Anode plate modification liquid and preparation method thereof, anode plate and preparation method thereof, and active oxygen water generator

By optimizing the molar ratio and preparation method of tin, antimony, and nickel elements in the anode plate modification solution, combined with the pipetting-sintering process, the problems of difficult control of ozone concentration and poor metal oxide layer technology in the traditional electrolysis method were solved, achieving high efficiency and stability. The active oxygen water is generated and the life of the anode plate is extended.

CN118724192APending Publication Date: 2024-10-01DONGGUAN NANBAI ELECTRONIC TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411107152.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When the traditional electrolysis method generates active oxygen water, the ozone concentration is difficult to control, the electrolysis performance is unstable and the efficiency is low, and the poor metal oxide layer technology leads to poor adhesion of precious metals and easy precipitation, causing heavy metal pollution, short service life, and limiting the activity. Application and promotion of oxygenated water.

Method used

An anode plate modification liquid is provided, which contains tin ions, antimony ions, nickel ions and citric acid. By optimizing the molar ratio and preparation method of these elements, and using a pipetting-sintering process, a metal oxide layer with good uniformity is formed, and the anode is improved. electrolytic performance and service life of the plate.

Benefits of technology

It achieves the performance of stably electrolyzing water to produce ozone in low conductivity media, improves the catalytic electrolysis efficiency and stability of the anode plate, extends the service life, reduces production costs, and reduces safety risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724192A_ABST
    Figure CN118724192A_ABST
Patent Text Reader

Abstract

The invention relates to an anode plate modification liquid and a preparation method thereof, an anode plate and a preparation method thereof, and an active oxygen water generator. The anode plate modification liquid comprises tin ions, antimony ions, nickel ions, citric acid and a solvent, and in the anode plate modification liquid, the molar ratio of the tin element to the antimony element to the nickel element is (40-54): (5-10): 1. By optimizing the molar ratio of the tin element, the antimony element and the nickel element in the anode plate modification liquid, the prepared anode plate has excellent performance of preparing ozone by electrolyzing water, and the ozone can still be stably prepared by electrolyzing water in a medium with relatively low conductivity; and citric acid is used for replacing hydrochloric acid, so that the uniformity of a metal oxide layer on the surface of the anode plate is improved, and the catalytic electrolysis performance of the anode plate is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of electrocatalysis, and in particular to an anode plate modification solution and a preparation method thereof, an anode plate and a preparation method thereof, and an active oxygen water generator. Background Art

[0002] Oxygenated water is a highly oxidizing aqueous solution made by dissolving ozone in water. Due to the strong oxidizing properties and broad-spectrum bactericidal ability of ozone, oxygenated water is widely used in medical and health care, food processing, drinking water treatment, home and public place disinfection, and agriculture.

[0003] At present, the main method for artificially preparing ozone is electrolysis. The electrolysis method uses a low-voltage DC power supply to directly electrolyze water to produce active oxygen water. The key to this process lies in the anode formula and its manufacturing process. However, traditional electrolysis technology has many shortcomings: (1) The concentration of ozone generated by electrolyzing water is difficult to control, and the electrolysis performance is unstable and the efficiency is low in a medium with low conductivity; (2) The metal oxide layer process is poor, and the precious metal has poor adhesion and is easy to precipitate, which in turn causes heavy metal pollution and has a short service life. These technical problems limit the application and promotion of active oxygen water. Summary of the invention

[0004] Based on this, it is necessary to provide an anode plate modification liquid and its preparation method, an anode plate and its preparation method, and an active oxygen water generator to improve the problems of mismatch between the formula of the existing anode plate and its preparation process, and the poor electrolytic performance and short life of the resulting anode plate.

[0005] In a first aspect of the present application, an anode plate modification solution is provided, comprising tin ions, antimony ions, nickel ions, citric acid and a solvent, wherein the molar ratio of tin element, antimony element and nickel element in the anode plate modification solution is 40~54:5~10:1.

[0006] In some embodiments, the molar ratio of nickel element to citric acid is 1:100-200.

[0007] In some embodiments, the molar concentration of nickel is 0.06 mol / L to 0.18 mol / L; and / or

[0008] The molar concentration of antimony element is: 0.6mol / L~0.9mol / L; and / or

[0009] The molar concentration of tin element is: 4mol / L~6mol / L.

[0010] In a second aspect of the present application, a method for preparing the anode plate modification solution provided in the first aspect of the present application is provided, comprising the following steps:

[0011] A tin source, an antimony source, a nickel source and citric acid are dissolved in a solvent, wherein the molar ratio of the tin element, the antimony element and the nickel element is 40-54:5-10:1.

[0012] In a third aspect of the present application, a method for preparing an anode plate is provided, comprising the following steps:

[0013] The titanium substrate is subjected to a pipetting-first sintering process, and then subjected to a pipetting-second sintering process;

[0014] The transfer-first sintering process comprises: transferring the anode plate modification solution provided in the second aspect of the present application to the surface of the titanium substrate, and performing a first sintering process;

[0015] The liquid transfer-second sintering process comprises: transferring the anode plate modification solution provided in the second aspect of the present application to the surface of the titanium substrate after the liquid transfer-first sintering process, and performing a second sintering process;

[0016] The sintering temperature of the second sintering process is higher than the sintering temperature of the first sintering process.

[0017] In some embodiments, the temperature of the first sintering treatment is 430° C. to 460° C.; and / or,

[0018] The first sintering treatment time is 8 minutes to 12 minutes; and / or,

[0019] The temperature of the second sintering treatment is 525° C. to 560° C.; and / or,

[0020] The second sintering treatment time is 40 min to 80 min.

[0021] In some embodiments, the transfer-first sintering process further includes: before the first sintering process, performing a first preheating process on the titanium substrate after transfer, the temperature of the first preheating process is 80°C to 120°C, and the time of the first preheating process is 8min to 10min; and / or,

[0022] The transfer-second sintering process further includes: before the second sintering process, performing a second preheating process on the titanium substrate after transfer, the temperature of the second preheating process is 80° C. to 120° C., and the time of the second preheating process is 8 min to 10 min.

[0023] In some embodiments, the pipetting-first sintering process is repeated 2 to 6 times.

[0024] In a fourth aspect of the present application, an anode plate is provided, which is prepared by the method for preparing the anode plate provided in the third aspect of the present application.

[0025] In a fifth aspect of the present application, an oxygenated water generator is provided, comprising an anode plate, a cathode plate and an electrolytic cell, wherein the anode plate is the anode plate provided in the fourth aspect of the present application, and the anode plate and the cathode plate are placed in the electrolytic cell, and the anode plate and the cathode plate are arranged opposite to each other with a gap.

[0026] The above-mentioned anode plate modification solution optimizes the molar ratio of tin, antimony and nickel elements, so that the subsequently prepared anode plate has excellent performance in electrolyzing water to produce ozone, and enables the oxygen water generator to stably electrolyze water to produce ozone in a medium with lower conductivity. By using citric acid instead of hydrochloric acid, not only the safety risk of the production process is reduced, but also anode plate modification solution with good uniformity is obtained, which helps to improve the uniformity of the metal oxide layer on the surface of the anode plate, thereby improving the catalytic electrolysis efficiency and stability of the anode plate.

[0027] The preparation method of the anode plate adopts a suitable brushing process and a sintering process in the pipetting-sintering process to obtain a metal oxide layer with better uniformity and stronger adhesion, thereby further improving the electrolytic performance and service life of the anode plate. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 Schematic diagram of the steps of a method for preparing an anode plate in one embodiment of the present application. DETAILED DESCRIPTION

[0029] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0030] In the description of this application, "multiple" means at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In this application, "at least one" means more than one, such as one, two and more than two. "Multiple" or "several" means at least two, such as two, three, etc.

[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0032] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0033] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0034] In this application, "above" or "below" includes the number itself. For example, "1 below" includes 1.

[0035] The temperature parameters in this application, unless otherwise specified, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.

[0036] The electrolysis method uses a low-voltage DC power supply to directly electrolyze water to generate active oxygen water. The key to this process lies in the anode formula and its manufacturing process. However, traditional electrolysis technology has many shortcomings: (1) The concentration of ozone generated by electrolyzing water is difficult to control, and the electrolysis performance is unstable and the efficiency is low in a medium with low conductivity; (2) The metal oxide layer process is poor, and the precious metal has poor adhesion and is easy to precipitate, which in turn causes heavy metal pollution and has a short service life. These technical problems limit the application and promotion of active oxygen water.

[0037] An embodiment of the present application provides an anode plate modification solution, which includes tin ions, antimony ions, nickel ions, citric acid and a solvent, wherein the molar ratio of tin, antimony and nickel in the anode plate modification solution is 40-54:5-10:1.

[0038] Optionally, the tin ions include Sn 2+ and Sn 4+ One or more of the antimony ions include Sb 3+ and Sb 5+One or more of the nickel ions include Ni 2+ .

[0039] The elemental composition of the metal oxide layer on the surface of the anode plate has an important influence on the efficiency of ozone production by electrolysis of water. Therefore, the molar ratio of tin, antimony and nickel in the anode plate modification solution is crucial. Among them, antimony can provide high-quality catalytic reaction sites, effectively improving the efficiency of ozone production by electrolysis. Adding a certain amount of antimony can also help the electrode to obtain a relatively stable electrolysis efficiency at a lower conductivity; nickel can improve the selectivity of ozone production by electrolysis of water by the electrode, which helps to improve the reaction activity of the antimony site. In addition, the use of the above elements instead of rare precious metal elements can also effectively reduce production costs.

[0040] Optionally, the molar ratio of tin, antimony and nickel is 40-54:5-10:1, including but not limited to 40:5:1, 40:10:1, 48:5:1, 48:8:1, 54:5:1, 54:10:1. When the molar ratio of tin, antimony and nickel is kept at the above ratio, anode plate modification solution with better performance can be obtained, which helps to improve the efficiency of preparing ozone by electrolyzing water of the prepared anode plate and the catalytic stability in low conductivity media.

[0041] In some embodiments, the molar ratio of nickel element to citric acid is 1:100-200, including but not limited to 1:100, 1:125, 1:140, 1:150, 1:175, 1:200.

[0042] Citric acid can form relatively stable complexes with metal ions, reduce the possibility of hydrolysis or precipitation of metal ions in the solution, and improve the stability of the solution. In addition, the coordination effect allows the metal complex to release metal ions more slowly, thereby providing a more uniform distribution of the metal oxide layer during the thermal decomposition process. Using citric acid instead of the hydrochloric acid component in the traditional anode plate modification solution can obtain a more stable anode plate modification solution, which is conducive to the subsequent preparation of a more uniform metal oxide layer. In addition, citric acid has lower corrosiveness than dilute hydrochloric acid, is safer for equipment and operators, and has less pollution to the environment.

[0043] In some embodiments, in the anode plate modification solution, the molar concentration of nickel element is: 0.06mol / L-0.18mol / L, including but not limited to: 0.06mol / L, 0.08mol / L, 0.10mol / L, 0.12mol / L, 0.16mol / L, 0.18mol / L; and / or, the molar concentration of antimony element is: 0.6mol / L~0.9mol / L, including but not limited to: 0.6mol / L, 0.7mol / L, 0.8mol / L, 0.9mol / L; and / or, the molar concentration of tin element is: 4mol / L~6mol / L, including but not limited to: 4mol / L, 5mol / L, 6mol / L.

[0044] When the molar concentration of the metal element in the anode plate modification liquid is high, the effect of the coating process on the uniformity of the coating may be magnified; when the molar concentration of the metal element in the anode plate modification liquid is low, it is not conducive to the formation of an effective metal oxide layer, and the thermal decomposition process needs to be repeated many times. Selecting the above molar concentration range of the metal element in the anode plate modification liquid can obtain a metal oxide layer with better uniformity and is convenient for industrial production.

[0045] Optionally, the solvent includes one or more of n-butanol and isobutanol.

[0046] Another embodiment of the present application provides a method for preparing the above-mentioned anode plate modification solution, comprising the following steps:

[0047] A tin source, an antimony source, a nickel source and citric acid are dissolved in a solvent, wherein the molar ratio of the tin element, the antimony element and the nickel element is 40-54:5-10:1.

[0048] Optionally, the solvent includes one or more of n-butanol and isobutanol.

[0049] Optionally, the tin source includes at least one of stannous chloride, stannic chloride and hydrates thereof.

[0050] Optionally, the antimony source includes at least one of antimony trichloride and antimony pentachloride.

[0051] Optionally, the nickel source includes at least one of nickel chloride and a hydrate thereof.

[0052] Alternatively, citric acid is mixed with ethanol to prepare a citric acid solution, the citric acid solution and a solvent in which various metal sources are dissolved are mixed, and after mixing, the ethanol in the mixed solution is evaporated.

[0053] In some embodiments, the anode plate modification solution is allowed to stand for 24 hours to 72 hours, including but not limited to 24 hours, 48 ​​hours, and 72 hours. The anode plate modification solution is allowed to stand for a period of time to form a more uniform metal oxide layer, thereby improving the electrolysis efficiency and stability of the anode plate.

[0054] Another embodiment of the present application provides a method for preparing an anode plate, comprising the following steps:

[0055] The titanium substrate is subjected to a pipetting-first sintering process, and then subjected to a pipetting-second sintering process;

[0056] The liquid transfer-first sintering treatment includes: transferring the anode plate modification liquid to the surface of the titanium substrate and performing the first sintering treatment;

[0057] The liquid transfer-second sintering process includes: transferring the anode plate modification solution to the surface of the titanium substrate after the liquid transfer-first sintering process, and performing a second sintering process;

[0058] The sintering temperature of the second sintering process is higher than the sintering temperature of the first sintering process.

[0059] In some embodiments, before the liquid transfer-first sintering process, a step of pre-treating the titanium substrate is also included. The pre-treating step is: grinding the titanium substrate and cleaning the polished titanium substrate. The polished titanium substrate is placed in an oxalic acid solution for etching, the etching temperature is 80°C to 90°C, and the etching time is 30min to 90min. The etched titanium substrate is cleaned to obtain a pre-treated titanium substrate.

[0060] Optionally, the etching temperature is 80°C to 90°C, including but not limited to: 80°C, 85°C, 90°C.

[0061] Optionally, the etching time is 30 min to 90 min, including but not limited to: 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, and 90 min.

[0062] Optionally, the mass concentration of the oxalic acid solution is 20wt%~50wt%, including but not limited to: 20wt%, 25wt%, 33.3wt%, 40wt%, 50wt%.

[0063] Optionally, the titanium substrate is subjected to graded grinding, and the mesh number of the grinding tool is 60 mesh to 180 mesh, including but not limited to: 60 mesh, 80 mesh, 100 mesh, 120 mesh, 150 mesh, and 180 mesh.

[0064] In some embodiments, the step of cleaning the polished titanium substrate comprises:

[0065] The titanium substrate is immersed in tap water and ultrasonically cleaned; the surface of the titanium substrate is scrubbed until there is no black dirt, and it is rinsed with tap water until there is no foam on the surface of the titanium substrate; the titanium substrate is cleaned with high-purity water.

[0066] In some embodiments, the step of cleaning the etched titanium substrate includes:

[0067] Rinse the titanium substrate in high-purity water at 40℃~50℃; put the titanium substrate into high-purity water, heat it to boiling, and keep boiling for 8s~20s.

[0068] In some embodiments, the step of pipetting-first sintering treatment includes: brushing the above-mentioned anode plate modification liquid evenly onto the surface of the pretreated titanium substrate to wet the entire surface of the titanium substrate, but not flowing down in streams, preheating at 80°C~120°C for 8min~10min, sintering at 430°C~460°C for 8min~12min, and naturally cooling to 50~70°C.

[0069] Compared with the dipping coating method, the brushing method can obtain a more uniform coating layer, thereby producing a more uniform metal oxide layer, thereby improving the electrolytic performance and durability of the anode plate.

[0070] Optionally, the temperature of the first preheat treatment is 80°C~120°C, including but not limited to: 80°C, 90°C, 100°C, 110°C, 120°C; the preheating time is 8min~10min, including but not limited to: 8min, 9min, 10min.

[0071] Optionally, the sintering temperature of the first sintering treatment is 430°C~460°C, including but not limited to: 430°C, 440°C, 450°C, 460°C; the sintering time is 8min~12min, including but not limited to: 8min, 9min, 10min, 11min, 12min.

[0072] In some embodiments, the step of pipetting-second sintering treatment includes: evenly brushing the above-mentioned anode plate modification liquid onto the surface of the titanium substrate after the pipetting-first sintering treatment, so that the surface of the titanium substrate is completely wetted, but not flowing down in streams, preheating at 80°C~120°C for 8min~10min, sintering at 525°C~560°C for 40min~80min, and naturally cooling to room temperature.

[0073] Optionally, the temperature of the second preheat treatment is 80°C~120°C, including but not limited to: 80°C, 90°C, 100°C, 110°C, 120°C; the preheating time is 8min~10min, including but not limited to: 8min, 9min, 10min.

[0074] Optionally, the sintering temperature of the second sintering treatment is 525°C~560°C, including but not limited to: 525°C, 535°C, 540°C, 550°C, 560°C; the sintering time is 40min~80min, including but not limited to: 40min, 50min, 60min, 70min, 80min.

[0075] In some embodiments, the pipetting-first sintering process is repeated 2 to 6 times, including but not limited to: 2 times, 3 times, 4 times, 5 times, 6 times.

[0076] In some embodiments, the placement direction of the titanium substrate is changed each time sintering is performed, the center point of the titanium substrate is kept unchanged, and the direction is changed based on the direction of the last placement, and the change is cyclically performed in the order of vertical flipping to the other side, rotating 90° clockwise, and vertical flipping to the other side. It can be understood that if the current change mode is vertical flipping to the other side, the next change mode is to rotate 90° clockwise and vertical flipping to the other side.

[0077] By using the above-mentioned brush coating process in combination with the sintering process, a more uniform metal oxide layer can be obtained, thereby improving the electrolytic performance of the anode plate.

[0078] Another embodiment of the present application provides an anode plate prepared by the above-mentioned method for preparing an anode plate.

[0079] Another embodiment of the present application provides an oxygenated water generator, including an anode plate, a cathode plate and an electrolytic cell, wherein the anode plate and the cathode plate are placed in the electrolytic cell, and the anode plate and the cathode plate are arranged opposite to each other with a gap.

[0080] In some embodiments, the distance between the anode plate and the cathode plate is 1 mm to 5 mm, including but not limited to 1 mm, 2 mm, 3 mm, 4 mm, and 5 mm.

[0081] Use the above-mentioned oxygenated water generator and apply 10mA / cm2 at a constant voltage of 10V~24V. 2 With an electric current of , water can be electrolyzed to produce ozone quickly and stably. The concentration of ozone increases steadily with the working time of the electrolysis generator, thereby achieving precise control of the concentration of active oxygen water.

[0082] The present application is further described in detail below in conjunction with specific embodiments.

[0083] In the following specific embodiments and comparative examples, the raw materials used, unless otherwise specified, are commercially available products with analytical purity; the instruments used, unless otherwise specified, are commercially available products; and the processes used, unless otherwise specified, are routinely selected by those skilled in the art.

[0084] Example 1

[0085] This embodiment provides an anode plate modifying solution and an anode plate.

[0086] The steps for preparing the anode plate modification solution are as follows:

[0087] Weigh 12 g of citric acid into a 50 mL beaker, add ethanol to 20 mL; adjust the bath temperature of the magnetic stirrer to 65 °C, place the beaker into the magnetic stirrer, continue stirring until the citric acid is completely dissolved, take out the beaker, seal the mouth of the beaker with plastic wrap and set aside.

[0088] Weigh 7g of tin tetrachloride pentahydrate, 0.73g of antimony trichloride, and 0.1g of nickel dichloride hexahydrate, put them into a 100mL beaker, and add n-butanol to 40mL; put the beaker into a magnetic stirrer, maintain the bath temperature at 65°C, adjust the speed so that the drugs do not splash, continue stirring until the drugs are completely dissolved, slowly add citric acid solution within 1 to 2 minutes, continue stirring until the solution evaporates to 40mL, take out the beaker, seal the cup mouth with plastic wrap, and let it stand for 48 hours before use.

[0089] The steps for preparing the anode plate are as follows:

[0090] The titanium substrate was sandblasted to a mesh size of 150. The titanium substrate was immersed in tap water and ultrasonically cleaned for 15 minutes; the titanium substrate was cleaned with a brush until there was no black dirt on the surface, and rinsed with tap water until there was no foam on the surface of the titanium substrate; the titanium substrate was rinsed three times with high-purity water, and after cleaning, it was placed in a beaker and soaked in high-purity water, and the mouth of the cup was covered with plastic wrap. Weigh 600mL of oxalic acid solution with a mass concentration of 33.3wt%, heat it to 85℃, put the titanium substrate into oxalic acid, and stir it continuously with a glass rod for 1 hour; clamp out the titanium substrate, put it into high-purity water at 40℃~50℃ for 30 seconds, and repeat the rinse three times; put the cleaned titanium substrate into high-purity water, heat it to boiling, and keep boiling for 10 seconds.

[0091] Place the anode plate in a 100°C oven and dry for 10 minutes. Use a brush to dip the anode plate modification liquid prepared in this embodiment, evenly brush both sides of the titanium substrate, put it on a shelf, and put it in a 100°C oven for preheating for 10 minutes; then, immediately put it in a 450°C high-temperature furnace and sinter it for 10 minutes; take it out and naturally cool it to 60°C, repeat the above brushing until it naturally cools to 60°C 5 times; after the sixth coating of the anode plate modification liquid, put it in a 100°C oven for preheating for 10 minutes, immediately put it in a 545°C high-temperature furnace, sinter it for 60 minutes; naturally cool it in the furnace for 10 hours. Among them, during each sintering, keep the center of the titanium substrate placed each time unchanged, and change the direction based on the direction of the last placement. The subsequent five changes are: vertical flip to the other side, rotate 90° clockwise and vertical flip to the other side, vertical flip to the other side, rotate 90° clockwise and vertical flip to the other side, and vertical flip to the other side.

[0092] Comparative Example 1

[0093] This comparative example provides an anode plate, and the preparation method of the anode plate is basically the same as that of Example 1, except that: the anode plate modification solution used is different. Compared with the anode plate modification solution of Example 1, the anode plate modification solution of this comparative example uses 3g of hydrochloric acid instead of citric acid.

[0094] Test Case

[0095] The prepared anode plate is used as the anode of the oxygenated water generator. The area of ​​the anode plate is 20 cm 2 The cathode is made of stainless steel sheet with an area of ​​20cm 2 , set the distance between the anode plate and the cathode plate to 5mm. Adjust the sodium sulfate electrolyte concentration in the water tank to 0.003mol / L, the circulating water flow rate to 2.5L / h, and the electrode current density to 10mA / cm 2 , the voltage is 18V, at room temperature 25°C, the ozone concentration of the oxygenated water generator including the anode sheets of each embodiment and the comparative example at different electrolysis times is tested by a dissolved ozone analyzer, and the ozone concentration of the above oxygenated water generator at different electrolysis times after the cumulative electrolysis reaction is 800h.

[0096] Test Example 1 and Test Example 2 correspond to the oxygenated water generator containing the anode plate of Example 1. Among them, Test Example 1 is an oxygenated water generator that has not been used, and Test Example 2 is an oxygenated water generator after 800 hours of cumulative electrolysis reaction. Test Example 3 and Test Example 4 correspond to the oxygenated water generator containing the anode plate of Comparative Example 1. Among them, Test Example 3 is an oxygenated water generator that has not been used, and Test Example 4 is an oxygenated water generator after 800 hours of cumulative electrolysis reaction.

[0097] The performance test data of each test case is shown in Table 1:

[0098] Table 1

[0099]

[0100] As can be seen from Table 1, the oxygenated water generator of Test Example 1 using the anode plate of Example 1 can obtain a stable and high ozone concentration for a long time. After 800 hours of cumulative electrolysis reaction, it can be seen from Test Example 2 that there is no significant difference in the stability and ozone concentration of its electrolysis to generate ozone. Test Example 3 using the anode plate of Comparative Example 1 has relatively poor stability and low ozone concentration, especially after 800 hours of cumulative electrolysis reaction, the ozone concentration of Test Example 4 has a significant decrease, and during the test time, the fluctuation between the maximum concentration and the minimum concentration is as high as 11%. It can be seen from the above data that compared with the anode plate of Comparative Example 1, the anode plate of Example 1 has a longer service life, and can still stably and efficiently electrolyze water to produce ozone after 800 hours of cumulative use.

[0101] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0102] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims, and the description may be used to interpret the content of the claims.

Claims

1. Anode plate modification solution, It is characterized in that The invention comprises tin ions, antimony ions, nickel ions, citric acid and a solvent. In the anode plate modification solution, the molar ratio of tin element, antimony element and nickel element is 40-54:5-10:

1.

2. The anode plate modification solution according to claim 1, It is characterized in that The molar ratio of nickel element to citric acid is 1:100~200.

3. The anode plate modification solution according to claim 1 or 2, It is characterized in that The molar concentration of nickel is 0.06mol / L~0.18mol / L; and / or The molar concentration of antimony element is: 0.6mol / L~0.9mol / L; and / or The molar concentration of tin element is: 4mol / L~6mol / L.

4. A method for preparing an anode plate modification solution, It is characterized in that The following steps are involved: A tin source, an antimony source, a nickel source and citric acid are dissolved in a solvent, wherein the molar ratio of the tin element, the antimony element and the nickel element is 40-54:5-10:

1.

5. A method for preparing an anode plate, It is characterized in that The following steps are involved: The titanium substrate is subjected to a pipetting-first sintering process, and then subjected to a pipetting-second sintering process; The transfer-first sintering treatment comprises: transferring the anode plate modification solution of any one of claims 1 to 3 to the surface of the titanium substrate, and performing a first sintering treatment; The transfer-second sintering treatment comprises: transferring the anode plate modification solution of any one of claims 1 to 3 to the surface of the titanium substrate after the transfer-first sintering treatment, and performing a second sintering treatment; The sintering temperature of the second sintering process is higher than the sintering temperature of the first sintering process.

6. The method for preparing the anode plate according to claim 5, It is characterized in that The temperature of the first sintering treatment is 430° C. to 460° C.; and / or, The first sintering treatment time is 8 minutes to 12 minutes; and / or, The temperature of the second sintering treatment is 525° C. to 560° C.; and / or, The second sintering treatment time is 40 min to 80 min.

7. The method for preparing the anode plate according to claim 6, It is characterized in that The liquid transfer-first sintering treatment further includes: before the first sintering treatment, performing a first preheating treatment on the titanium substrate after liquid transfer, the temperature of the first preheating treatment is 80° C. to 120° C., and the time of the first preheating treatment is 8 min to 10 min; and / or, The transfer-second sintering process further includes: before the second sintering process, performing a second preheating process on the titanium substrate after transfer, the temperature of the second preheating process is 80° C. to 120° C., and the time of the second preheating process is 8 min to 10 min.

8. The method for preparing the anode plate according to any one of claims 5 to 7, It is characterized in that Repeat the pipetting-first sintering process 2–6 times.

9. An anode plate, It is characterized in that The anode plate is prepared by the method for preparing the anode plate as described in any one of claims 5 to 8.

10. An oxygen water generator, It is characterized in that The invention comprises an anode plate, a cathode plate and an electrolytic cell, wherein the anode plate is the anode plate according to claim 9, the anode plate and the cathode plate are placed in the electrolytic cell, and the anode plate and the cathode plate are arranged opposite to each other with a gap.

Citation Information

Patent Citations

  • Ozone generating electrode, anode production process and ozone generator

    CN105002517A

  • Nickel-boron-antimony-co-doped stannic oxide electrical catalytic anode and preparation method and application thereof

    CN107555548A

  • Filtering type electro-catalysis disinfection reactor and disinfection method

    CN116177687A

  • System and method for electrochemical oxidation mitigation of harmful algal bloom and cyanotoxins

    US20210238065A1