Coal-based solid waste filling paste and preparation method thereof

Through the preparation of coal-based solid waste filling paste, the problem of poor fluidity of mine filling materials is solved by using solid waste materials such as coal gangue, and a paste with high fluidity and strength is achieved, which meets the needs of long-distance transportation and filling in mines. , promoting the sustainable development of the coal industry.

CN118724545APending Publication Date: 2024-10-01FENY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410973117.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The materials used in existing mine filling technology have poor fluidity, resulting in resource waste and environmental damage during the mining process, making it difficult to achieve sustainable development of the coal industry.

Method used

Coal-based solid waste filling paste is used, and the relative proportions of Portland cement and sulfaluminate cement and the coal The proportion of gangue is made into a paste with higher fluidity, which is used to fill the goaf to reduce the risk of blockage and improve transportation efficiency.

Benefits of technology

It achieves high fluidity and strength of coal-based solid waste filling paste, can be self-leveling and transported within 1-2 hours, reduces pumping pressure and the risk of pipe blockage, meets the needs of long-distance transportation underground in mines, and reduces the The heat of hydration prevents thermal cracking of the underground filling body and improves the filling effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724545A_ABST
    Figure CN118724545A_ABST
Patent Text Reader

Abstract

The embodiment of the invention discloses a coal-based solid waste filling paste and a preparation method thereof, relates to the technical field of mine filling mining, and aims to solve the problem that the flowability of materials for filling is generally poor. The coal-based solid waste filling paste comprises the following components in parts by weight: 50-55% of coal gangue, 15-20% of fly ash, 4-8% of desulfurized fly ash, 2-5% of Portland cement, 0.5-2% of sulphoaluminate cement, 5-10% of mineral powder and 14-16% of water. The method is suitable for the application scene of filling during mining.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of mine filling and mining, and in particular to a coal-based solid waste filling paste and a preparation method thereof. Background Art

[0002] Coal is the main energy source in my country, and it accounts for a high proportion in the production and consumption structure of primary energy. With the implementation of the sustainable development strategy around the world, the sustainable development of the coal industry has also been further promoted in the mining industry.

[0003] In order to meet the sustainable development needs of the coal industry, mine filling technology is generally used in the mining process. However, the fluidity of the materials currently used for filling is generally poor. Summary of the invention

[0004] In view of this, an embodiment of the present invention provides a coal-based solid waste filling paste with high fluidity and a preparation method thereof.

[0005] To achieve the above object, the embodiments of the present invention adopt the following technical solutions: In a first aspect, an embodiment of the present invention provides a coal-based solid waste filling paste, comprising the following components in parts by weight: 50-55% coal gangue, 15-20% fly ash, 4-8% desulfurization ash, 2-5% silicate cement, 0.5-2% sulfoaluminum cement, 5-10% mineral powder and 14-16% water.

[0006] According to a specific implementation method of an embodiment of the present invention, the coal-based solid waste filling paste includes the following components in parts by weight: 51-53% coal gangue, 17-19% fly ash, 4-5% desulfurization ash, 2-3% silicate cement, 0.5-1% sulphoaluminum cement, 6-8% mineral powder and 14-16% water.

[0007] According to a specific implementation of an embodiment of the present invention, the coal-based solid waste filling paste further includes 0.5-2% (by weight) of sodium sulfate.

[0008] According to a specific implementation of an embodiment of the present invention, the coal-based solid waste filling paste further includes 0.5-2% (by weight) of a water reducing agent.

[0009] According to a specific implementation method of an embodiment of the present invention, the coal-based solid waste filling paste includes the following components in parts by weight: 52% coal gangue, 18% fly ash, 4.5% desulfurization ash, 2% Portland cement, 0.5% sulfoaluminum cement, 7% mineral powder, 0.5 sodium sulfate, 15% water, and 0.5% water reducer.

[0010] In the second aspect, an embodiment of the present invention provides a method for preparing a coal-based solid waste filling paste, comprising: mixing a curing agent, fly ash, desulfurization ash and a water reducer solution according to a first preset ratio to obtain a slurry base material, wherein the first preset ratio includes the following components in parts by weight: 30.3% curing agent, 54.6% fly ash, 13.6% desulfurization ash, and 1.5% water reducer; stirring the slurry base material to prepare a slurry; adding a preset weight of coal gangue to the slurry and stirring for a preset time to prepare a coal-based solid waste filling paste.

[0011] According to a specific implementation manner of an embodiment of the present invention, before the curing agent, fly ash, desulfurized ash and water reducing agent solution mixed in a first preset ratio are stirred to obtain a slurry base, the method further includes: mixing silicate cement, sulphoaluminate cement, mineral powder and sodium sulfate in a second preset ratio to obtain a curing agent base, wherein the second preset ratio includes the following components in parts by weight: 20% silicate cement, 5% sulphoaluminate cement, 70% mineral powder and 5% sodium sulfate; stirring the curing agent base to determine whether the uniformity of the curing agent base meets the preset curing agent uniformity; if so, completing the preparation of the curing agent; if not, continuing to stir the curing agent base.

[0012] According to a specific implementation method of an embodiment of the present invention, a curing agent, fly ash, desulfurization ash and a water reducing agent solution mixed in a first preset ratio are stirred to obtain a slurry base material; stirring the slurry base material to prepare a slurry specifically includes: using a first feeding device to steadily transfer the fly ash and desulfurization ash in a first storage bin to a first conveying mechanism, and the first conveying mechanism spirally transfers the fly ash and the desulfurization ash to a first feeding mechanism; using a second feeding device to steadily transfer the curing agent in a second storage bin to a second conveying mechanism, and the second conveying mechanism The curing agent spirally transfers the curing agent to the second feeding mechanism; the water reducer and water in a preset ratio are mixed in the water reducer containing tank to prepare a water reducer solution, and a quantitative water pump is connected to the water reducer containing tank, wherein the preset ratio includes the following components in parts by weight: 3.23% water reducer and 96.77% water; the preset weight of fly ash and desulfurization ash transferred by the first feeding mechanism, the preset weight of curing agent transferred by the second feeding mechanism and the preset weight of water reducer solution transferred by the quantitative water pump are stirred in an agitator to prepare a slurry.

[0013] According to a specific implementation method of an embodiment of the present invention, the preset weight of fly ash and desulfurization ash transferred by the first feeding mechanism specifically includes: making the fly ash and the desulfurization ash move along a spiral path in the first feeding mechanism; obtaining the weight of the fly ash and the desulfurization ash through the first feeding mechanism; obtaining the flow rate of the fly ash and the desulfurization ash through the first feeding mechanism; the first feeding mechanism determines whether the weight of the transferred fly ash and desulfurization ash reaches the preset weight based on the obtained weight and flow rate of the fly ash and the desulfurization ash; if so, stopping the transfer; if not, continuing the transfer.

[0014] According to a specific implementation method of an embodiment of the present invention, a preset weight of coal gangue is added to the slurry and stirred for a preset time to prepare a coal-based solid waste filling paste, which specifically includes: feeding the coal gangue blocks to a crusher, and crushing the coal gangue blocks by the crusher; transferring the processed coal gangue blocks to a vibrating screen, and screening the processed coal gangue blocks by the vibrating screen to obtain coal gangue that meets the supply demand; after the slurry is prepared, using a coal gangue feeding mechanism to transfer the coal gangue to the agitator; stirring the slurry and the coal gangue in the agitator to a preset time threshold to prepare a coal-based solid waste filling paste.

[0015] According to a specific implementation method of an embodiment of the present invention, the processed gangue blocks are screened by the vibrating screen to obtain the gangue that meets the supply demand, which specifically includes: judging whether the gangue is less than 16 mm; if so, the processed gangue blocks are used as the gangue that meets the supply demand; if not, they are transferred to the crusher for further crushing.

[0016] According to a specific implementation of an embodiment of the present invention, stirring silicate cement, sulphoaluminate cement, mineral powder and sodium sulfate mixed in a second preset ratio to prepare a curing agent specifically includes: using a third feeding device to steadily transfer silicate cement to a third conveying mechanism, and the third conveying mechanism spirally transfers the silicate cement to a third feeding mechanism; using a fourth feeding device to steadily transfer sulphoaluminate cement to a fourth conveying mechanism, and the fourth conveying mechanism spirally transfers the sulphoaluminate cement to a fourth feeding mechanism; using a fifth feeding device to steadily transfer mineral powder to a fifth conveying mechanism, and the fifth conveying mechanism spirally transfers the mineral powder to a fifth feeding mechanism; using a sixth feeding device to steadily transfer sodium sulfate to a sixth conveying mechanism, and the sixth conveying mechanism spirally transfers the sodium sulfate to a sixth feeding mechanism; mixing and stirring the preset weight of silicate cement transferred by the third feeding mechanism, the preset weight of sulphoaluminate transferred by the fourth feeding mechanism, the preset weight of mineral powder transferred by the fifth feeding mechanism and the preset weight of sodium sulfate transferred by the sixth feeding mechanism in a stirrer to prepare a curing agent.

[0017] According to a specific implementation of the embodiment of the present invention, after preparing the curing agent, the method further includes: storing the curing agent in a second storage bin.

[0018] According to a specific implementation method of an embodiment of the present invention, the weight proportions of the raw materials of the coal-based solid waste filling paste are: 50-55% coal gangue, 15-20% fly ash, 4-8% desulfurization ash, 2-5% silicate cement, 0.5-2% sulfoaluminum cement, 5-10% mineral powder, 0.5-2% sodium sulfate, 14-16% water, and 0.5-2% water reducer.

[0019] The coal-based solid waste filling paste and the preparation method thereof provided in the embodiment of the present invention utilize coal gangue, fly ash, desulfurization ash, Portland cement, sulfoaluminum cement, mineral powder and water to make the coal-based solid waste filling paste. By controlling the relative ratio of Portland cement and sulfoaluminum cement to be close to 4:1, and controlling the ratio of coal gangue to be close to 1 / 2, the prepared coal-based solid waste filling paste has better fluidity. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 The present invention is a schematic flow chart of an embodiment of a method for preparing a coal-based solid waste filling paste.

[0022] Figure 2 The composition table of coal gangue of Shangwan Coal Mine detected by XRF according to one embodiment of the coal-based solid waste filling paste of the present invention; Figure 3 This is a graph showing the mineral composition of coal gangue from Shangwan Coal Mine detected by XRD according to an embodiment of the coal-based solid waste filling paste of the present invention; Figure 4 This is a table of the composition of Jinjie fly ash detected by XRF in one embodiment of the coal-based solid waste filling paste of the present invention; Figure 5 This is a table of the composition of Handan desulfurization ash detected by XRF according to an embodiment of the coal-based solid waste filling paste of the present invention; Figure 6 This is a table of mineral powder components detected by XRF of an embodiment of the coal-based solid waste filling paste of the present invention; Figure 7 This is a diagram showing the stirring effect of the coal-based solid waste filling paste of the present invention; Figure 8 This is a diagram showing the filling effect of the coal-based solid waste filling paste of the present invention. DETAILED DESCRIPTION

[0023] The embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0024] It should be clear that the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The rational development of coal resources is no longer limited to fully recovering the resources that can be used under contemporary technical conditions, but should also take into full consideration the rational protection of prospective resources. Under existing technical conditions, prospective resources cannot be used or their future development and utilization value cannot be recognized at all. Prospective resources are often greatly damaged, making it difficult to develop them again, or even if they are developed, they will increase the technical difficulty. The current mining technology causes a large amount of coal resources to be lost and wasted in the mining and selection process, which will further aggravate the shortage of resources in the long run. Backfilling can effectively inhibit the destruction of surrounding rocks, create a good mining environment and technical conditions for the future development of prospective resources, and can also preserve the useful minerals currently used as waste materials for a long time through backfilling until they can be used again. Therefore, it can be said that coal mine backfilling is an effective technical approach to protect prospective resources and build industrial ecological coal mines.

[0026] In order to ensure the sustainable development of the coal industry, it is urgent to liberate the problem of "three-under" compressed coal, so it is imperative to study the mining technology of "three-under" compressed coal. Filling mining meets the needs of mining without relocating buildings such as villages, and solves the mining problem of "three-under" compressed coal. Filling mining can effectively control surface mining subsidence, protect the ecological environment of the mining area, protect groundwater resources from damage, increase the recovery rate of coal resources, improve mine safety production conditions, realize coal mining without relocation, and liberate coal resources under village buildings, under railways, and above and below water bodies.

[0027] In backfill mining, coal-based solid waste backfill paste is generally filled into the goaf to limit rock movement and surface subsidence. An embodiment of the present invention provides a coal-based solid waste backfill paste with high fluidity, comprising the following components by weight: 50-55% coal gangue, 15-20% fly ash, 4-8% desulfurized ash, 2-5% silicate cement, 0.5-2% sulfoaluminum cement, 5-10% mineral powder and 14-16% water.

[0028] In the implementation manner of the present application, coal gangue is used as coarse aggregate, and fly ash and desulfurization ash are used as fine aggregate, so that coal-based solid waste can be fully utilized.

[0029] The coal-based solid waste filling paste provided in the embodiment of the present invention is made of coal gangue, fly ash, desulfurization ash, Portland cement, sulfoaluminum cement, mineral powder and water. The relative ratio of Portland cement and sulfoaluminum cement is controlled to be close to 4:1, and the ratio of coal gangue is controlled to be close to 1 / 2, so that the prepared coal-based solid waste filling paste has good fluidity.

[0030] In one embodiment, the coal-based solid waste filling paste includes the following components in parts by weight: 51-53% coal gangue, 17-19% fly ash, 4-5% desulfurized ash, 2-3% silicate cement, 0.5-1% sulfoaluminum cement, 6-8% mineral powder and 14-16% water.

[0031] The coal-based solid waste filling paste provided in this embodiment can be transported to the mine and can self-level. Its slump is not less than 270mm; the fluidity time is not less than 1h, and there will be no blockage in the pipeline with a length of more than 3km. Due to the long distance of underground pipeline transportation in mines, the coal-based solid waste filling paste needs to have high fluidity, a slump of not less than 260mm, and an expansion of not less than 500mm. While ensuring strength, it can effectively control pipeline resistance, reduce pumping pressure, and reduce the risk of pipe blockage.

[0032] In one embodiment, the coal-based solid waste filling paste further comprises 0.5-2% (by weight) of sodium sulfate.

[0033] Mineral powder and fly ash can produce gelling properties under the stimulation of sodium sulfate, thereby reducing the amount of cement used and lowering costs; at the same time, the large-scale use of mineral powder instead of cement can reduce the hydration heat of the filling paste, thereby effectively preventing the heating and cracking of the underground filling body.

[0034] In one embodiment, the coal-based solid waste filling paste further comprises 0.5-2% (by weight) of a water reducing agent.

[0035] In this embodiment, by introducing a water reducing agent, the amount of water used can be reduced, the water-binder ratio can be reduced, and the overall strength can be improved, so that the coal-based solid waste filling paste has better workability and workability.

[0036] In one embodiment, the coal-based solid waste filling paste includes the following components in parts by weight: 52% coal gangue, 18% fly ash, 4.5% desulfurization ash, 2% silicate cement, 0.5% sulfoaluminum cement, 7% mineral powder, 0.5% sodium sulfate, 15% water, and 0.5% water reducer.

[0037] In this embodiment, by optimizing the usage ratio of silicate cement and sulphoaluminum cement to 4:1, the coal-based solid waste filling paste can have a strength of not less than 0.5Mpa after 4-8 hours of production, and a fluidity of not less than 270mm within 1-2 hours of production.

[0038] The coal-based solid waste filling paste and the preparation method thereof provided in the embodiments of the present invention utilize coal gangue, fly ash, desulfurization ash, silicate cement, sulfoaluminum cement, mineral powder, sodium sulfate, water and water reducing agent to prepare the coal-based solid waste filling paste. By controlling the relative ratio of silicate cement and sulfoaluminum cement to be close to 4:1 and the ratio of coal gangue to be close to 1 / 2, the prepared coal-based solid waste filling paste has better fluidity.

[0039] In one embodiment, by controlling the relative ratio of silicate cement and sulphoaluminum cement to be close to 4:1, and making the overall proportion of silicate cement in the coal-based solid waste filling paste to be 2%, and the overall proportion of sulphoaluminum cement in the coal-based solid waste filling paste to be 0.5%, the prepared coal-based solid waste filling paste can have a preset curing strength within 4-8 hours and have good fluidity within 1-2 hours.

[0040] The embodiment of the present invention provides a method for preparing a coal-based solid waste filling paste with high fluidity, as follows: Figure 1 , the embodiments of the present invention are further described.

[0041] Figure 1 This is a schematic diagram of a method for preparing a coal-based solid waste filling paste according to an embodiment of the present invention. Figure 1 As shown, the method of this embodiment includes: S110, mixing a curing agent, fly ash, desulfurized ash and a water reducing agent solution according to a first preset ratio to obtain a slurry base material, wherein the first preset ratio includes the following components in parts by weight: 30.3% curing agent, 54.6% fly ash, 13.6% desulfurized ash and 1.5% water reducing agent. The curing agent can improve the curing speed, strength and durability of the filling material.

[0042] S120, stirring the slurry base material to prepare slurry.

[0043] S130, adding a preset weight of coal gangue to the slurry and stirring for a preset time to prepare a coal-based solid waste filling paste, and transporting the coal-based solid waste filling paste to a target area through a pipeline.

[0044] The stirring time after adding the gangue to the slurry may be 1.5-2.5 minutes. In one embodiment, the stirring time after adding the gangue to the slurry is 1.5 minutes. In another embodiment, the stirring time after adding the gangue to the slurry is 2 minutes. In another embodiment, the stirring time after adding the gangue to the slurry is 2.5 minutes.

[0045] The weight of the coal-based solid waste filling paste can be 1.8 tons, of which the weight of the added coal gangue can be 0.94 tons.

[0046] A filling pump may be provided at the feed end of the pipeline, and the coal-based solid waste filling paste may be transported to the target area through the pipeline by the filling pump.

[0047] The method for preparing a coal-based solid waste filling paste provided in an embodiment of the present invention comprises stirring a curing agent, fly ash, desulfurization ash and a water reducing agent solution mixed in a first preset ratio to prepare a slurry, which can fix the coal-based solid waste filling paste within a preset time. A preset weight of coal gangue is added to the slurry and stirred for a preset time to prepare a coal-based solid waste filling paste, so as to transport the coal-based solid waste filling paste to a target area through a pipeline. By controlling the weight of the coal gangue, the prepared coal-based solid waste filling paste can have good fluidity.

[0048] In one embodiment, the stirring of the slurry base to prepare the slurry comprises: Determine whether the uniformity of the slurry base material meets the preset slurry uniformity; if so, complete the preparation of the slurry; if not, continue to stir the slurry base material.

[0049] The preset slurry uniformity may be the uniformity of a sample precisely stirred manually.

[0050] In one embodiment, after the slurry base material is subjected to multiple semi-industrial stirring, samples are taken for mortar testing, and the strength of the slurry base material after the mortar test is compared with the strength of the sample precisely stirred manually. If the difference in strength between the two is within a preset threshold range, it is determined that the preparation of the slurry has been completed.

[0051] In one embodiment, before the curing agent, fly ash, desulfurized ash and water reducing agent solution mixed in a first preset ratio are stirred to prepare the slurry, the method further includes: mixing silicate cement, sulphoaluminate cement, mineral powder and sodium sulfate in a second preset ratio to obtain a curing agent base material, wherein the second preset ratio includes the following components in parts by weight: 20% silicate cement, 5% sulphoaluminate cement, 70% mineral powder and 5% sodium sulfate; stirring the curing agent base material to determine whether the uniformity of the curing agent base material meets the preset curing agent uniformity; if so, completing the preparation of the curing agent; if not, continuing to stir the curing agent base material.

[0052] The water reducing agent solution can be prepared by mixing a preset weight of water reducing agent powder or water reducing agent mother solution with a preset weight of water.

[0053] Fly ash can produce gelling properties under the action of curing agent, reduce the amount of silicate cement and sulphoaluminate cement in the raw materials for preparing curing agent, and reduce the production cost of coal-based solid waste filling paste.

[0054] Specifically, fly ash can produce gelling properties under the stimulation of sodium sulfate in the curing agent.

[0055] In addition, the mineral powder in the curing agent can also produce gelling properties under the stimulation of sodium sulfate, reducing the amount of acid salt cement and sulfoaluminate cement. In other words, the coal-based solid waste filling paste in this embodiment uses a large amount of mineral powder to replace cement. The hydration heat phenomenon of the coal-based solid waste filling paste is mainly caused by cement. Therefore, it can effectively solve the problem of heating and cracking of the coal-based solid waste filling paste in mines.

[0056] The water reducing agent solution in the curing agent can reduce the amount of water used and the water-binder ratio, thereby increasing the strength of the coal-based solid waste filling paste after curing, and making the coal-based solid waste filling paste have better workability or workability.

[0057] The coal gangue in the coal-based solid waste filling paste prepared by using the curing agent prepared in this embodiment is a coarse aggregate, and the fly ash and desulfurization ash are fine aggregates.

[0058] Adjust the parameter ratios of each material in the formula and optimize the formula ratio to ensure that the coal-based solid waste filling paste has fluidity within 2 hours and can stand on its own after 8 hours; the addition ratio of sulphoaluminate cement and sodium sulfate is particularly important, as the above two factors affect the setting time and early strength of the coal-based solid waste filling paste. For example, under the same working conditions, the weight of the mineral powder in the formula is fixed, and the amount of sulphoaluminate cement and silicate cement is controlled, and the experimental results are shown in the following table:

[0059] Based on the change in compressive strength, sulfate was added to optimize the ratio, and the experimental results are shown in the following table:

[0060] Based on the change in compressive strength, the ratio was further optimized and the experimental results were shown in the following table:

[0061] Based on the change in compressive strength, the influence of water reducer (influence of concentration) was optimized, and the experimental results were shown in the following table:

[0062] The proportions of the raw materials for obtaining the final coal-based solid waste filling paste are shown in the following table:

[0063] The stirring effect of coal-based solid waste filling paste is as follows Figure 7 As shown in Figure 2, the filling effect of coal-based solid waste filling paste is as follows: Figure 8 shown.

[0064] Among them, the specific implementation principle of judging whether the uniformity of the curing agent base material meets the preset curing agent uniformity is similar to the implementation principle of judging whether the uniformity of the slurry base material meets the preset slurry uniformity, which will not be repeated here.

[0065] In one embodiment, a curing agent, fly ash, desulfurized ash and a water reducing agent solution mixed in a first preset ratio are stirred to prepare a slurry, specifically comprising: using a first feeding device to steadily transfer the fly ash and desulfurized ash in a first storage bin to a first conveying mechanism, and the first conveying mechanism spirally transfers the fly ash and the desulfurized ash to a first feeding mechanism; using a second feeding device to steadily transfer the curing agent in a second storage bin to a second conveying mechanism, and the second conveying mechanism spirally transfers the curing agent to a second feeding mechanism; mixing a preset ratio of water reducing agent and water in a water reducing agent containing tank to prepare a water reducing agent solution, and connecting a quantitative water pump to the water reducing agent containing tank, wherein the preset ratio includes the following components in parts by weight: 3.23% water reducing agent and 96.77% water; stirring the preset weight of fly ash and desulfurized ash transferred by the first feeding mechanism, the preset weight of curing agent transferred by the second feeding mechanism and the preset weight of water reducing agent solution transferred by the quantitative water pump in a stirrer to prepare a slurry.

[0066] By delivering the curing agent, fly ash and desulfurization ash in a steady flow through each feeding device, each raw material can be evenly delivered to the agitator, thereby evenly mixing the raw materials and making the performance of the coal-based solid waste filling paste prepared based on the prepared slurry uniform.

[0067] In addition, the raw materials for preparing coal-based solid waste filling paste usually contain a large amount of dust. The solidifying agent, fly ash and desulfurization ash are delivered in a steady flow through various feeding devices, which can effectively prevent dust from flying and reduce pollution.

[0068] Each raw material is spirally delivered by each conveying mechanism, and each raw material can be mixed continuously and evenly to prevent the raw material from being stratified, thereby improving the uniformity of the raw material.

[0069] Among them, each feeding device can use a steady-flow feeding device, each conveying mechanism can use a screw conveyor, each feeding mechanism can use a screw scale, and the agitator can use a double-horizontal-shaft forced continuous mixer. The water-reducing agent storage tank can be directly connected to the water storage tank.

[0070] In one embodiment, two twin-shaft forced continuous mixers form a secondary mixer.

[0071] In one embodiment, the preset weight of fly ash and desulfurization ash transferred by the first feeding mechanism specifically includes: making the fly ash and the desulfurization ash move along a spiral path in the first feeding mechanism; obtaining the weight of the fly ash and the desulfurization ash through the first feeding mechanism; obtaining the flow rate of the fly ash and the desulfurization ash through the first feeding mechanism; the first feeding mechanism determines whether the weight of the transferred fly ash and desulfurization ash reaches the preset weight based on the obtained weight and flow rate of the fly ash and the desulfurization ash; if so, stopping the transfer; if not, continuing the transfer.

[0072] Making the fly ash and the desulfurized ash move along a spiral path in the first feeding mechanism can further enhance the uniformity of the raw materials.

[0073] Exemplarily, the weight of the fly ash and the desulfurized ash can be obtained through the weighing system in the first feeding mechanism; the flow rate of the fly ash and the desulfurized ash can be obtained through the flow statistics system in the first feeding mechanism. A weight sensor can be set in the weighing system to obtain the weight of the fly ash and the desulfurized ash, and a flow sensor can be set in the flow statistics system to obtain the flow rate of the fly ash and the desulfurized ash.

[0074] Among them, the obtained weight of fly ash and desulfurization ash can be the weight of fly ash and desulfurization ash per unit volume. In this way, it is possible to judge whether the supply of fly ash and desulfurization ash reaches the preset weight by multiplying the obtained weight of fly ash and desulfurization ash by the flow rate.

[0075] In one embodiment, after adding a preset weight of coal gangue to the slurry and stirring for a preset time, a coal-based solid waste filling paste is prepared, which specifically includes: feeding the coal gangue blocks to a crusher, and crushing the coal gangue blocks by the crusher; transferring the processed coal gangue blocks to a vibrating screen, and screening the processed coal gangue blocks by the vibrating screen to obtain coal gangue that meets the supply demand; after the slurry is prepared, using a coal gangue feeding mechanism to transfer the coal gangue to the agitator; stirring the slurry and the coal gangue in the agitator to a preset time threshold, to prepare a coal-based solid waste filling paste.

[0076] Coal gangue blocks are waste generated during coal production and processing, and their sizes vary. The coal gangue used to prepare coal-based solid waste filling paste needs to meet certain size requirements.

[0077] The screen in the vibrating screen can be replaced according to the size requirements of the coal gangue used to prepare the coal-based solid waste filling paste.

[0078] The gangue feeding mechanism can deliver a preset weight of gangue to the agitator.

[0079] In one embodiment, the preset time threshold for stirring the slurry and the coal gangue is 2 minutes.

[0080] In one embodiment, a dust collector is connected to the agitator, which can effectively prevent dust from flying and reduce dust pollution to the produced coal-based solid waste filling paste.

[0081] In order to make the prepared coal-based solid waste filling paste have better fluidity, in one embodiment, the processed coal gangue blocks are screened by the vibrating screen to obtain coal gangue that meets the supply demand, specifically including: judging whether the coal gangue is less than 16 mm; if so, the processed coal gangue blocks are used as coal gangue that meets the supply demand; if not, they are transferred to the crusher for further crushing.

[0082] In one embodiment, the silicate cement, sulphoaluminate cement, mineral powder and sodium sulfate mixed in a preset ratio are stirred to prepare a curing agent, specifically comprising: using a third feeding device to steadily transfer the silicate cement to a third conveying mechanism, and the third conveying mechanism spirally transfers the silicate cement to a third feeding mechanism; using a fourth feeding device to steadily transfer the sulphoaluminate cement to a fourth conveying mechanism, and the fourth conveying mechanism spirally transfers the sulphoaluminate cement to a fourth feeding mechanism; using a fifth feeding device to steadily transfer the mineral powder to a fifth conveying mechanism, and the fifth conveying mechanism spirally transfers the mineral powder to a fifth feeding mechanism; using a sixth feeding device to steadily transfer the sodium sulfate to a sixth conveying mechanism, and the sixth conveying mechanism spirally transfers the sodium sulfate to a sixth feeding mechanism; mixing and stirring the preset weight of silicate cement transferred by the third feeding mechanism, the preset weight of sulphoaluminate transferred by the fourth feeding mechanism, the preset weight of mineral powder transferred by the fifth feeding mechanism and the preset weight of sodium sulfate transferred by the sixth feeding mechanism in a stirrer to prepare the curing agent.

[0083] Each loading device, each conveying mechanism, each feeding mechanism can be the same as the loading device, each conveying mechanism, each feeding mechanism used for preparing the slurry.

[0084] Portland cement, sulphoaluminate cement, mineral powder and sodium sulfate are mainly powders, so the agitator in this embodiment can use a powder mixing homogenizer.

[0085] In one embodiment, after preparing the curing agent, the method further comprises: storing the curing agent in a second storage bin, wherein a steady flow feeding device can be used to transfer the curing agent to the second storage bin for storage.

[0086] In one embodiment, the weight proportions of the raw materials are: 50-55% coal gangue, 15-20% fly ash, 4-8% desulfurized ash, 2-5% silicate cement, 0.5-2% sulfoaluminum cement, 5-10% mineral powder, 0.5-2% sodium sulfate, 14-16% water, and 0.5-2% water reducer. In this way, by controlling the relative ratio of silicate cement and sulfoaluminum cement to be close to 4:1, and controlling the ratio of coal gangue to be close to 1 / 2, the prepared coal-based solid waste filling paste has better fluidity, thereby meeting the requirements of continuous mining and filling process in mines.

[0087] A person skilled in the art can appropriately adjust the ratio of the raw materials of the coal-based solid waste filling paste according to the actual demand for the compressive strength of the coal-based solid waste filling paste. The following is an implementation method of the present invention for obtaining the ratio of the raw materials of the coal-based solid waste filling paste.

[0088] Conduct non-destructive analysis and testing on coal gangue to obtain the composition and structure of coal gangue.

[0089] Fly ash is coal-fired solid waste produced by power plants, thermal power plants, chemical plants, etc. The quality grade of fly ash used to prepare coal-based solid waste filling paste is not lower than II. Non-destructive analysis and testing are carried out on fly ash to obtain its composition and structure.

[0090] Desulfurization ash is solid waste generated by desulfurization in power plants, thermal power plants, chemical plants, etc. Non-destructive analysis and testing is performed on the desulfurization ash to obtain its composition and structure.

[0091] The silicate cement model may be P.O42.5 cement, and the strength grade of sulphoaluminium cement may be 42.5; the sodium sulfate may be industrial grade sodium sulfate, and the purity of the exemplary sodium sulfate may be greater than 90%.

[0092] The strength grade of mineral powder can be higher than S95 grade, and non-destructive analysis and testing can be carried out to obtain the composition and structure of mineral powder.

[0093] Among them, non-destructive analysis and testing can be XRF (X-ray Fluorescence Spectrometer) testing or XRD (X-ray diffraction) testing.

[0094] For details, see Figures 2 to 6 In one embodiment, XRF detection is performed on the gangue from Shangwan Coal Mine to obtain the following composition table of the gangue from Shangwan Coal Mine:

[0095] XRD test was carried out on the gangue from Shangwan Coal Mine. For specific results, see Figure 3 , Figure 3The horizontal coordinate 2theta / (degree) in the image is 2θ, and degree is the diffraction angle. Figure 3 The vertical coordinate Intensity / (au) where Intensity stands for intensity, au (arbitary units) stands for arbitrary units.

[0096] XRF test was performed on Jinjie fly ash, and the composition table of Jinjie fly ash was obtained as follows:

[0097] XRF test was performed on Handan desulfurization ash, and the composition table of Handan desulfurization ash was obtained as follows:

[0098] XRF test was performed on the mineral powder to obtain the mineral powder composition table as follows:

[0099] Specifically, it can be X-ray fluorescence qualitative and semi-quantitative analysis detection.

[0100] In one embodiment, after determining the composition of each raw material of the coal-based solid waste filling paste, an experiment is conducted to optimize the ratio of each raw material, as follows: In order to make the coal-based solid waste filling paste have better fluidity, the size of the coal gangue is optimized as follows: Particle size / mm -16~+9.75 -9.5~+4.75 -4.75~+2.36 -2.36~+1.18 -1.18~+0.6 -0.6~+0.3 -0.3 ~+0.0 content / % 10 15 15 20 15 10 15 Particle size / mm +9.5 +4.75 +2.36 +1.18 +0.6 +0.3 -0.3 Cumulative content / % 10 25 40 60 75 85 100 Under the same working conditions, the weight fraction of mineral powder in the formula is fixed, and the amount of sulphoaluminate cement and silicate cement is controlled. The experimental results are as follows:

[0101] Based on the change in compressive strength, sulfate was added to optimize the ratio of items 7 and 8 above, and the experimental results were as follows:

[0102] Based on the change in compressive strength, the ratio of item 3 above was optimized, and the experimental results were as follows:

[0103] Based on the change in compressive strength, the above ratio 1 is fixed, and the effect of water reducer on it (the effect of concentration on it) is optimized. The experimental results are as follows:

[0104] The proportions of the raw materials for obtaining the final coal-based solid waste filling paste are as follows:

[0105] The coal-based solid waste filling paste and its preparation method provided in the embodiments of the present invention can comprehensively utilize solid wastes such as coal gangue, fly ash, desulfurization ash, etc. generated during coal mining and use, and cooperate with the mine filling coal mining process to achieve the requirements of sustainable development of mines.

[0106] In addition, the coal-based solid waste filling paste and its preparation method provided in the embodiments of the present invention, by optimizing the ratio, can make the coal-based solid waste filling paste have higher fluidity within 1-2 hours, can produce solidification strength that meets the strength technical requirements within 4-8, can meet the mining and filling process cycle requirements of the mine in three shifts a day, realize continuous mining and filling, and thus achieve the balance of coal mine mining and filling.

[0107] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0108] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

[0109] In particular, for the device embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment.

[0110] For the convenience of description, the above device is described by dividing the functions into various units / modules. Of course, when implementing the present invention, the functions of each unit / module can be implemented in the same or multiple software and / or hardware.

[0111] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.

Claims

1. A coal-based solid waste filling paste, It is characterized in that The invention comprises the following components in parts by weight: 50-55% of coal gangue, 15-20% of fly ash, 4-8% of desulfurized ash, 2-5% of silicate cement, 0.5-2% of sulphoaluminium cement, 5-10% of mineral powder and 14-16% of water.

2. The coal-based solid waste filling paste according to claim 1, It is characterized in that The invention comprises the following components in parts by weight: 51-53% of coal gangue, 17-19% of fly ash, 4-5% of desulfurized ash, 2-3% of silicate cement, 0.5-1% of sulphoaluminium cement, 6-8% of mineral powder and 14-16% of water.

3. The coal-based solid waste filling paste according to claim 1, It is characterized in that It also contains 0.5-2% by weight of sodium sulfate.

4. The coal-based solid waste filling paste according to claim 3, It is characterized in that It also includes 0.5-2% (by weight) of a water reducing agent.

5. The coal-based solid waste filling paste according to claim 4, It is characterized in that The invention comprises the following components in parts by weight: 52% of coal gangue, 18% of fly ash, 4.5% of desulfurized ash, 2% of silicate cement, 0.5% of sulphoaluminium cement, 7% of mineral powder, 0.5% of sodium sulfate, 15% of water and 0.5% of water reducing agent.

6. A method for preparing coal-based solid waste filling paste, It is characterized in that include: Mixing a curing agent, fly ash, desulfurized ash and a water reducing agent solution in a first preset ratio to obtain a slurry base material, wherein the first preset ratio includes the following components in parts by weight: 30.3% curing agent, 54.6% fly ash, 13.6% desulfurized ash and 1.5% water reducing agent; Stirring the slurry base material to prepare slurry; A coal-based solid waste filling paste is prepared by adding a preset weight of coal gangue into the slurry and stirring for a preset time.

7. The method for preparing the coal-based solid waste filling paste according to claim 6, It is characterized in that Before stirring the curing agent, fly ash, desulfurized ash and water reducing agent solution mixed in a first preset ratio to obtain a slurry base material, the method further comprises: Mixing silicate cement, sulphoaluminate cement, mineral powder and sodium sulfate in a second preset ratio to obtain a curing agent base, wherein the second preset ratio includes the following components in parts by weight: 20% silicate cement, 5% sulphoaluminate cement, 70% mineral powder and 5% sodium sulfate; Stirring the curing agent base material, and determining whether the uniformity of the curing agent base material meets the preset curing agent uniformity; If yes, the preparation of the curing agent is completed; If not, continue stirring the curing agent base.

8. The method for preparing the coal-based solid waste filling paste according to claim 6, It is characterized in that Stirring the curing agent, fly ash, desulfurized ash and water reducing agent solution mixed in a first preset ratio to obtain a slurry base material; The slurry base material is stirred to prepare the slurry, specifically comprising: The first feeding device is used to steadily transfer the fly ash and desulfurization ash in the first storage bin to the first conveying mechanism, and the first conveying mechanism spirally transfers the fly ash and the desulfurization ash to the first feeding mechanism; The second feeding device is used to steadily transfer the curing agent in the second storage bin to the second conveying mechanism, and the second conveying mechanism spirally transfers the curing agent to the second feeding mechanism; Mixing a water reducer and water in a preset ratio in a water reducer container to prepare a water reducer solution, and connecting a quantitative water pump to the water reducer container, wherein the preset ratio includes the following components in parts by weight: 3.23% water reducer and 96.77% water; A preset weight of fly ash and desulfurized ash delivered by the first feeding mechanism, a preset weight of curing agent delivered by the second feeding mechanism, and a preset weight of water reducing agent solution delivered by the quantitative water pump are stirred in a stirrer to prepare a slurry.

9. The method for preparing the coal-based solid waste filling paste according to claim 8, It is characterized in that The preset weight of fly ash and desulfurized ash delivered by the first feeding mechanism specifically includes: Allowing the fly ash and the desulfurized ash to travel along a spiral path in the first feeding mechanism; Obtaining the weight of the fly ash and the desulfurized ash through the first feeding mechanism; Obtaining the flow rates of the fly ash and the desulfurized ash through the first feeding mechanism; The first feeding mechanism determines whether the weight of the fly ash and the desulfurization ash transferred reaches a preset weight based on the acquired weight and flow rate of the fly ash and the desulfurization ash; If so, stop delivering; If not, continue passing.

10. The method for preparing the coal-based solid waste filling paste according to claim 6, It is characterized in that After adding a preset weight of coal gangue to the slurry and stirring for a preset time, a coal-based solid waste filling paste is prepared, which specifically includes: Loading the gangue blocks to a crusher, and crushing the gangue blocks by the crusher; The processed gangue blocks are transferred to a vibrating screen, and the processed gangue blocks are screened by the vibrating screen to obtain the gangue that meets the supply demand; After the slurry is prepared, the gangue is transferred to the agitator using a gangue feeding mechanism; The slurry and the coal gangue are stirred in the stirrer to a preset time threshold to prepare a coal-based solid waste filling paste.

Citation Information

Patent Citations

  • Self-compaction filling paste body and preparation process thereof

    CN102924010A

  • Mining composite cementing material and mining filling material

    CN105314944A

  • Gangue paste cementing material, preparation method thereof, gangue paste filling material and preparation method thereof

    CN111689753A

  • Low-cost multi-source solid waste filling cementing material as well as preparation method and application thereof

    CN115925286A

  • All-solid waste cementing material as well as preparation method and application thereof

    CN116924711A