Glass composition for optical fiber core, optical fiber, manufacturing method of optical fiber, application of optical fiber as gain medium, and optical fiber amplifier

By introducing specific amounts of Al2O3, M12O, M2O, La2O3 and GeO2 into the optical fiber core, the local environment of Er ions is optimized, the luminous intensity and gain spectrum flatness of the L-band are improved, and the L-band gain problem of existing optical fibers is solved. It is suitable for communication optical fiber and realizes industrial application with simple structure and low cost.

CN118724468APending Publication Date: 2024-10-01HUAWEI TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310353172.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The gain of existing optical fibers in the L-band (1565nm ~ 1625nm) is insufficient, especially after 1600nm, the gain is almost ineffective, and the gain spectrum is uneven, which cannot meet the bandwidth and capacity requirements of optical fiber communication.

Method used

A glass composition for optical fiber core is used, containing 35-75% P2O5, 5-20% Al2O3, 1-20% M12O, 1-10% M2O, 0.1-3% Er2O3, 0.1-5% La2O3 , 1~7.5% GeO2, through the introduction of specific amounts of Al2O3, M12O, M2O, La2O3 and GeO2, the local environment of Er ions is optimized, and the luminous intensity and gain spectrum flatness of the long wavelength in the L band are improved.

Benefits of technology

In the L-band long wavelength ≥1600nm part, the luminous intensity and gain spectrum flatness are significantly improved, and the gain coefficient is increased. It is suitable for L-band optical fiber as a gain medium, especially in communication applications. It has a simple structure, low cost, and is easy to industrialize.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724468A_ABST
    Figure CN118724468A_ABST
Patent Text Reader

Abstract

The invention relates to a glass composition for an optical fiber core, an optical fiber, a manufacturing method of the optical fiber, application of the optical fiber as a gain medium and an optical fiber amplifier. The glass composition for the fiber core of the optical fiber comprises the following components in percentage by mole in terms of oxides: 35-75% of P2O5, 5-20% of Al2O3, 1-20% of M12O, 1-10% of M2O, 0.1-3% of Er2O3, 0.1-5% of La2O3 and 1-7.5% of GeO2, M1 is at least one element selected from Li, Na, K, Rb and Cs, and M2 is at least one element selected from Mg, Ca, Sr, Ba and Zn. The optical fiber comprises a fiber core and at least one wrapping layer which is located on the outer side of the fiber core in the radius direction in the mode of surrounding the fiber core, and the fiber core is made of the glass composition for the fiber core of the optical fiber. The optical fiber amplifier provided by the invention adopts the optical fiber provided by the invention.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of optical fiber communication technology, and in particular to a glass composition for an optical fiber core, an optical fiber, and an optical fiber amplifier. Background Art

[0002] Currently, commercial erbium-doped silica fiber has been widely used in C-band (1530nm~1565nm) relay optical amplification, but has not yet been extended to the L-band (1565nm~1625nm), and cannot meet the growing bandwidth and capacity requirements of optical fiber communications.

[0003] In recent years, researchers have tried to obtain quartz optical fibers with large L-band gain bandwidth by modifying quartz optical fibers. However, quartz optical fibers still have problems such as difficulty in preparing high-concentration doping, low L-band long-wavelength gain, and uneven gain spectrum.

[0004] In the existing technology of L-band fiber amplification, erbium-doped tellurite fiber has a higher gain, but tellurite fiber has a high refractive index and poor mechanical properties, which is not conducive to fusion with commercial matching quartz fiber, bringing many uncontrollable factors to practical applications. In contrast, erbium-doped phosphate glass has attracted widespread attention due to its advantages such as high doping concentration, large gain coefficient, flat gain spectrum, and low cost. However, in the existing technology of quartz L-band erbium fiber, most of them can only support amplification in the 1570-1600nm band, and there is almost no gain after 1600nm.

[0005] In addition, even if the glass with amplification exists in the band after 1600nm, the performance in this band cannot meet the requirements of optical fiber. 2 O 5 The ratio of the content of Er-doped phosphate glass was used to obtain the extended L-band fluorescence of Er-doped phosphate glass. However, there are two shortcomings in this technical solution: first, the L-band gain is not flat enough, and the dispersion of Er ions is not considered; second, the performance characterization of the optical fiber is not involved. The accumulation of optical signal fiber in length will cause spectral changes. Therefore, there is still a need to improve the performance of optical fiber materials in the expansion of the L-band, especially in the expansion of the L-band in communication systems.

[0006] Patent Literature

[0007] Patent document 1: CN 113402166A Summary of the invention

[0008] In view of this, a glass composition for an optical fiber core is proposed, which has improved luminous intensity in the long wavelength (≥1600nm) part of the L band, increased gain spectrum flatness and increased gain coefficient, and is therefore suitable for making the core of an L-band optical fiber as a gain medium.

[0009] Also provided is an optical fiber, which has improved luminous intensity in the long wavelength (≥1600nm) part of the L-band, increased gain spectrum flatness and increased gain coefficient, and has a simple structure, low cost and easy industrialization. Therefore, it is suitable for L-band optical fiber as a gain medium, especially L-band optical fiber for communications.

[0010] A method for manufacturing an optical fiber is also provided, which can easily manufacture the optical fiber mentioned above in this application.

[0011] Also provided is a use of the optical fiber of the present application as a gain medium.

[0012] A fiber amplifier is also provided, which has an improved luminous intensity in a long wavelength (≥1600 nm) portion of an L-band, an increased gain spectrum flatness, and an increased gain coefficient.

[0013] In a first aspect, an embodiment of the present application provides a glass composition for an optical fiber core, which comprises, in terms of mole % of oxides, 35 to 75% P 2 O 5 、5~20% Al 2 O 3 , 1~20% M 1 2 O, 1~10% M 2 O, 0.1~3%Er 2 O 3 , 0.1~5% La 2 O 3 1~7.5% GeO 2 ,M 1 is at least one element selected from Li, Na, K, Rb, and Cs, M 2 It is at least one selected from Mg, Ca, Sr, Ba, and Zn.

[0014] In this case, the optical fiber core glass composition of the present application has improved luminous intensity in the long wavelength (≥1600nm) part of the L band, increased gain spectrum flatness and increased gain coefficient, and is therefore suitable for making the core of an L-band optical fiber as a gain medium.

[0015] According to the first aspect, in a first possible implementation of the optical fiber core glass composition, the optical fiber core glass composition, in terms of mole % converted into oxides, comprises: 40 to 65% P 2 O 5 、6~10% Al 2 O 3 , 5~12% M 12 O, 2~6%M 2 O, 0.2~2%Er 2 O 3 , 0.5~2.5%La 2 O 3 , 2~8%GeO 2 .

[0016] According to the first aspect, in the first or second possible implementations of the optical fiber core glass composition, M 1 K, M 2 For ba.

[0017] In a second aspect, an embodiment of the present application provides an optical fiber, comprising: a core and at least one cladding located radially outside the core in a manner surrounding the core, wherein the core is made of a glass composition for an optical fiber core according to any one of the first to third possible implementation methods of the first aspect.

[0018] In this case, by using the optical fiber core glass composition of the present application to make the core, the luminous intensity of the optical fiber of the present application in the long wavelength (≥1600nm) part of the L band is improved, and the gain spectrum flatness is increased and the gain coefficient is also increased. In addition, the structure is simple, the cost is low, and it is easy to industrialize. Therefore, it is suitable for L-band optical fiber as a gain medium, especially L-band optical fiber for communications.

[0019] According to the second aspect, in a first possible implementation of the optical fiber, at least one of the claddings is made of a glass composition A for optical fiber cladding, and the glass composition A for optical fiber cladding comprises: 35-75% P 2 O 5 、5~20%Al 2 O 3 , 1~20% M 1 2 O, 1~10% M 2 O, 1~7.5% GeO 2 ,M 1 is at least one element selected from Li, Na, K, Rb, and Cs, M 2 It is at least one selected from Mg, Ca, Sr, Ba, and Zn.

[0020] According to the second aspect, in the first or second possible implementation of the optical fiber, the composition of the glass composition A for the optical fiber cladding is the same as the composition of the glass composition for the optical fiber core, except that it does not contain Er and La.

[0021] According to the second aspect, in any one of the first to third possible implementations of the optical fiber, the optical fiber comprises only one cladding layer.

[0022] According to the second aspect, in any one of the first to fourth possible implementations of the optical fiber, the diameter of the fiber core is 80-200 μm, the thickness of the at least one cladding layer is 80-200 μm, and the diameter of the optical fiber is 180-400 μm.

[0023] In a third aspect, an embodiment of the present application provides a method for manufacturing an optical fiber according to any one of the first to fifth possible implementations of the second aspect, comprising:

[0024] a) preparing the glass composition for the optical fiber core,

[0025] b) preparing at least one glass composition for optical fiber cladding,

[0026] c) processing the optical fiber core glass composition into a glass rod, and processing at least one optical fiber cladding glass composition into a glass tube, respectively,

[0027] d) placing the glass rod and the at least one glass tube into a wire drawing device and drawing them.

[0028] In this case, the optical fiber of the present application is prepared by the "tube-rod method" commonly used in the art, and therefore, the above-mentioned optical fiber of the present application can be easily prepared, and therefore, the optical fiber prepared in the present application is easy to industrialize.

[0029] In a fourth aspect, an embodiment of the present application provides a use of an optical fiber as a gain medium according to any one of the first to fifth possible implementations of the second aspect.

[0030] In this case, as a gain medium, the light emission intensity in the long wavelength (≥1600 nm) portion of the L band is improved, and the gain spectrum flatness is increased and the gain coefficient is also increased.

[0031] In a fifth aspect, an embodiment of the present application provides a fiber amplifier, characterized in that the fiber amplifier uses an optical fiber according to any one of the first to fifth possible implementation methods of the second aspect.

[0032] In this case, by using the optical fiber of the present application, the luminous intensity of the optical fiber amplifier of the present application in the long wavelength (≥1600 nm) portion of the L band is improved, and the gain spectrum flatness is increased and the gain coefficient is also increased.

[0033] These and other aspects of the present application will become more apparent from the following description of the embodiment(s). BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The accompanying drawings, which are incorporated in and constitute a part of the specification, illustrate exemplary embodiments, features, and aspects of the present application and, together with the description, serve to explain the principles of the present application.

[0035] Figure 1 The fluorescence spectra of the optical fibers prepared in Example 1, Example 2 and Comparative Example 1 are shown.

[0036] Figure 2 The graph shows the results of a signal amplification test in the L band on the optical fiber of Example 2.

[0037] Figure 3 A test system for performing L-band signal amplification test on the optical fiber of Example 2 is shown. DETAILED DESCRIPTION

[0038] Various exemplary embodiments, features and aspects of the present application will be described in detail below with reference to the accompanying drawings. The same reference numerals in the accompanying drawings represent elements with the same or similar functions. Although various aspects of the embodiments are shown in the accompanying drawings, the drawings are not necessarily drawn to scale unless otherwise specified.

[0039] The word “exemplary” is used exclusively herein to mean “serving as an example, example, or illustration.” Any embodiment described herein as “exemplary” is not necessarily to be construed as preferred or advantageous over other embodiments.

[0040] In addition, in order to better illustrate the present application, numerous specific details are given in the following specific embodiments. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In some examples, methods, means, components and circuits well known to those skilled in the art are not described in detail in order to highlight the subject matter of the present application.

[0041] <First aspect>

[0042] In order to solve the above technical problems, the present application provides a glass composition for an optical fiber core, which comprises, in terms of mole % of oxide conversion: 35-75% P 2 O 5 、5~20% Al 2 O 3 , 1~20% M 1 2 O, 1~10% M 2 O, 0.1~3%Er 2 O 3 , 0.1~5%La 2 O 3 1~7.5%GeO 2 . M 1is at least one element selected from Li, Na, K, Rb, and Cs, M 2 It is at least one selected from Mg, Ca, Sr, Ba, and Zn.

[0043] Specifically, in the glass composition for optical fiber core of the present application, Al is simultaneously introduced in a specific amount. 2 O 3 、M 1 2 O.M. 2 O.La 2 O 3 and GeO 2 , optimizes the local environment of Er ions in the phosphate glass grid, increases the Stark splitting of Er ions, improves the luminous intensity of L-band long wavelengths, and increases the flatness of the gain spectrum; in particular, the introduction of a specific amount of La ions increases the dispersibility of Er ions, increases the effective doping concentration of Er ions, and thus increases the gain coefficient. Therefore, the glass composition for optical fiber core of the present application is suitable for making the core of L-band optical fiber.

[0044] In some preferred embodiments, from the viewpoint of better achieving the above technical effects of the present application, the glass composition for the optical fiber core preferably includes 40 to 65% P in terms of mol% converted to oxides. 2 O 5 , more preferably comprising 42 to 60% P 2 O 5 .

[0045] In some preferred embodiments, from the viewpoint of better achieving the above technical effects of the present application, the glass composition for the optical fiber core preferably includes 6 to 10% Al in terms of mol% calculated as oxide. 2 O 3 , more preferably 8 to 9.5% Al 2 O 3 .

[0046] In some preferred embodiments, from the viewpoint of better achieving the above technical effects of the present application, the glass composition for the optical fiber core preferably includes 5 to 12% M 1 2 O, more preferably 6.5 to 10.5% M 1 2 O.

[0047] In some preferred embodiments, from the viewpoint of better achieving the above technical effects of the present application, the glass composition for the optical fiber core preferably includes 2 to 6% M 2O, more preferably 3 to 5.5% M 2 O.

[0048] In some preferred embodiments, from the viewpoint of better achieving the above technical effects of the present application, the glass composition for the optical fiber core preferably includes 0.2 to 2% Er in terms of mole % converted to oxides. 2 O 3 , more preferably containing 0.5 to 1.5% Er 2 O 3 .

[0049] In some preferred embodiments, from the viewpoint of better achieving the above technical effects of the present application, the glass composition for the optical fiber core preferably includes 0.5 to 2.5% La in terms of mole % converted to oxides. 2 O 3 , more preferably containing 1-2% La 2 O 3 .

[0050] In some preferred embodiments, from the viewpoint of better achieving the above technical effects of the present application, the glass composition for the optical fiber core preferably includes 2 to 8% GeO in terms of mol% calculated as oxide. 2 , more preferably 4-6% GeO 2 .

[0051] In other preferred embodiments, from the perspective of better achieving the above technical effects of the present application and further reducing the manufacturing cost, M 1 Preferably, it is at least one element selected from Na and K, and more preferably, it is K.

[0052] In other preferred embodiments, from the perspective of better achieving the above technical effects of the present application and further reducing the manufacturing cost, M 2 Preferably, it is at least one selected from Mg, Ca, and Ba, and more preferably, it is Ba.

[0053] In the present application, within the scope of not impairing the technical effect of the present application, the glass composition for optical fiber core optionally contains other arbitrary components, which can be listed as B 2 O 3 、Bi 2 O 3 、As 2 O 5 , Sb 2 O 5 、TeO 2 , Ga 2 O 3 、In 2 O 3 、SiO2 、ZrO 2 ,FeO,Fe 2 O 3 , CuO, Sb 2 O 3 、SnO、SnO 2 、V 2 O 5 、MnO、MnO 2 、CeO 2 、MoO 3 、PbO、WO 3 Various oxide components used in glass compositions such as 2,4-dioxide, 2,6 ...

[0054] In some more preferred embodiments, the optical fiber core glass composition does not contain any other components except P. 2 O 5 、Al 2 O 3 、M 1 2 O.M. 2 O.E 2 O 3 ,La 2 O 3 ,GeO 2 Other ingredients besides.

[0055] <Second Aspect>

[0056] The present application provides an optical fiber comprising: a core and at least one cladding located radially outside the core in a manner surrounding the core, wherein the core is made of the glass composition for optical fiber core described in <First Aspect> of the present application.

[0057] Specifically, by using the glass composition for optical fiber core described in the <first aspect> of the present application to make a core, the optical fiber of the present application has an improved luminous intensity in the long wavelength (≥1600nm) part of the L-band, and the gain spectrum flatness is increased and the gain coefficient is also increased. In addition, the structure is simple, the cost is low, and it is easy to industrialize. Therefore, it is suitable for L-band optical fiber as a gain medium, especially L-band optical fiber for communications.

[0058] There is no particular limitation on the specific composition of the cladding glass of the optical fiber, and those commonly used in the art can be adopted. In addition, the composition of each cladding can be the same or different.

[0059] In some preferred embodiments, from the perspective of better achieving the technical effect of the present application, at least one of the more than one cladding layers is made of a glass composition A for optical fiber cladding, and the glass composition A for optical fiber cladding comprises: 35-75% P 2 O 5 、5~20% Al 2 O 3 , 1~20% M 1 2 O, 1~10% M 2 O, 1~7.5% GeO 2 , where M 1 is at least one element selected from Li, Na, K, Rb, and Cs, M 2 It is at least one selected from Mg, Ca, Sr, Ba, and Zn.

[0060] In addition, P 2 O 5 、Al 2 O 3 、M 1 2 O.M. 2 O、GeO 2 The content and M 1 and M 2 The more preferred embodiments of each are the same as those of P in the above optical fiber core glass composition. 2 O 5 、Al 2 O 3 、M 1 2 O.M. 2 O、GeO 2 The content and M 1 and M 2 The respective preferred embodiments are the same and will not be described in detail here.

[0061] In some more preferred embodiments, the composition of the optical fiber cladding glass composition A used to form at least one of the one or more cladding layers is the same as the composition of the optical fiber core glass composition except that Er and La are not contained.

[0062] In other embodiments, from the viewpoint of making the optical fiber structure simpler and facilitating industrial preparation and practical use, the optical fiber of the present application is preferably a single-clad optical fiber, that is, comprising only one cladding; more preferably, the single-layer cladding is made of the above-mentioned glass composition A for optical fiber cladding.

[0063] In the present application, in addition to the core and the cladding, the optical fiber of the present application may also have other layers as needed, for example, an intermediate layer adjacent to the radially outer side of the core in a manner of surrounding the core, a groove layer adjacent to the radially outer side of the intermediate layer in a manner of surrounding the intermediate layer, etc.

[0064] In the present application, there is no particular limitation on the size of the optical fiber, which can be appropriately adjusted according to actual needs such as actual application scenarios.

[0065] In some preferred embodiments, the diameter of the core in the optical fiber is preferably 80 to 200 μm, more preferably 100 to 160 μm.

[0066] In other preferred embodiments, the thickness of the cladding of at least one layer in the optical fiber is preferably 80 to 200 μm, more preferably 100 to 160 μm.

[0067] In other preferred embodiments, the diameter of the optical fiber is preferably 180-400 μm, more preferably 200-300 μm.

[0068] <Third Aspect>

[0069] The present application provides a method for manufacturing the optical fiber of the present application, which comprises: a) preparing the glass composition for the optical fiber core; b) preparing at least one glass composition for the optical fiber cladding; c) processing the glass composition for the optical fiber core into a glass rod, and processing at least one glass composition for the optical fiber cladding into glass tubes respectively; d) placing the glass rod and the at least one glass tube into a drawing device and drawing them.

[0070] Specifically, the optical fiber of the present application is prepared by the "tube-rod method" commonly used in the art, so the optical fiber of the present application can be easily prepared, and therefore, the optical fiber prepared in the present application is easy to industrialize. The following describes each step in detail.

[0071] (Step a): Preparation of glass composition for optical fiber core)

[0072] In the present application, the glass composition for optical fiber core can be prepared by various methods known in the art without any particular limitation. For example, it can be prepared by the following method.

[0073] First, a raw material mixture is prepared. The raw materials are not particularly limited as long as they are raw materials used in the manufacture of a common oxide-based glass composition, and oxides, carbonates, etc. can be used. For example, in some preferred embodiments, M 1 2 O (especially K 2 O) and M 2O (especially BaO) in the form of carbonates (such as K 2 CO 3 、BaCO 3 In addition, the types and proportions of the raw materials are appropriately adjusted in order to obtain the composition range of the optical fiber core glass composition of the present application.

[0074] Next, the raw material mixture is heated by a known method to obtain a melt. The heating and melting conditions are not particularly limited, and for example, the heating and melting temperature (melting temperature) may be 800 to 1400° C. and the heating and melting time may be 30 to 300 minutes.

[0075] Thereafter, the melt is cooled and solidified to obtain the glass composition for the optical fiber core of the present application. There is no particular limitation on the cooling method. A method of rapid cooling using a flattening machine, a press, or dripping into a cooling liquid may also be used.

[0076] The glass composition for an optical fiber core of the present application thus obtained may be in any form, for example, in the form of a block, a plate, a thin plate (scaly), or a powder.

[0077] (Step b): Preparation of glass composition for optical fiber cladding)

[0078] In the present application, the preparation of the glass composition for optical fiber cladding can be made by various methods known in the art without any particular limitation. For example, except for the different raw materials used, the example of the method for preparing the glass composition for optical fiber cladding is the same as the example of the method for preparing the glass composition for optical fiber core in the above step a).

[0079] In some preferred embodiments, at least one of the more than one glass compositions for optical fiber cladding is preferably the above-mentioned glass composition A for optical fiber cladding of the present application. In some more preferred embodiments, when only one cladding is used, the glass composition for optical fiber cladding is more preferably the above-mentioned glass composition A for optical fiber cladding of the present application.

[0080] (Step c): Preparation of preform)

[0081] In the present application, the glass composition for optical fiber core is processed into a glass rod, and at least one glass composition for optical fiber cladding is processed into a glass tube. Here, "glass tube" refers to a hollow glass cylinder.

[0082] Preferably, the size of the glass tube used to prepare the cladding adjacent to the core matches the size of the glass rod, and the sizes of the other glass tubes match each other. Here, "matching" refers to the state in which the glass tubes or the glass tube and the glass rod are adjacent to each other when they are nested with each other in the subsequent steps.

[0083] In the present application, there is no particular limitation on the method for manufacturing the glass rod and the glass tube, and various methods known in the art may be used.

[0084] (Step d): Drawing of preform)

[0085] In the present application, the glass rod and the at least one glass tube are placed in a drawing device and drawn. During the drawing process, the radial position relationship between the core and the cladding is maintained while drawing, so that the optical fiber has a suitable diameter.

[0086] There is no particular limitation on the wire drawing equipment used in this step. For example, a wire drawing tower may be used.

[0087] There is no particular limitation on the wire drawing conditions such as the wire drawing speed and the wire drawing temperature. For example, the wire drawing temperature may be 1400 to 4000°C.

[0088] <Fourth Aspect>

[0089] The present application provides a use of the optical fiber of the present application as a gain medium. As long as it can be used as a gain medium, there is no particular restriction on the use of the product using the optical fiber of the present application. For example, the optical fiber of the present application can be used to prepare a communication optical fiber amplifier, and is also applicable to other L-band optical fibers or solid-state lasers, etc.

[0090] In some preferred embodiments, the optical fiber of the present application is preferably used in an optical fiber amplifier.

[0091] <Fifth Aspect>

[0092] The present application provides an optical fiber amplifier, which adopts the optical fiber of the present application.

[0093] In the present application, there is no particular limitation on the structure of the optical fiber amplifier, which may be those known in the art.

[0094] In some specific embodiments, the optical fiber amplifier includes an L-band signal light source, a pump source, an isolator, a gain fiber (at least a portion of which uses the optical fiber of the present application), a matching passive quartz fiber, and a wavelength division multiplexer.

[0095] In some preferred embodiments, in the optical fiber amplifier, the optical fiber of the present application is fusion-spliced ​​with a commercial passive matching quartz optical fiber using a fusion splicer.

[0096] <Example>

[0097] The embodiments of the present application are described in detail below, but the present application is not limited to the following embodiments.

[0098] Embodiment 1:

[0099] In this embodiment, a single-clad optical fiber is prepared, as follows.

[0100] (1) Preparation of core and cladding glass: Weigh the raw materials according to molar percentage, where the core glass component is: 55 mol% P 2 O 5 、8.4mol%Al 2 O 3 、10mol%K 2 CO 3 , 5mol%BaCO 3 、1mol%Er 2 O 3 、1.5mol%La 2 O 3 , 5mol%GeO 2 ; The raw materials are mixed evenly and melted to obtain core glass; the cladding glass component is the above core glass component minus Er 2 O 3 ,La 2 O 3 , mixing the raw materials uniformly and melting them to obtain cladding glass;

[0101] (2) Preparation of preform: processing the core glass into a glass rod and processing the cladding glass into a glass tube matching the size of the core rod;

[0102] (3) Drawing of optical fiber: The core rod and the glass tube are placed in a drawing tower for drawing.

[0103] The diameter of the core in the optical fiber is 125 μm, and the diameter of the optical fiber is 250 μm.

[0104] Embodiment 2:

[0105] In this embodiment, a single-clad optical fiber is prepared, as follows.

[0106] (1) Preparation of core and cladding glass: Weigh the raw materials according to molar percentage, where the core glass component is: 45 mol% P 2 O 5 、9.2mol%Al 2 O 3 、7.1mol%K 2 CO 3 、3.2mol%BaCO 3 、1mol%Er 2 O 3 、1.5mol%La 2 O 3 , 5mol%GeO 2; The raw materials are mixed evenly and melted to obtain cladding glass;

[0107] (2) Preparation of preform: processing the core glass into a glass rod and processing the cladding glass into a glass tube matching the size of the core rod;

[0108] (3) Drawing of optical fiber: The core rod and the glass tube are placed in a drawing tower for drawing.

[0109] The diameter of the core in the optical fiber is 125 μm, and the diameter of the optical fiber is 250 μm.

[0110] Comparative Example 1:

[0111] In this comparative example, a single-clad optical fiber was prepared, as follows.

[0112] (1) Preparation of core and cladding glass: Weigh the raw materials according to molar percentage, where the main glass component of the core layer is: 55 mol% P 2 O 5 、1mol%Er 2 O 3 ; The raw materials are mixed evenly and melted to obtain cladding glass;

[0113] (2) Preparation of preform: processing the core glass into a glass rod and processing the cladding glass into a glass tube matching the size of the core rod;

[0114] (3) Drawing of optical fiber: The core rod and the glass tube are placed in a drawing tower for drawing.

[0115] The diameter of the core in the optical fiber is 125 μm, and the diameter of the optical fiber is 250 μm.

[0116] (Test results)

[0117] Figure 1 The fluorescence spectra of the optical fibers prepared in Example 1, Example 2 and Comparative Example 1 are shown in FIG. Figure 1 It can be seen that the fluorescence spectrum of the unoptimized phosphate optical fiber in comparative example 1 is relatively narrow, and the fluorescence intensity of the long wavelength in the L band is low; the spectrum of the optimized phosphate optical fiber in examples 1 and 2 is wide in the L band, and the fluorescence intensity of the long wavelength in the L band is also strong. In addition, in example 2 with a high amount after optimization, the fluorescence spectrum of the optical fiber is wider, and the gain of the long wavelength is greater.

[0118] Furthermore, the flatness was measured by the ratio of the fluorescence intensity at 1620 nm to that at 1600 nm. The I1620 / I1600 intensity ratios of Example 1 and Example 2 were 0.80 and 0.83, respectively, while the ratio in Comparative Example 1 was only 0.70.

[0119] Figure 2The signal amplification test of the L band is performed on the optical fiber of Example 2. It can be seen that the optical fiber of Example 2 of the present application has the characteristics of high L band flatness, high gain and large gain bandwidth.

[0120] The flow chart and block diagram in the accompanying drawings show the possible architecture, function and operation of the device, system, method and computer program product according to multiple embodiments of the present application. In this regard, each square frame in the flow chart or block diagram can represent a part of a module, program segment or instruction, and a part of the module, program segment or instruction includes one or more executable instructions for realizing the logical function of the specification. In some alternative implementations, the functions marked in the square frame can also occur in a sequence different from that marked in the accompanying drawings. For example, two continuous square frames can actually be executed substantially in parallel, and they can also be executed in reverse order sometimes, depending on the functions involved.

[0121] It should also be noted that each box in the block diagram and / or flowchart, and the combination of boxes in the block diagram and / or flowchart, can be implemented by hardware (such as a circuit or ASIC (Application Specific Integrated Circuit)) that performs the corresponding function or action, or can be implemented by a combination of hardware and software, such as firmware.

[0122] Although the present invention is described herein in conjunction with various embodiments, in the process of implementing the claimed invention, those skilled in the art may understand and implement other variations of the disclosed embodiments by viewing the drawings, the disclosure, and the appended claims. In the claims, the word "comprising" does not exclude other components or steps, and "one" or "an" does not exclude multiple situations. A single processor or other unit may implement several functions listed in the claims. Certain measures are recorded in different dependent claims, but this does not mean that these measures cannot be combined to produce good results.

[0123] The embodiments of the present application have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or improvements to the technology in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. A glass composition for an optical fiber core, characterized in that: In terms of mole % of oxide conversion, it includes: 35-75% P2O5, 5-20% Al2O3, 1-20% M 1 2O, 1~10%M 2 O, 0.1~3% Er2O3, 0.1~5% La2O3, 1~7.5% GeO2, M 1 is at least one element selected from Li, Na, K, Rb, and Cs, M 2 It is at least one selected from Mg, Ca, Sr, Ba, and Zn.

2. The glass composition for optical fiber core according to claim 1, characterized in that: In terms of mole % of oxide conversion, it includes: 40-65% P2O5, 6-10% Al2O3, 5-12% M 1 2O, 2~6%M 2 O, 0.2~2% Er2O3, 0.5~2.5% La2O3, 2~8% GeO2.

3. The glass composition for optical fiber core according to claim 1 or 2, characterized in that: M 1 K, M 2 For ba.

4. An optical fiber, characterized in that: It includes: A core and at least one cladding layer located radially outside the core so as to surround the core, wherein the core is made of the glass composition for an optical fiber core according to any one of claims 1 to 3.

5. The optical fiber according to claim 4, characterized in that At least one of the claddings is made of a glass composition A for optical fiber cladding, wherein the glass composition A for optical fiber cladding comprises: 35-75% P2O5, 5-20% Al2O3, 1-20% M 1 2O, 1~10%M 2 O, 1~7.5%GeO2, M 1 is at least one element selected from Li, Na, K, Rb, and Cs, M 2 It is at least one selected from Mg, Ca, Sr, Ba, and Zn.

6. The optical fiber according to claim 5, characterized in that The composition of the optical fiber cladding glass composition A is the same as the composition of the optical fiber core glass composition except that Er and La are not contained.

7. The optical fiber according to any one of claims 4 to 6, characterized in that: It contains only one cladding layer.

8. The optical fiber according to any one of claims 4 to 7, characterized in that: The diameter of the fiber core is 80-200 μm, the thickness of the at least one cladding layer is 80-200 μm, and the diameter of the optical fiber is 180-400 μm.

9. A method for manufacturing an optical fiber according to any one of claims 4 to 8, characterized in that: include: a) preparing the glass composition for the optical fiber core, b) preparing at least one glass composition for optical fiber cladding, c) processing the optical fiber core glass composition into a glass rod, and processing at least one optical fiber cladding glass composition into a glass tube, respectively, d) placing the glass rod and the at least one glass tube into a wire drawing device and drawing them.

10. Use of the optical fiber according to any one of claims 4 to 8 as a gain medium.

11. An optical fiber amplifier, characterized in that: The optical fiber amplifier uses the optical fiber according to any one of claims 4-8.