Low-shrinkage high-freezing-resistance sprayed concrete as well as preparation method and application thereof
Through the treatment of solid waste admixtures of magnesia slag, fly ash, silica fume, bagasse ash and sugarcane fiber, the problems of high shrinkage deformation and low frost resistance of shotcrete are solved, and low shrinkage and high frost resistance are achieved. Shotcrete promotes the utilization of solid waste resources and engineering applications.
Patent Information
- Application Number
- CN202411217779.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Shotcrete has problems of high shrinkage deformation and low frost resistance in engineering applications, which easily causes cracks and increases the risk of frost damage. At the same time, related industrial solid waste cannot be effectively utilized, causing environmental pollution.
Solid waste admixtures are prepared using magnesium slag, fly ash, silica fume, bagasse ash and sugarcane fiber. Through grinding and pre-water activation, combined with Ca(OH)2 solution treatment, low shrinkage and high frost resistance shotcrete is formed. , utilizing the pozzolanic activity, ball lubrication and filling effects of these materials to enhance the bridging effect of fibers and improve the concrete structure.
Significantly reduces the shrinkage rate of shotcrete and improves its frost resistance, reduces the volume shrinkage phenomenon during the curing process, and enhances the resistance to low-temperature freeze-thaw cycles, realizing the utilization of solid waste resources, and is suitable for strict shrinkage control and engineering construction with high frost resistance requirements.
Smart Images

Figure CN118724540A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, in particular to shotcrete, and more particularly to a low-shrinkage, high-freeze-resistant shotcrete and a preparation method and application thereof. Background Art
[0002] Shotcrete is widely used in various tunnel projects and support (anchor support, lining support, etc.) projects due to its special construction method, extremely short initial and final setting time and high early strength. However, due to the use of accelerators and the injection molding process, shotcrete has the characteristics of high porosity. During the hydration process of concrete, the hydration reaction of cementitious materials and the evaporation of water in a dry environment jointly lead to the occurrence of shrinkage. The high porosity of shotcrete provides a convenient channel for the transmission of water in it. The rapid transmission of water causes large early shrinkage deformation of shotcrete. In addition, shrinkage of concrete can easily lead to cracks, thereby increasing the risk of concrete damage by freezing.
[0003] Magnesium slag is the reduction waste discharged from the smelting of magnesium in magnesium metal plants. Generally, 5 to 10 tons of waste slag can be produced for every ton of magnesium metal refined. However, due to the lack of safe and effective utilization methods, most of the magnesium slag is landfilled in gullies or stored on the surface, posing a certain threat to the ecological environment. Bagasse is the waste left by sugar mills after squeezing sugarcane. Bagasse is generally used as fuel to produce steam and electricity. In this process, a large amount of bagasse ash is inevitably produced. If these bagasse ash are not properly handled, it is very likely to cause new environmental challenges. Fly ash and silica fume are two important industrial by-products, which are widely used in the field of concrete. Fly ash is unburned fine particles produced by coal-fired boilers during the combustion process, which are collected by dust removal systems. It is gray or gray-black, contains a variety of oxide components, such as silicon, aluminum, iron, etc., has volcanic ash properties, can replace part of cement in concrete, and improve the performance of concrete. Silica fume, also known as silicon micropowder or microsilica powder, is a by-product produced during the smelting of ferrosilicon alloys and industrial silicon, which is collected and processed by special devices. Silica fume particles are extremely fine, with an average particle size close to the nanometer level. They are extremely active and are a high-quality concrete admixture that can significantly improve the strength and durability of concrete.
[0004] In view of the problems existing in the engineering application of shotcrete, and taking into account the waste of related industrial solid waste and the pollution to the environment, it is necessary to conduct relevant research and improvement attempts to solve the problems of high shrinkage deformation and low frost resistance of shotcrete while turning waste into treasure and achieving green development. Summary of the invention
[0005] To solve the above problems, the present invention provides a low shrinkage, high frost resistance shotcrete and a preparation method and application thereof, so as to solve the problems of high shrinkage deformation and low frost resistance of shotcrete in engineering applications.
[0006] The present invention is achieved in that:
[0007] The present invention provides a low shrinkage, high frost resistance shotcrete in one aspect, comprising by weight:
[0008] 12-18 parts of cement, 6-9 parts of water, 30-40 parts of fine aggregate, 30-40 parts of coarse aggregate, 2-8 parts of solid waste admixture, 1-2 parts of accelerator, 0.1-0.3 parts of water reducer; and
[0009] The solid waste admixture comprises, by weight: 30-40 parts of magnesium slag, 15-20 parts of fly ash, 10-15 parts of silica ash, 10-20 parts of bagasse ash and 10-20 parts of sugarcane fiber.
[0010] As a further improvement of any of the above schemes, the solid waste admixture comprises, by weight: 35 parts of magnesium slag, 15 parts of fly ash, 15 parts of silica ash, 15 parts of bagasse ash and 15 parts of sugarcane fiber.
[0011] As a further improvement of any of the above schemes, the solid waste admixture comprises, by weight: 30 parts of magnesium slag, 15 parts of fly ash, 10 parts of silica ash, 10 parts of bagasse ash and 10 parts of sugarcane fiber.
[0012] As a further improvement of any of the above schemes, the solid waste admixture comprises, by weight: 40 parts of magnesium slag, 20 parts of fly ash, 15 parts of silica ash, 20 parts of bagasse ash and 20 parts of sugarcane fiber.
[0013] As a further improvement of any of the above solutions, the solid waste admixture is prepared according to the following process:
[0014] Weigh 30-40 parts of magnesium slag, 15-20 parts of fly ash, 10-15 parts of silica ash, 10-20 parts of bagasse ash and 10-20 parts of sugarcane fiber by weight;
[0015] Magnesium slag, fly ash and bagasse ash were ground to a specific surface area of 400-500 m 2 / kg, grind the silica fume to a specific surface area of 2000-3000 m 2 / kg;
[0016] The ground magnesium slag, fly ash and bagasse ash are added with the ground silica ash and sugarcane fiber and mixed evenly;
[0017] After mixing, add 10-20 parts of saturated Ca(OH)2 solution for pre-absorption of water and activation.
[0018] As a further improvement of any of the above solutions, the cement is ordinary Portland cement or sulfate-resistant cement; and / or
[0019] The fine aggregate is natural sand or machine-made sand with a fineness modulus of 2.6; and / or
[0020] The coarse aggregate is crushed stone or ceramsite with a continuous gradation of 5-10 mm; and / or
[0021] The accelerating setting agent is an aluminum sulfate type alkali-free accelerating setting agent or a hydrofluoric acid type alkali-free accelerating setting agent; and / or
[0022] The water reducing agent is a polycarboxylate water reducing agent.
[0023] As a further improvement of any of the above schemes, the magnesium slag comprises by weight: 40-65 parts of CaO, 60-80 parts of SiO2, 5-8 parts of MgO, and 2-5 parts of Fe2O3; and / or
[0024] The fly ash comprises by weight: 2.5-10 parts of CaO, 35-55 parts of SiO2, 20-30 parts of Al2O3, 0.5-2 parts of MgO, 0.5-1 parts of SO3, 2-20 parts of Fe2O3; and / or
[0025] The silica ash comprises by weight: 0.1-0.5 parts of CaO, 90-96 parts of SiO2, 0.5-2 parts of Al2O3, and 0.5-2 parts of MgO; and / or
[0026] The bagasse ash comprises by weight: 60-80 parts of SiO2, 10-20 parts of Al2O3, 1-5 parts of CaO, 1-3 parts of MgO, 3-8 parts of Fe2O3, 1-6 parts of K2O, and 1-2 parts of Na2O; and / or
[0027] The mass fraction of the sugarcane fiber is as follows: 40-50 parts of cellulose, 20-30 parts of hemicellulose, 1-5 parts of acid-soluble lignin, and 15-25 parts of acid-insoluble lignin.
[0028] As a further improvement of any of the above solutions, the shrinkage rate of the low-shrinkage, high-freeze-resistant shotcrete is not higher than 365 με, and the frost resistance is not lower than F250.
[0029] Another aspect of the present invention provides a method for preparing the low shrinkage and high frost resistance shotcrete, comprising the following steps:
[0030] Weigh the required raw materials according to the proportion, mix cement, solid waste admixture, fine aggregate and coarse aggregate, add water and slowly add water reducing agent to obtain concrete;
[0031] Atomized concrete and accelerator are sprayed at the nozzle of the spray mixer to form a beam to obtain sprayed concrete.
[0032] Another aspect of the present invention provides an application of the low shrinkage, high frost resistance shotcrete in low temperature freeze-thaw cycle support engineering.
[0033] The beneficial effects of the present invention on the prior art are as follows: the present invention provides a low-shrinkage, high-freeze-resistant shotcrete and a preparation method and application thereof. Aiming at the problems of high shrinkage deformation and low frost resistance of shotcrete, the present invention synergistically utilizes magnesium slag, fly ash, silica ash, bagasse ash and sugarcane fiber to prepare solid waste admixtures, utilizes the volcanic ash activity of magnesium slag, fly ash, silica ash and bagasse ash, the ball lubrication and filling effects of fly ash and silica ash, and the toughening effect of bagasse ash and sugarcane fiber, utilizes saturated Ca(OH)2 solution to activate the reaction of the solid waste admixtures, and at the same time pre-absorbs water for magnesium slag and bagasse ash, so that they continuously release water, thereby improving the high shrinkage deformation performance and frost resistance of shotcrete, and the shrinkage rate can be reduced to 365 με or less, and the frost resistance can reach F250 or above. The present invention not only effectively promotes the resource recovery and high-value utilization of solid waste, but also significantly reduces the volume shrinkage of shotcrete during the solidification process, while greatly enhancing its ability to resist damage from low-temperature freeze-thaw cycles. It can be widely used in various engineering construction projects that require strict shrinkage control and high frost resistance of concrete materials, especially shotcrete support projects.
[0034] It should be understood that the implementation of any embodiment of the present invention does not mean that multiple or all of the above-mentioned beneficial effects must be possessed or achieved at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. Obviously, the drawings in the following description are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.
[0036] The structures, proportions, sizes, etc. illustrated in this specification are only used to match the contents disclosed in the specification so as to facilitate understanding and reading by persons familiar with the technology. They are not used to limit the conditions under which the present invention can be implemented, and therefore have no substantial technical significance. Any structural modification, change in proportion or adjustment in size shall still fall within the scope of the technical contents disclosed in the present invention without affecting the effects and purposes that can be achieved by the present invention.
[0037] Figure 1 A schematic diagram of a ground mineral admixture for shotcrete according to the present invention is shown as an example;
[0038] Figure 2 A schematic diagram of a sprayed concrete slab according to the present invention is shown as an example;
[0039] Figure 3 A schematic diagram of cutting a large slab of shotcrete according to the present invention is shown as an example;
[0040] Figure 4 A schematic diagram of a shrinkage experiment of shotcrete according to the present invention is shown as an example;
[0041] Figure 5 A schematic diagram of a freeze-thaw experiment of shotcrete according to the present invention is shown as an example;
[0042] Figure 6 The following is a schematic diagram showing the comparison of shrinkage and frost resistance of a shotcrete according to the present invention. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical solution and advantages of the embodiments of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in conjunction with the embodiments and drawings. Here, the illustrative embodiments of the present invention and their description are used to explain the present invention, but are not intended to limit the present invention.
[0044] It should be understood that the terms "include / comprise", "consist of..." or any other variations are intended to cover non-exclusive inclusion, so that a product, device, process or method that includes a series of elements includes not only those elements, but also may include other elements not explicitly listed when necessary, or also include elements inherent to such product, device, process or method. Without further restrictions, the sentences "include / comprise...", "consist of..." and similar terms should be understood as open inclusion, that is, "including but not limited to", and the elements defined therein do not exclude the presence of other identical elements in the product, device, process or method that includes the elements. The term "based on" should be understood as "based at least in part on". The term "one embodiment" or "the embodiment" should be understood as "at least one embodiment". The terms "first", "second", etc. may refer to different or identical objects.
[0045] In view of the problems of high shrinkage deformation and low frost resistance of shotcrete mentioned in the background technology, in order to significantly reduce the shrinkage deformation of shotcrete and improve its ability to resist damage from low-temperature freeze-thaw cycles, the present invention has successfully developed a shotcrete material that has both low shrinkage characteristics and excellent frost resistance.
[0046] The low shrinkage, high frost resistance shotcrete and its preparation method, specific implementation of application and better preferred scheme proposed by the present invention are described in detail below.
[0047] Unless otherwise specified, the raw materials, additives, and instruments and equipment in the embodiments of the present invention can be purchased through commercial channels.
[0048] The invention first provides a low shrinkage and high frost resistance shotcrete, which comprises, by weight, 12-18 parts of cement, 6-9 parts of water, 30-40 parts of fine aggregate, 30-40 parts of coarse aggregate, 2-8 parts of solid waste admixture, 1-2 parts of accelerator, and 0.1-0.3 parts of water reducer; wherein the solid waste admixture comprises, by weight, 30-40 parts of magnesium slag, 15-20 parts of fly ash, 10-15 parts of silica ash, 10-20 parts of bagasse ash and 10-20 parts of sugarcane fiber.
[0049] The present invention synergistically utilizes the volcanic ash activity of magnesium slag, fly ash, silica ash and bagasse ash, the ball lubrication and filling effect of fly ash and silica ash, the toughening effect of bagasse ash and sugarcane fiber, and the internal curing and activation effect of Ca(OH)2 to prepare a new type of solid waste admixture. Subsequently, by integrating the solid waste admixture into the formula of shotcrete, a shotcrete material with both low shrinkage characteristics and excellent antifreeze performance is obtained.
[0050] As a preferred implementation scheme, the solid waste admixture is prepared according to the following process:
[0051] Weigh 30-40 parts of magnesium slag, 15-20 parts of fly ash, 10-15 parts of silica ash, 10-20 parts of bagasse ash and 10-20 parts of sugarcane fiber by weight;
[0052] Magnesium slag, fly ash and bagasse ash were ground to a specific surface area of 400-500 m 2 / kg, grind the silica fume to a specific surface area of 2000-3000 m 2 / kg;
[0053] The ground magnesium slag, fly ash and bagasse ash are added with the ground silica ash and sugarcane fiber and mixed evenly;
[0054] After mixing, add 10-20 parts of saturated Ca(OH)2 solution for pre-absorption of water and activation.
[0055] The technical principles and effects of the present invention are as follows:
[0056] 1. Potential expansion characteristics of magnesium slag: The activity of magnesium slag after mechanical activation and Ca(OH)2 excitation is greatly improved. During the hydration process, MgO hydrates to produce Mg(OH)2 with micro-expansion properties, as shown in Formula 1; Mg3N2 hydrates to produce Mg(OH)2 and NH3, as shown in Formula 2. The Mg(OH)2 produced by hydration can effectively compensate for the shrinkage deformation of shotcrete, and NH3 can form tiny pores, offsetting the hydrostatic pressure in the capillary pores in part of the concrete, reducing the expansion pressure, and enhancing the frost resistance of shotcrete.
[0057] MgO + H2O→Mg(OH)2 (1)
[0058] Mg3N2+ 6H2O→Mg 2+ +6OH - +3NH3 (2)
[0059] Second, the pozzolanic activity of magnesium slag, fly ash, silica fume, and bagasse ash: During the cement hydration reaction, cement dissolves in water to form a cement pore solution environment, which contains Ca-rich 2+ 、SiO4 4- 、HSiO3 4- and [Al(OH)6] 3− Liquid phase reaction system of plasma. Magnesium slag, fly ash, silica ash and bagasse ash can continuously react with ions in the liquid phase to produce hydration products such as Ca(OH)2, CSH (Formula 3), and CASH gel (Formula 4), which can adjust the pore structure of concrete, thereby extending the water evaporation path and effectively slowing down the rate of drying shrinkage, thereby reducing the shrinkage of shotcrete and improving the frost resistance of shotcrete.
[0060] Ca 2+ +Si-O+OH - →(CSH)+H2O (3)
[0061] 6Ca 2+ +2Al(OH)4 - +3SO4 2- +4OH - +26H2O→Ca6Al2(SO)3(OH) 12 26H2O (4)
[0062] 3. The ball lubrication and filling effect of fly ash and silica fume: The spherical micro-beads in fly ash and silica fume lubricate like "balls" during concrete mixing, reducing aggregate friction, improving workability and fluidity, and making the components more evenly mixed, thereby improving the internal structure of concrete to reduce shrinkage cracks while improving frost resistance; in addition, fly ash and silica fume fill the voids of cement particles with their extremely fine particles, increase density, refine pore structure, reduce shrinkage and improve frost resistance.
[0063] Fourth, the toughening effect of bagasse ash and sugarcane fiber: After the Ca(OH)2 pre-reaction, the hemicellulose in bagasse ash and sugarcane fiber begins to decompose and gradually refine, and the contact area between the fiber and the concrete substrate also expands, which greatly enhances the physical and chemical bonding between the fiber and the substrate. This enhanced bonding helps to form a tighter and more stable structure inside the concrete, effectively reducing cracks caused by stress concentration. When experiencing freeze-thaw cycles, the bridging effect of the fiber can reduce the expansion of microcracks inside the concrete, thereby improving the concrete's resistance to freeze-thaw cycles.
[0064] 5. Ca(OH)2 internal curing and activation: Pre-wetting of solid waste admixtures allows them to act as a "water reservoir" in concrete. When the free water in the cement paste is consumed to a certain extent, the water stored in the solid waste admixtures begins to diffuse around, promoting the hydration reaction of the surrounding unhydrated cementitious materials and increasing the internal relative humidity and hydration degree of the cement paste. Pre-wetting of solid waste admixtures ensures that the concrete can continue to obtain the required water during the hydration process, thereby avoiding internal "self-drying phenomenon" and early self-shrinkage, and reducing the generation of microcracks.
[0065] Based on the above principles, with the help of the volcanic ash activity of magnesium slag, fly ash, silica ash and bagasse ash, the ball lubrication and filling effect of fly ash and silica ash, the toughening effect of bagasse ash and sugarcane fiber, and the internal curing and activity stimulation effect of Ca(OH)2 solution, the low shrinkage and high frost resistance shotcrete can achieve the recycling of magnesium slag, fly ash, silica ash, bagasse ash and sugarcane fiber, while effectively reducing the shrinkage rate of shotcrete (no more than 365 με) and significantly improving the frost resistance of shotcrete (F250, F300).
[0066] The magnesium slag oxides are composed in mass proportions as follows: 40-65 parts of CaO, 60-80 parts of SiO2, 5-8 parts of MgO, 2-5 parts of Fe2O3 and a small amount of other oxides.
[0067] The fly ash mass fraction is composed of: 2.5-10 parts of CaO, 35-55 parts of SiO2, 20-30 parts of Al2O3, 0.5-2 parts of MgO, 0.5-1 parts of SO3, 2-20 parts of Fe2O3 and a small amount of other oxides.
[0068] The mass percentage of silica fume oxides is as follows: 0.1-0.5 parts of CaO, 90-96 parts of SiO2, 0.5-2 parts of Al2O3, 0.5-2 parts of MgO and a small amount of other oxides.
[0069] The mass percentage composition of bagasse ash oxides is: 60-80 parts of SiO2, 10-20 parts of Al2O3, 1-5 parts of CaO, 1-3 parts of MgO, 3-8 parts of Fe2O3, 1-6 parts of K2O, 1-2 parts of Na2O and a small amount of other oxides.
[0070] The mass fraction of sugarcane fiber is as follows: 40-50 parts of cellulose, 20-30 parts of hemicellulose, 1-5 parts of acid-soluble lignin, and 15-25 parts of acid-insoluble lignin.
[0071] The present invention further provides a method for preparing the low shrinkage and high frost resistance shotcrete, comprising the following steps:
[0072] (1) Accurately weigh the following raw materials by weight: 14-20 parts of cement, 6-9 parts of water, 30-40 parts of fine aggregate, 30-40 parts of coarse aggregate, 2-8 parts of solid waste admixture, 1-2 parts of accelerator, and 0.1-0.3 parts of water reducer;
[0073] (2) Using the solid waste admixture provided above;
[0074] (3) Mixing ordinary Portland cement (PO) and solid waste admixture to obtain a cementitious material;
[0075] (4) Add fine aggregate and coarse aggregate to the cementitious material and mix them dry to obtain a dry mix;
[0076] (5) Add water to the dry mix and stir while slowly adding a water reducing agent to obtain concrete;
[0077] (6) Atomized concrete and accelerator are sprayed at the nozzle of the spray mixer to form a material beam to obtain sprayed concrete.
[0078] The spray mixer uses one pipe to pump concrete and another pipe to pump accelerator. The two meet at the nozzle and are mixed by high-pressure air to form an atomized state, which is sprayed out. This is sprayed concrete.
[0079] The shrinkage and frost resistance properties of the low shrinkage and high frost resistance shotcrete of the present invention are explained below in combination with specific embodiments and comparative examples.
[0080] Shotcrete shrinkage test and frost resistance test:
[0081] like Figure 1 As shown in FIG. 1 , magnesium slag, fly ash, silica fume and bagasse ash are ground separately using a ball mill. The mixed material is sprayed into shape using a wet spraying trolley as shown in FIG. Figure 2 As shown. Figure 3 As shown in the figure, after the test block is cured for 1 day, it is cut into 100mm×100mm×400mm test blocks using a cutting machine. Figure 4As shown in the figure, two copper probes are pre-installed and fixed at the center of both sides of the mold. The probes are placed inside the mold, the center holes are fixed with screws and connected to the sensors through the screws to test the shrinkage deformation of the shotcrete. Figure 5 As shown, the freezing resistance was tested using a rapid freeze-thaw chamber.
[0082] Before the test, magnesium slag, fly ash and bagasse ash were ground to a specific surface area of 400-500 m 2 / kg, silica fume powder is ground to a specific surface area of 2000-3000 m 2 / kg. Tests show that the specific surface area can better improve the reactivity of the material, better fill the tiny pores in the concrete, and improve the density of the concrete, which helps to reduce harmful pores in the concrete, improve its pore structure, and thus improve the performance of the concrete. A larger or smaller specific surface area is not conducive to the purpose of the present invention. If it is further ground to a larger specific surface area, the grinding process will cause a rapid increase in cost, and powders with a larger specific surface area are more likely to agglomerate, which is not conducive to uniform dispersion in the concrete. If the specific surface area is too small, the reactivity of the material is poor, which is not conducive to filling the tiny pores in the concrete.
[0083] Example 1
[0084] Weigh magnesium slag, fly ash, silica ash, bagasse ash and sugarcane fiber according to mass proportions. The specific composition is as follows:
[0085] 30 parts of magnesium slag, 15 parts of fly ash, 15 parts of silica ash, 15 parts of bagasse ash and 10 parts of sugarcane fiber are mixed evenly, and 15 parts of saturated Ca(OH)2 solution are added for pre-wetting, which is recorded as solid waste admixture 1.
[0086] (1) Accurately weigh the following raw materials by weight: 16 parts of cement, 8 parts of water, 35 parts of fine aggregate, 35 parts of coarse aggregate, 2 parts of solid waste admixture 1, 1.8 parts of accelerator, and 0.2 parts of water reducer.
[0087] (2) After mixing cement, solid waste admixture 1, fine aggregate and coarse aggregate, add water and slowly add a water reducing agent to obtain concrete;
[0088] (3) Atomizing concrete and accelerating agent at the nozzle of the spray mixer to form a material beam for spraying, thereby obtaining sprayed concrete 1.
[0089] Example 2
[0090] (1) Accurately weigh the following raw materials by weight: 14 parts of cement, 6 parts of water, 30 parts of fine aggregate, 35 parts of coarse aggregate, 4 parts of solid waste admixture 1, 1.8 parts of accelerator, and 0.2 parts of water reducer.
[0091] (2) After mixing cement, solid waste admixture 1, fine aggregate and coarse aggregate, add water and slowly add a water reducing agent to obtain concrete;
[0092] (3) Atomized concrete and accelerator are sprayed at the nozzle of the spray mixer to form a material beam to obtain sprayed concrete 2.
[0093] Example 3
[0094] (1) Accurately weigh the following raw materials by weight: 20 parts of cement, 9 parts of water, 40 parts of fine aggregate, 40 parts of coarse aggregate, 8 parts of solid waste admixture 1, 2 parts of accelerator, and 0.3 parts of water reducer.
[0095] (2) After mixing cement, solid waste admixture 1, fine aggregate and coarse aggregate, add water and slowly add a water reducing agent to obtain concrete;
[0096] (3) Atomized concrete and accelerator are sprayed at the nozzle of the spray mixer to form a material beam to obtain sprayed concrete 3.
[0097] Comparative Example 1
[0098] (1) Accurately weigh the following raw materials by weight: 20 parts of cement, 8 parts of water, 35 parts of fine aggregate, 35 parts of coarse aggregate, 1.8 parts of accelerator, and 0.2 parts of water reducer.
[0099] (2) After mixing cement, fine aggregate and coarse aggregate, add water and slowly add water reducing agent to obtain concrete;
[0100] (3) Atomizing concrete and accelerating agent at the nozzle of the spray mixer to form a material beam for spraying to obtain sprayed concrete 4.
[0101] Comparative Example 2
[0102] (1) Accurately weigh the following raw materials by weight: 14 parts of cement, 8 parts of water, 35 parts of fine aggregate, 35 parts of coarse aggregate, 10 parts of solid waste admixture 1, 1.8 parts of accelerator, and 0.2 parts of water reducer.
[0103] (2) After mixing cement, solid waste admixture 1, fine aggregate and coarse aggregate, add water and slowly add a water reducing agent to obtain concrete;
[0104] (3) Atomizing concrete and accelerating agent at the nozzle of the spray mixer to form a material beam for spraying to obtain sprayed concrete 5.
[0105] Comparative Example 3
[0106] Weigh magnesium slag, fly ash, silica ash, bagasse ash and sugarcane fiber according to mass components. The specific composition is as follows:
[0107] 20 parts of magnesium slag: 18 parts of fly ash: 15 parts of silica ash: 20 parts of bagasse ash: 15 parts of sugarcane fiber are mixed evenly, and 10 parts of saturated Ca(OH)2 solution are added for pre-wetting, and recorded as solid waste admixture 2.
[0108] (1) Accurately weigh the following raw materials by weight: 16 parts of cement, 8 parts of water, 35 parts of fine aggregate, 35 parts of coarse aggregate, 4 parts of solid waste admixture 2, 1.8 parts of accelerator, and 0.2 parts of water reducer.
[0109] (2) After mixing cement, solid waste admixture 2, fine aggregate and coarse aggregate, add water and slowly add water reducing agent to obtain concrete;
[0110] (3) Atomizing concrete and accelerating agent at the nozzle of the spray mixer to form a material beam for spraying to obtain sprayed concrete 6.
[0111] Comparative Example 4
[0112] Weigh magnesium slag, fly ash, silica ash, bagasse ash and sugarcane fiber according to mass components. The specific composition is as follows:
[0113] 45 parts of magnesium slag, 15 parts of fly ash, 10 parts of silica ash, 16 parts of bagasse ash and 16 parts of sugarcane fiber are mixed evenly, and 20 parts of saturated Ca(OH)2 solution are added for pre-wetting, which is recorded as solid waste admixture 3.
[0114] (1) Accurately weigh the following raw materials by weight: 16 parts of cement, 8 parts of water, 35 parts of fine aggregate, 35 parts of coarse aggregate, 4 parts of solid waste admixture 3, 1.8 parts of accelerator, and 0.2 parts of water reducer.
[0115] (2) After mixing cement, solid waste admixture 3, fine aggregate and coarse aggregate, add water and slowly add water reducing agent to obtain concrete;
[0116] (3) Atomizing concrete and accelerating agent at the nozzle of the spray mixer to form a material beam for spraying to obtain sprayed concrete 7.
[0117] Comparative Example 5
[0118] Weigh magnesium slag, fly ash, silica ash, bagasse ash and sugarcane fiber according to mass components. The specific composition is as follows:
[0119] 35 parts of magnesium slag: 10 parts of fly ash: 12 parts of silica ash: 10 parts of bagasse ash: 10 parts of sugarcane fiber are mixed evenly, and 10 parts of saturated Ca(OH)2 solution are added for pre-wetting, which is recorded as solid waste admixture 4.
[0120] (1) Accurately weigh the following raw materials by weight: 16 parts of cement, 8 parts of water, 35 parts of fine aggregate, 35 parts of coarse aggregate, 4 parts of solid waste admixture, 1.8 parts of accelerator, and 0.2 parts of water reducer.
[0121] (2) After mixing cement, solid waste admixture 4, fine aggregate and coarse aggregate, add water and slowly add water reducing agent to obtain concrete;
[0122] (3) Atomizing concrete and accelerating agent at the nozzle of the spray mixer to form a material beam for spraying to obtain sprayed concrete 8.
[0123] Comparative Example 6
[0124] Weigh magnesium slag, fly ash, silica ash, bagasse ash and sugarcane fiber according to mass components. The specific composition is as follows:
[0125] 35 parts of magnesium slag: 25 parts of fly ash: 10 parts of silica ash: 10 parts of bagasse ash: 10 parts of sugarcane fiber are mixed evenly, and 10 parts of saturated Ca(OH)2 solution are added for pre-wetting, and recorded as solid waste admixture 5.
[0126] (1) Accurately weigh the following raw materials by weight: 16 parts of cement, 8 parts of water, 35 parts of fine aggregate, 35 parts of coarse aggregate, 4 parts of solid waste admixture 5, 1.8 parts of accelerator, and 0.2 parts of water reducer.
[0127] (2) After mixing cement, solid waste admixture 5, fine aggregate and coarse aggregate, add water and slowly add water reducing agent to obtain concrete;
[0128] (3) Atomizing concrete and accelerating agent at the nozzle of the spray mixer to form a material beam for spraying to obtain sprayed concrete 9.
[0129] Comparative Example 7
[0130] Weigh magnesium slag, fly ash, silica ash, bagasse ash and sugarcane fiber according to mass components. The specific composition is as follows:
[0131] 35 parts of magnesium slag: 15 parts of fly ash: 5 parts of silica ash: 15 parts of bagasse ash: 15 parts of sugarcane fiber are mixed evenly, and 15 parts of saturated Ca(OH)2 solution are added for pre-wetting, which is recorded as solid waste admixture 6.
[0132] (1) Accurately weigh the following raw materials by weight: 16 parts of cement, 8 parts of water, 35 parts of fine aggregate, 35 parts of coarse aggregate, 4 parts of solid waste admixture 6, 1.8 parts of accelerator, and 0.2 parts of water reducer.
[0133] (2) After mixing cement, solid waste admixture 6, fine aggregate and coarse aggregate, add water and slowly add water reducing agent to obtain concrete;
[0134] (3) Atomizing concrete and accelerating agent at the nozzle of the spray mixer to form a material beam for spraying to obtain sprayed concrete 10.
[0135] Comparative Example 8
[0136] Weigh magnesium slag, fly ash, silica ash, bagasse ash and sugarcane fiber according to mass components. The specific composition is as follows:
[0137] 35 parts of magnesium slag, 15 parts of fly ash, 20 parts of silica ash, 10 parts of bagasse ash and 10 parts of sugarcane fiber are mixed evenly, and 10 parts of saturated Ca(OH)2 solution are added for pre-wetting, which is recorded as solid waste admixture 7.
[0138] (1) Accurately weigh the following raw materials by weight: 16 parts of cement, 8 parts of water, 35 parts of fine aggregate, 35 parts of coarse aggregate, 4 parts of solid waste admixture 7, 1.8 parts of accelerator, and 0.2 parts of water reducer.
[0139] (2) After mixing cement, solid waste admixture 7, fine aggregate and coarse aggregate, add water and slowly add water reducing agent to obtain concrete;
[0140] (3) Atomizing concrete and accelerating agent at the nozzle of the spray mixer to form a material beam for spraying to obtain sprayed concrete 11.
[0141] Comparative Example 9
[0142] Weigh magnesium slag, fly ash, silica ash, bagasse ash and sugarcane fiber according to mass components. The specific composition is as follows:
[0143] 40 parts of magnesium slag, 15 parts of fly ash, 10 parts of silica ash, 5 parts of bagasse ash and 20 parts of sugarcane fiber are mixed evenly, and 10 parts of saturated Ca(OH)2 solution are added for pre-wetting, which is recorded as solid waste admixture 8.
[0144] (1) Accurately weigh the following raw materials by weight: 16 parts of cement, 8 parts of water, 35 parts of fine aggregate, 35 parts of coarse aggregate, 4 parts of solid waste admixture 8, 1.8 parts of accelerator, and 0.2 parts of water reducer.
[0145] (2) After mixing cement, solid waste admixture 8, fine aggregate and coarse aggregate, add water and slowly add water reducing agent to obtain concrete;
[0146] (3) Atomizing concrete and accelerating agent at the nozzle of the spray mixer to form a material beam for spraying to obtain sprayed concrete 12.
[0147] Comparative Example 10
[0148] Weigh magnesium slag, fly ash, silica ash, bagasse ash and sugarcane fiber according to mass components. The specific composition is as follows:
[0149] 30 parts of magnesium slag, 15 parts of fly ash, 10 parts of silica ash, 25 parts of bagasse ash and 10 parts of sugarcane fiber are mixed evenly, and 10 parts of saturated Ca(OH)2 solution are added for pre-wetting, which is recorded as solid waste admixture 9.
[0150] (1) Accurately weigh the following raw materials by weight: 16 parts of cement, 8 parts of water, 35 parts of fine aggregate, 35 parts of coarse aggregate, 4 parts of solid waste admixture 9, 1.8 parts of accelerator, and 0.2 parts of water reducer.
[0151] (2) After mixing cement, solid waste admixture 9, fine aggregate and coarse aggregate, add water and slowly add water reducing agent to obtain concrete;
[0152] (3) Atomizing concrete and accelerating agent at the nozzle of the spray mixer to form a material beam for spraying to obtain sprayed concrete 13.
[0153] Comparative Example 11
[0154] Weigh magnesium slag, fly ash, silica ash, bagasse ash and sugarcane fiber according to mass components. The specific composition is as follows:
[0155] 30 parts of magnesium slag, 15 parts of fly ash, 15 parts of silica ash, 20 parts of bagasse ash and 5 parts of sugarcane fiber are mixed evenly, and 15 parts of saturated Ca(OH)2 solution are added for pre-wetting, and recorded as solid waste admixture 10.
[0156] (1) Accurately weigh the following raw materials in parts by weight: 16 parts of cement, 8 parts of water, 35 parts of fine aggregate, 35 parts of coarse aggregate, 6 parts of solid waste admixture 10, 1.8 parts of accelerator, and 0.2 parts of water reducer.
[0157] (2) After mixing cement, solid waste admixture 10, fine aggregate and coarse aggregate, add water and slowly add a water reducing agent to obtain concrete;
[0158] (3) Atomizing concrete and accelerating agent at the nozzle of the spray mixer to form a material beam for spraying to obtain sprayed concrete 14.
[0159] Comparative Example 12
[0160] Weigh magnesium slag, fly ash, silica ash, bagasse ash and sugarcane fiber according to mass components. The specific composition is as follows:
[0161] 30 parts of magnesium slag, 15 parts of fly ash, 10 parts of silica ash, 10 parts of bagasse ash and 25 parts of sugarcane fiber are mixed evenly, and 10 parts of saturated Ca(OH)2 solution are added for pre-wetting, which is recorded as solid waste admixture 11.
[0162] (1) Accurately weigh the following raw materials in parts by weight: 16 parts of cement, 8 parts of water, 35 parts of fine aggregate, 35 parts of coarse aggregate, 6 parts of solid waste admixture 11, 1.8 parts of accelerator, and 0.2 parts of water reducer.
[0163] (2) After mixing cement, solid waste admixture 11, fine aggregate and coarse aggregate, add water and slowly add a water reducing agent to obtain concrete;
[0164] (3) Atomizing concrete and accelerating agent at the nozzle of the spray mixer to form a material beam for spraying to obtain sprayed concrete 15.
[0165] Comparative Example 13
[0166] Weigh magnesium slag, fly ash, silica ash, bagasse ash and sugarcane fiber according to mass components. The specific composition is as follows:
[0167] 30 parts of magnesium slag, 15 parts of fly ash, 15 parts of silica ash, 15 parts of bagasse ash and 20 parts of sugarcane fiber are mixed evenly, and 5 parts of saturated Ca(OH)2 solution are added for pre-wetting, which is recorded as solid waste admixture 12.
[0168] (1) Accurately weigh the following raw materials in parts by weight: 16 parts of cement, 8 parts of water, 35 parts of fine aggregate, 35 parts of coarse aggregate, 8 parts of solid waste admixture 12, 1.8 parts of accelerator, and 0.2 parts of water reducer.
[0169] (2) After mixing cement, solid waste admixture 12, fine aggregate and coarse aggregate, add water and slowly add a water reducing agent to obtain concrete;
[0170] (3) Atomizing concrete and accelerating agent at the nozzle of the spray mixer to form a material beam for spraying to obtain sprayed concrete 16.
[0171] Comparative Example 14
[0172] Weigh magnesium slag, fly ash, silica ash, bagasse ash and sugarcane fiber according to mass components. The specific composition is as follows:
[0173] 30 parts of magnesium slag, 15 parts of fly ash, 10 parts of silica ash, 10 parts of bagasse ash and 10 parts of sugarcane fiber are mixed evenly, and 25 parts of saturated Ca(OH)2 solution are added for pre-wetting, which is recorded as solid waste admixture 13.
[0174] (1) Accurately weigh the following raw materials in parts by weight: 16 parts of cement, 8 parts of water, 35 parts of fine aggregate, 35 parts of coarse aggregate, 8 parts of solid waste admixture 13, 1.8 parts of accelerator, and 0.2 parts of water reducer.
[0175] (2) After mixing cement, solid waste admixture 13, fine aggregate and coarse aggregate, add water and slowly add a water reducing agent to obtain concrete;
[0176] (3) Atomizing concrete and accelerating agent at the nozzle of the spray mixer to form a material beam for spraying to obtain sprayed concrete 17.
[0177] The statistical results of the comparative test are shown in Table 1.
[0178] Table 1 Statistics of 28-day shrinkage and frost resistance of shotcrete
[0179]
[0180] Comparing Examples 1, 2, 3 and Control Example 1, it can be seen that the use of solid waste admixtures significantly reduces the shrinkage deformation of shotcrete. Comparing Examples 1, 2, 3 and Control Example 2, it can be seen that when the amount of solid waste admixtures is too high, the reduction of cement limits the supply of sufficient Ca²⁺ and OH⁻ ions, which are the key to the effective participation of admixtures in hydration reactions. Therefore, the reduction in the overall degree of hydration reduces the generation of beneficial hydration products, especially those that contribute positively to frost resistance, thereby weakening the concrete's ability to resist freeze-thaw cycles.
[0181] By comparing Examples 1, 2, 3 and Control Examples 3, 4, it can be seen that there is an optimal dosage of magnesium slag in solid waste admixtures. When the dosage of magnesium slag is low, the shrinkage compensated by the hydration of MgO and Mg3N2 in the magnesium slag to generate Mg(OH)2 with micro-expansion properties is small; when the dosage is high, it has a negative impact on the frost resistance of shotcrete.
[0182] By comparing Examples 1, 2, 3 and Control Examples 5, 6, it can be seen that when the fly ash content is low, the ball lubrication effect of the fly ash is insufficient, and the shotcrete is not easy to compact, resulting in large shrinkage and poor frost resistance; when the fly ash content is too large, the powder grading is poor, and the concrete cannot be compacted, resulting in large shrinkage and poor frost resistance.
[0183] By comparing Examples 1, 2, 3 and Control Examples 7, 8, it can be seen that when the silica fume content is low, the smaller silica fume particles cannot fully fill the pores generated during the hydration process, resulting in slightly poor frost resistance; when the silica fume content is high, the high reactivity of the silica fume leads to an increase in the shrinkage value.
[0184] By comparing Examples 1, 2, 3 and Comparative Examples 9 and 10, it can be seen that when the amount of bagasse ash added is low, the frost resistance of the shotcrete is poor; when the amount of bagasse ash added is high, the frost resistance of the shotcrete is also poor, but the shrinkage deformation increases. This is because bagasse ash has good water absorption and "water storage" capabilities, and continuously hydrates during the hydration process, improves the density of the shotcrete, optimizes the pore structure of the shotcrete, and thus improves the frost resistance.
[0185] By comparing Examples 1, 2, 3 and Comparative Examples 11 and 12, it can be seen that adding sugarcane fiber can reduce the shrinkage deformation of shotcrete and improve the frost resistance of shotcrete. However, the dosage should not be too high. A high dosage of fiber will make the workability of shotcrete worse, thereby increasing the porosity and reducing the frost resistance. When the fiber dosage is low, the bridging effect of the fiber is limited, the degree of microcrack expansion in the concrete can be reduced to a low level, and the effect of improving the frost resistance is relatively limited.
[0186] By comparing Examples 1, 2, 3 and Comparative Examples 13 and 14, it can be seen that the solid waste admixtures after Ca(OH)2 pre-reaction and pre-water absorption have more obvious effects on shrinkage deformation and frost resistance, but the content should not be too high. Too high a Ca(OH)2 solution will increase the water-cement ratio, thereby increasing the shrinkage of the shotcrete and reducing the frost resistance. Too low a Ca(OH)2 solution usage will make the internal curing effect of the solid waste admixture unclear, and the activation effect on the solid waste admixture is insufficient, resulting in poor improvement of the shrinkage deformation and frost resistance of the shotcrete.
[0187] The above comparison results are further Figure 6 It can be seen more clearly and intuitively. Figure 6 The above shotcrete shrinkage and frost resistance comparison diagram is shown. It is obvious from the figure that the low shrinkage and high frost resistance shotcrete provided by the present invention has both low shrinkage and high frost resistance. Although the existing conventional concrete can basically achieve similar effects in terms of shrinkage or frost resistance alone, it cannot achieve the technical effects of low shrinkage and high frost resistance at the same time, which leads to the fact that it cannot meet the performance requirements of shotcrete for low shrinkage and high frost resistance, and cannot be applied to low-temperature freeze-thaw cycle support projects.
[0188] The low shrinkage and high frost resistance shotcrete provided by the present invention can be widely used in low-temperature freeze-thaw cycle support projects, such as support for plateau tunnel portals, water diversion tunnels in cold-region tunnels, and slopes in cold regions. The shrinkage rate of the shotcrete formed can be reduced to below 365 με, and the frost resistance can reach F250 or even F300.
[0189] In summary, the present invention synergistically utilizes the volcanic ash activity of magnesium slag, fly ash, silica ash, and bagasse ash, the ball lubrication and filling effects of fly ash and silica ash, the toughening effect of bagasse ash and sugarcane fiber, and the effects of curing and activity stimulation of the admixtures soaked in Ca(OH)2 solution, and proposes a shotcrete with low shrinkage and high frost resistance and a preparation method thereof. This method not only effectively promotes the resource utilization and high-value utilization of solid waste, but also significantly reduces the volume shrinkage phenomenon of shotcrete during the curing process, and greatly enhances its ability to resist low-temperature freeze-thaw cycle damage. Therefore, the technology and products can be widely used in various engineering constructions that require strict shrinkage control and high frost resistance of shotcrete materials, especially low-temperature freeze-thaw cycle shotcrete support projects.
[0190] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.
[0191] Although several specific implementation details are included in the above discussion, these should not be construed as limiting the scope of the present invention. Certain features described in the context of separate embodiments may also be implemented in a single implementation in combination. On the contrary, the various features described in the context of a single implementation may also be implemented in multiple implementations individually or in any suitable sub-combination.
Claims
1. A low shrinkage, high frost resistance shotcrete, It is characterized in that Includes by weight: 12-18 parts of cement, 6-9 parts of water, 30-40 parts of fine aggregate, 30-40 parts of coarse aggregate, 2-8 parts of solid waste admixture, 1-2 parts of accelerator, 0.1-0.3 parts of water reducer; and The solid waste admixture comprises, by weight: 30-40 parts of magnesium slag, 15-20 parts of fly ash, 10-15 parts of silica ash, 10-20 parts of bagasse ash and 10-20 parts of sugarcane fiber.
2. The low shrinkage, high frost resistance shotcrete according to claim 1, It is characterized in that The solid waste admixture comprises, by weight: 35 parts of magnesium slag, 15 parts of fly ash, 15 parts of silica ash, 15 parts of bagasse ash and 15 parts of sugarcane fiber.
3. The low shrinkage, high frost resistance shotcrete according to claim 1, It is characterized in that The solid waste admixture comprises, by weight: 30 parts of magnesium slag, 15 parts of fly ash, 10 parts of silica ash, 10 parts of bagasse ash and 10 parts of sugarcane fiber.
4. The low shrinkage, high frost resistance shotcrete according to claim 1, It is characterized in that The solid waste admixture comprises, by weight, 40 parts of magnesium slag, 20 parts of fly ash, 15 parts of silica ash, 20 parts of bagasse ash and 20 parts of sugarcane fiber.
5. The low shrinkage, high frost resistance shotcrete according to any one of claims 1 to 4, It is characterized in that The solid waste admixture is prepared according to the following process: Weigh 30-40 parts of magnesium slag, 15-20 parts of fly ash, 10-15 parts of silica ash, 10-20 parts of bagasse ash and 10-20 parts of sugarcane fiber by weight; Magnesium slag, fly ash and bagasse ash were ground to a specific surface area of 400-500 m 2 / kg, grind the silica fume to a specific surface area of 2000-3000 m 2 / kg; The ground magnesium slag, fly ash and bagasse ash are added with the ground silica ash and sugarcane fiber and mixed evenly; After mixing, add 10-20 parts of saturated Ca(OH) 2 The solution is pre-absorbed with water and activated.
6. The low shrinkage, high frost resistance shotcrete according to claim 1, It is characterized in that The cement is ordinary Portland cement or sulfate-resistant cement; and / or The fine aggregate is natural sand or machine-made sand with a fineness modulus of 2.6; and / or The coarse aggregate is crushed stone or ceramsite with a continuous gradation of 5-10 mm; and / or The accelerating setting agent is an aluminum sulfate type alkali-free accelerating setting agent or a hydrofluoric acid type alkali-free accelerating setting agent; and / or The water reducing agent is a polycarboxylate water reducing agent.
7. The low shrinkage, high frost resistance shotcrete according to claim 1, It is characterized in that The magnesium slag comprises by weight: 40-65 parts of CaO, 60-80 parts of SiO 2 , 5-8 parts MgO, 2-5 parts Fe 2 O 3 ; and / or The fly ash mass fraction composition includes: 2.5-10 parts of CaO, 35-55 parts of SiO 2 , 20-30 parts Al 2 O 3 、0.5-2 parts MgO、0.5-1 parts SO 3 , 2-20 parts Fe 2 O 3 ; and / or The silica ash mass fraction comprises: 0.1-0.5 parts CaO, 90-96 parts SiO 2 , 0.5-2 parts Al 2 O 3 , 0.5-2 parts MgO; and / or The bagasse ash mass fraction composition includes: 60-80 parts SiO 2 , 10-20 parts Al 2 O 3 , 1-5 parts CaO, 1-3 parts MgO, 3-8 parts Fe 2 O 3 , 1-6 portions K 2 O, 1-2 parts Na 2 O; and / or The mass proportion of the sugarcane fibers is as follows: 40-50 parts of cellulose, 20-30 parts of hemicellulose, 1-5 parts of acid-soluble lignin, and 15-25 parts of acid-insoluble lignin.
8. The low shrinkage, high frost resistance shotcrete according to claim 1, It is characterized in that The shrinkage rate of the low shrinkage and high frost resistance shotcrete is not higher than 365 με and the frost resistance is not lower than F250.
9. A method for preparing low shrinkage and high frost resistance shotcrete according to any one of claims 1 to 8, It is characterized in that The steps include: Weigh the required raw materials according to the proportion, mix cement, solid waste admixture, fine aggregate and coarse aggregate, add water and slowly add water reducing agent to obtain concrete; Atomized concrete and accelerator are sprayed at the nozzle of the spray mixer to form a beam to obtain sprayed concrete.
10. Use of the low shrinkage, high frost resistance shotcrete according to any one of claims 1 to 8 in low temperature freeze-thaw cycle support engineering.
Citation Information
Patent Citations
Lithium slag composite admixture, preparation method thereof and sprayed concrete
CN117361917A
Low-cost high-strength sprayed concrete and preparation method thereof
CN117534398A
Set accelerator and technique for spraying with the same
SG151600A1
Cited By
Sprayed concrete interface reinforced mortar used under water seepage working condition of tunnel in cold region as well as preparation method and application of sprayed concrete interface reinforced mortar
CN120040152A
A shotcrete interface reinforcement mortar for use in tunnel water seepage conditions in cold regions, and its preparation method and application
CN120040152B