interface, which greatly promotes the reaction rate. The thickness of the flower-shaped thin slice is less than 50 nanometers. During the reaction, the thin slice is easily etched with holes by lithium hydroxide, thereby generating more surface area, which promotes the reaction. For the synthesis of Li2NiO2 (liquid-solid and solid-solid reactions), the flower-shaped nickel oxide prepared by the present invention is conducive to accelerating the reaction speed, reducing the reaction temperature, shortening the reaction time, improving the product purity, reducing the residual alkali, and can greatly improve the production efficiency of Li2NiO2 and reduce its cost. In addition, its preparation process is simple and easy to operate, and is suitable for industrial scale-up production. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is the XRD spectrum of conventional nickelous oxide;
[0023] Figure 2 This is a SEM photo of conventional nickelous oxide.
[0024] Figure 3 is the XRD pattern of the flower-shaped nickelous oxide of the present invention;
[0025] Figure 4 This is a SEM photo of the flower-shaped nickelous oxide of the present invention;
[0026] Figure 5 The XRD pattern of Li2NiO2 prepared by the present invention;
[0027] Figure 6 The XRD diffraction patterns of Li2NiO2 prepared in Comparative Examples 1, 2 and Application Examples 1, 2 of the present invention. DETAILED DESCRIPTION
[0028] The following is a further detailed description of the method for preparing the flower-shaped nickelous oxide, the method for preparing the positive electrode lithium supplement Li2NiO2 using the flower-shaped nickelous oxide, and the application thereof, in conjunction with the accompanying drawings and specific embodiments.
[0029] Embodiment 1:
[0030] The method for preparing flower-shaped nickelous oxide of the present invention comprises the following preparation steps:
[0031] (1) preparing a nickel soluble salt solution, a precipitant solution and a template solution, injecting the three solutions into a reaction kettle by a precipitation method, controlling the precipitation temperature at 20 to 40° C. and the precipitation pH value at 6 to 12, raising the temperature to between 60 and 150° C. after the feeding is completed, continuing the hydrothermal reaction for 4 to 24 hours, and then filtering, washing and drying to obtain Ni(OH)2.
[0032] The precipitant is one or more of conventional precipitants such as NaOH, KOH, LiOH, ammonia water, urea and carbonate; the template is one or more of surfactants such as hexamethylenetetramine, 1,6-hexanediamine, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium bromide and the like (including common anionic surfactants, cationic surfactants, zwitterionic surfactants and nonionic surfactants); the soluble nickel salt is one of nickelous sulfate, nickelous nitrate, nickelous chloride and nickelous acetate; the molar ratio of the soluble nickel salt to the template is 1:0.05 to 1:2; OH - / Ni 2+ The ratio is greater than or equal to 2.0 (for the purpose of completely precipitating the nickel salt), the initial concentration of the nickel salt is between 0.01 and 3.0 M, the hydrothermal reaction temperature is between 60 and 150° C., and the reaction time is between 4 and 24 h (the yield is more than 90%);
[0033] The precipitation method is one of the following: parallel flow precipitation method, positive addition method and reverse addition method.
[0034] (2) The dried Ni(OH)2 is placed in a calcining furnace and calcined at 250-500°C for 2-5 hours in an air atmosphere to obtain flower-shaped nickelous oxide.
[0035] The flower-like nickel oxide is composed of thin sheets with a thickness of about 50 nanometers and has a rich pore structure (pore volume of 0.36 to 0.50 cm 3 / g, mesopore diameter between 10 and 17 nanometers) and high specific surface area (between 130 and 190 m 2 / g), the tap density of flower-shaped nickelous oxide is 0.5~1.5g / cm 3 .
[0036] Embodiment 2:
[0037] A method for preparing a positive electrode lithium supplement Li2NiO2 using the flower-shaped nickelous oxide described in Example 1 comprises the following steps:
[0038] (1) mixing flower-shaped nickelous oxide and a lithium source uniformly, wherein the molar ratio of lithium to nickel is 1.90:1 to 2.5:1;
[0039] (2) placing the mixed material in step (1) in a calcining furnace, and calcining it at a temperature of 550 to 750° C. for 8 to 16 hours under an inert atmosphere to obtain a positive electrode lithium supplement Li2NiO2.
[0040] Wherein, the lithium source in step (1) is one of LiOH, LiOH·H2O, and Li2CO3.
[0041] It has been verified that under the same preparation conditions, the reaction rate of flower-shaped nickelous oxide is faster, the obtained Li2NiO2 has higher purity, low nickelous oxide residue, less residual alkali on the surface, and better electrochemical performance. Compared with industrial nickelous oxide (solid particles of 300 nanometers, small specific surface area, and no pore structure), the flower-shaped nickelous oxide prepared by the present invention is more suitable for reacting with a lithium source to prepare Li2NiO2, that is, it is more suitable for the preparation of positive electrode lithium supplement Li2NiO2.
[0042] Embodiment three:
[0043] The flower-shaped nickelous oxide prepared in Example 1 can also be used as an active nickel source for the synthesis of other lithium nickelate materials, such as LiNiO2, ternary positive electrode materials NCM (nickel cobalt manganese LiNi 1-x-y Mn x Co y O2), NCA (nickel cobalt aluminum LiNi 1-x-y Co x Al y O2) etc.
[0044] The effects of the present invention are verified below in combination with comparative examples and application examples:
[0045] Comparative Example 1
[0046] Commercial nickelous oxide was mixed with LiOH in a molar ratio of lithium to nickel of 2.05:1. The mixture was placed in a calcining furnace and calcined at 550°C for 16 hours under an inert atmosphere to obtain Li2NiO2. The XRD diffraction pattern and scanning electron microscope photos of commercial nickelous oxide are shown in Figure 1 and Figure 2 .Depend on Figure 1 It can be seen that the XRD diffraction pattern of traditional nickelous oxide is consistent with the standard nickelous oxide diffraction pattern and has no impurity phase. Figure 2 Scanning electron microscope photos show that traditional nickel oxide is a solid polyhedron with uneven particle sizes ranging from 100 nanometers to 500 nanometers, with an average particle size of about 300 to 400 nanometers. The BET specific surface area measured by nitrogen adsorption and desorption experiments is 16.8 m 2 / g (see Table 1).
[0047] Comparative Example 2
[0048] Commercially available nickel oxide and LiOH·H2O were mixed evenly, with the molar ratio of lithium to nickel being 2.00:1. The mixed material was placed in a calcining furnace and calcined at 750°C for 8 hours under an inert atmosphere to obtain Li2NiO2.
[0049] Application Example 1
[0050] Prepare nickelous sulfate solution, NaOH solution and hexamethylenetetramine solution, and use the parallel flow method to inject the three solutions into the reactor at the same time. Among them, the molar ratio of nickelous sulfate and hexamethylenetetramine is 1:0.5. Control the precipitation temperature at 100°C and the precipitation pH value at 7. After the feeding is completed, continue stirring at a temperature of 100°C for 4 hours, then filter, wash and dry to obtain Ni(OH)2. Place the dried Ni(OH)2 in a calcining furnace and calcine at 300°C for 2 hours in an air atmosphere to obtain flower-shaped nickelous oxide. The tap density of the flower-shaped nickelous oxide is 1.0g / cm 3 The XRD diffraction pattern and scanning electron microscope image of the prepared flower-like nickel oxide are shown in Figure 3 and Figure 4 The XRD diffraction pattern of flower-like nickelous oxide is consistent with the standard diffraction pattern of nickelous oxide, and there is no impurity phase. Figure 4 The scanning electron microscope photo shows that the prepared nickel oxide has a flower-like structure with a diameter of about 4 to 8 microns. This flower-like structure is composed of a large number of ultra-thin nanosheets. The thickness of the nanosheet is about 30 nanometers. The BET specific surface area measured by nitrogen adsorption and desorption experiments is 134.8 m 2 / g, pore volume is 0.41cm 3 / g, and the average pore size is 17.5 nanometers (see Table 1). Compared with the traditional nickelous oxide in Comparative Example 1, the flower-shaped nickelous oxide prepared in Application Example 1 has the advantages of high specific surface area and high pore volume, rich pore structure, etc., which can effectively promote the interphase contact and interphase mass transfer between the lithium source and the nickel source, and is conducive to improving the reaction rate.
[0051] Mix flower-shaped nickelous oxide and LiOH evenly, with a molar ratio of lithium to nickel of 2.05:1. Place the mixture in a calcining furnace and calcine at 550°C for 16 hours under an inert atmosphere to obtain Li2NiO2. (Compare with Comparative Example 1)
[0052] Application Example 2
[0053] Application Example 2 is basically the same as Application Example 1, with the only difference being that the calcination process is 750° C. for 8 h to produce Li2NiO2 (compared with Comparative Example 2).
[0054] Application Example 3
[0055] Prepare nickelous nitrate solution, KOH solution and hexadecyltrimethylammonium bromide solution. Use the positive addition method to first add the nickelous nitrate solution into the reactor, and then slowly add the KOH solution and hexadecyltrimethylammonium bromide solution. The molar ratio of nickelous nitrate to hexadecyltrimethylammonium bromide is 1:0.2. Control the precipitation temperature at 60°C and the precipitation pH value at 10. After the feeding is completed, continue stirring at 60°C for 10 hours, then filter, wash and dry to obtain Ni(OH)2. Place the dried Ni(OH)2 in a calcining furnace and calcine at 250°C for 5 hours in an air atmosphere to obtain flower-shaped nickelous oxide. The tap density of the flower-shaped nickelous oxide is 0.5g / cm 3 The SEM photo of Application Example 3 is shown in Figure 5 , it can be seen that it is a flower-like structure with a petal thickness of about 30 nanometers.
[0056] The flower-like nickelous oxide and LiOH·H2O are uniformly mixed, and the molar ratio of lithium to nickel is 2.00:1. The mixed material is placed in a calcining furnace and calcined at 750°C for 8 hours under an inert atmosphere to obtain Li2NiO2.
[0057] Application Example 4
[0058] Prepare nickelous chloride solution, ammonia solution and octadecyltrimethylammonium bromide solution. Use the reverse addition method to first add the ammonia solution and octadecyltrimethylammonium bromide solution to the reactor, and then slowly add the nickelous chloride solution. The molar ratio of nickelous chloride to octadecyltrimethylammonium bromide is 1:2. Control the precipitation temperature to 80°C and the precipitation pH value to 8. After the feeding is completed, continue stirring at 90°C for 5 hours, then filter, wash and dry to obtain Ni(OH)2. Place the dried Ni(OH)2 in a calcining furnace and calcine at 500°C for 2 hours in an air atmosphere to obtain flower-shaped nickelous oxide. The tap density of the flower-shaped nickelous oxide is 1.5g / cm 3 .
[0059] The flower-shaped nickelous oxide and Li2CO3 are uniformly mixed, and the molar ratio of lithium to nickel is 1.90:1. The mixed material is placed in a calcining furnace and calcined at 600°C for 10 hours under an inert atmosphere to obtain Li2NiO2.
[0060] Application Example 5
[0061] Prepare nickelous acetate solution, KOH solution and 1,6-hexanediamine solution, and use the parallel precipitation method to inject the three solutions into the reactor. Among them, the molar ratio of nickelous acetate and 1,6-hexanediamine is 1:1. Control the precipitation temperature to 70°C and the precipitation pH value to 9. After the feeding is completed, continue stirring at a temperature of 80°C for 8 hours, then filter, wash and dry to obtain Ni(OH)2. Place the dried Ni(OH)2 in a calcining furnace and calcine at 400°C for 3 hours in an air atmosphere to obtain flower-shaped nickelous oxide. The tap density of the flower-shaped nickelous oxide is 0.8g / cm 3 .
[0062] The flower-shaped nickelous oxide and LiOH are uniformly mixed, and the molar ratio of lithium to nickel is 1.90:1 to 2.05:1. The mixed material is placed in a calcining furnace and calcined at 700°C for 8 hours under an inert atmosphere to obtain Li2NiO2.
[0063] Application Example 6
[0064] Prepare nickelous nitrate solution, ammonia solution and hexamethylenetetramine solution. Use positive addition method to first add nickelous nitrate solution into the reactor, and then slowly add ammonia solution and hexamethylenetetramine solution. The molar ratio of nickelous nitrate to hexamethylenetetramine is 1:0.8. Control the precipitation temperature at 95°C and the precipitation pH value at 6. After the feeding is completed, continue stirring at 95°C for 6 hours, then filter, wash and dry to obtain Ni(OH)2. Place the dried Ni(OH)2 in a calcining furnace and calcine at 350°C for 4 hours in an air atmosphere to obtain flower-shaped nickelous oxide.
[0065] The tap density of the flower-like nickelous oxide is 1.2 g / cm 3 .
[0066] The flower-like nickelous oxide and LiOH·H2O are mixed evenly, and the molar ratio of lithium to nickel is 1.95:1. The mixed material is placed in a calcining furnace and calcined at 650°C for 10 hours under an inert atmosphere to obtain Li2NiO2.
[0067] Application Example 7
[0068] Prepare nickelous sulfate solution, NaOH solution and hexamethylenetetramine solution. Use the reverse addition method to first add the NaOH solution and hexamethylenetetramine solution to the reactor, and then slowly add the nickelous sulfate solution. The molar ratio of nickelous sulfate to hexamethylenetetramine is 1:1.5. Control the precipitation temperature at 60-100°C and the precipitation pH value at 6-10. After the feeding is completed, continue stirring at a temperature of 60-100°C for 4-10 hours, then filter, wash and dry to obtain Ni(OH)2. Place the dried Ni(OH)2 in a calcining furnace and calcine at 250-500°C for 2-5 hours in an air atmosphere to obtain flower-shaped nickelous oxide. The tap density of the flower-shaped nickelous oxide is 1.0g / cm 3 .
[0069] The flower-shaped nickelous oxide and Li2CO3 are mixed evenly, and the molar ratio of lithium to nickel is 2.02:1. The mixed material is placed in a calcining furnace and calcined at 580°C for 12 hours under an inert atmosphere to obtain Li2NiO2.
[0070] Electrochemical performance test
[0071] The Li2NiO2, binder (PVDF), and conductive agent (SP) prepared in Comparative Examples 1 and 2 and Application Examples 1 to 7 are mixed in a mass ratio of 85:9:6, and N-methylpyrrolidone (NMP) is added as a dispersant to prepare a slurry. The slurry is evenly coated on an aluminum foil, dried, pressed into sheets, and then punched out. The sheets are dried in a drying oven at 80°C for 12 hours and then used for later use.
[0072] Metal lithium sheet was used as the counter electrode, LB-266 electrolyte was used, and the solvent was a three-component mixed solvent, i.e., a mixture of EC:DMC:EMC with a volume ratio of 1:1:1. Polypropylene film was used as the separator, and CR2032 button cells were assembled in a Braun glove box.
[0073] Test conditions: The charge and discharge test of button cells is carried out on the Blue Power Battery Test System. The charge and discharge voltage is 2.7-4.3V, the charge and discharge rate is 0.05C, and the first charge capacity is tested.
[0074] Nitrogen adsorption and desorption experiments were carried out on conventional nickelous oxide (Comparative Examples 1 and 2) and the flower-shaped nickelous oxide prepared in Application Examples 1 to 7, and their specific surface areas and pore structures were analyzed. The results are shown in Table 1. As can be seen from Table 1, the flower-shaped nickelous oxide prepared by the present invention has a higher specific surface area (greater than 100 m 2 / g) and rich pore structure (pore volume exceeds 0.3cm 3 / g, with larger macroscopic pores and mesoporous pores larger than 10 nanometers). The corresponding traditional nickel oxide has a small specific surface area and no pore structure.
[0075] Table 1 Pore structure analysis data of different nickel oxides
[0076]
[0077] Table 2 is an analysis of the Li2NiO2 prepared by Comparative Examples 1-2 and Application Examples 1-7. The residual nickelous oxide in the Li2NiO2 product was analyzed by XRD (external standard method). The residual alkali (LiOH and Li2CO3) in Li2NiO2 was detected by HCl standard solution titration. Figure 6 The XRD diffraction patterns of Li2NiO2 prepared by Comparative Examples 1, 2 and Application Examples 1, 2 are shown. It can be seen that the purity of the Li2NiO2 samples prepared by conventional nickelous oxide in Comparative Examples 1 and 2 is not high, and there are obvious nickelous oxide diffraction peaks, and the content of nickelous oxide exceeds 10%. This indicates that the reaction rate of conventional nickelous oxide with lithium source is slow, and the conversion of nickelous oxide is incomplete. However, the Li2NiO2 samples prepared by flower-shaped nickelous oxide have basically no nickelous oxide diffraction peaks, and the nickelous oxide content is less than 5%. This indicates that the flower-shaped nickelous oxide has high activity and fast reaction rate. Obviously, the fast reaction rate is attributed to the physicochemical properties of the flower-shaped nickelous oxide raw material synthesized by the present invention. According to the traditional reaction engineering principle, the flower-shaped nickelous oxide raw material nickelous oxide has a high specific surface area and rich pore structure (high pore volume and rich mesoporous pores), which can provide more interphase area and is conducive to the reaction; the rich mesoporous pore structure is conducive to the diffusion of reactants from the main phase to the interphase, and also promotes the reaction. It is worth noting that the petals of the flower-like nickelous oxide are ultra-thin, with a thickness of no more than 40 nanometers. As the reaction proceeds, more holes will be etched by the ultra-thin petals reacting with the lithium source, thereby generating more reaction interfaces, which is beneficial to promoting the reaction. The analysis results of other samples are shown in Table 2. As can be seen from Table 2, the Li2NiO2 sample prepared from flower-like nickelous oxide is significantly better than the sample prepared from traditional nickelous oxide, such as Li2NiO2 purity, nickelous oxide residue, residual alkali content and other indicators.
[0078] Table 2 Residual nickel oxide and residual alkali content of different Li2NiO2
[0079]
[0080] Table 3 lists the electrochemical performance test results of Li2NiO2 in Comparative Examples 1-2 and Application Examples 1-7. As can be seen from Table 3, the first charge capacity of the Li2NiO2 sample prepared from flower-shaped nickelous oxide is significantly better than that of the sample prepared from commercial nickelous oxide. The first charge capacity of Li2NiO2 prepared from traditional nickelous oxide is about 360mAh / g, while the first charge capacity of Li2NiO2 prepared from flower-shaped nickelous oxide exceeds 420mAh / g, an increase of ~17%.
[0081] Table 3 Electrochemical performance test results
[0082]
[0083] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. A method for preparing flower-shaped nickelous oxide, characterized in that: The method comprises the following preparation steps: (1) preparing a nickel soluble salt solution, a precipitant solution and a template solution, injecting the three solutions into a reaction kettle by a precipitation method, controlling the precipitation temperature at 20 to 40° C. and the precipitation pH value at 6 to 12, raising the temperature to between 60 and 150° C. after the feeding is completed, continuing the hydrothermal reaction for 4 to 24 hours, and then filtering, washing and drying to obtain Ni(OH)2; (2) The dried Ni(OH)2 is placed in a calcining furnace and calcined at 250-500°C for 2-5 hours in an air atmosphere to obtain flower-shaped nickelous oxide.
2. The flower-shaped nickelous oxide and the preparation method thereof according to claim 1, characterized in that: The soluble salt of nickel in step (1) is one of nickelous sulfate, nickelous nitrate, nickelous chloride and nickelous acetate.
3. The flower-shaped nickelous oxide and the preparation method thereof according to claim 1, characterized in that: The precipitant in step (1) is one or more of NaOH, KOH, LiOH, ammonia water, urea and carbonate.
4. The flower-shaped nickelous oxide and the preparation method thereof according to claim 1, characterized in that: The template agent in step (1) is one or more surfactants selected from the group consisting of hexamethylenetetramine, 1,6-hexanediamine, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium bromide and the like.
5. The flower-shaped nickelous oxide and its preparation method and use according to claim 1, characterized in that: In the step (1), the molar ratio of the soluble nickel salt of nickel to the template is 1:0.05 to 1:2, and the Ni 2+ / OH - The ratio is greater than or equal to 2.0, the initial concentration of the nickel salt is between 0.01 and 3.0 M, the hydrothermal reaction temperature is between 60 and 150° C., and the reaction time is between 4 and 24 h.
6. The flower-shaped nickelous oxide and the preparation method thereof according to claim 1, characterized in that: The precipitation method in step (1) is one of the following: parallel flow precipitation method, forward addition method and reverse addition method.
7. The flower-shaped nickelous oxide and the preparation method thereof according to claim 1, characterized in that: Flower-like nickel oxide is a secondary structure composed of thin nickel oxide flakes. The thickness of the nickel oxide flakes is less than 50 nanometers. Flower-like nickel oxide has a rich pore structure with a pore volume of 0.36 to 0.50 cm 3 / g, mesopore diameter between 10 and 17 nanometers and high specific surface area, with a surface area of 130 to 190 m 2 / g, the tap density of the flower-shaped nickelous oxide is 0.5-1.5 g / cm 3 .
8. A method for preparing a positive electrode lithium supplement Li2NiO2 using the flower-shaped nickelous oxide as claimed in any one of claims 1 to 7, characterized in that: The following steps are involved: (1) uniformly mixing flower-shaped nickelous oxide and a lithium source, wherein the molar ratio of lithium to nickel is 1.90:1 to 2.5:1; (2) The mixed material in step (1) is placed in a calcining furnace and calcined at 550-750° C. for 8-16 hours under an inert atmosphere to obtain a positive electrode lithium supplement Li2NiO2.
9. The method for preparing a positive electrode lithium supplement Li2NiO2 according to claim 8, characterized in that: The lithium source in step (1) is one of LiOH, LiOH·H2O and Li2CO3.
10. The flower-like nickelous oxide prepared in claim 1 is used as an active nickel source for the synthesis of other lithium nickelate materials, such as LiNiO2, ternary positive electrode materials NCM, NCA.
Citation Information
Cited By
New energy battery antimony-based negative electrode material and preparation method thereof
CN119725503A
An antimony-based anode material for a new energy battery and its preparation method
CN119725503B