Preparation method of carburized ZTA ceramic material

Through acoustic resonance mixing and carburizing heat treatment technology, carbon atoms migrate to the zirconia lattice and grain boundaries, stabilizing the tetragonal phase, solving the problems of insufficient fracture strength and wear resistance of ceramic materials, and realizing the high fracture strength and wear resistance of ZTA ceramic materials. Improved wear resistance.

CN118724568AActive Publication Date: 2024-10-01苏州芯合半导体材料有限公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410767327.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

It is difficult to significantly improve the fracture strength and wear resistance of ceramic materials with existing technology. Especially during the preparation process of ZTA ceramics, the stability of zirconia is affected by the content of yttrium stabilizer, which causes the ceramic to phase change at high temperatures and is prone to cracks, etc. defect.

Method used

Acoustic resonance technology is used to mix alumina powder and yttrium-stabilized zirconia powder, and the ZTA ceramic blank is obtained by dry pressing and pre-sintering. It is then carburized and heat treated and hot isostatically pressed in a graphite environment to migrate carbon atoms to zirconia. The crystal lattice and grain boundaries stabilize the tetragonal phase and avoid phase changes and cracks.

Benefits of technology

It significantly improved the fracture strength of ZTA ceramic materials by about 20%, and showed significant improvement in wear resistance in wear tests, avoiding ceramic cracks and abnormal expansion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724568A_ABST
    Figure CN118724568A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of ZTA ceramics, and particularly relates to a preparation method of a carburized ZTA ceramic material. The method comprises the following steps: 1) preparing a ZTA ceramic blank; 2) carburizing heat treatment; and 3) hot isostatic pressing treatment. Compared with the prior art, the carburized ZTA ceramic material has the technical advantages that the carburized ZTA ceramic material is a product pre-sintered at the temperature of 1200 DEG C, the porosity is reserved, and a certain strength is given to a blank. According to the invention, permeation of carbon atoms is realized through migration of the carbon atoms in the pre-sintered ceramic, and a part of the carbon atoms act in zirconium oxide crystal lattices to stabilize a high-temperature phase of zirconium oxide, so that the stable tetragonal phase of the zirconium oxide can be better retained at room temperature, conversion to a monoclinic phase is avoided, and the volume change of the zirconium oxide is increased; and thus, defects such as cracks in the ceramic are avoided. And the other part stays at the grain boundary of the ceramic particles, so that abnormal phenomena such as ceramic crack propagation and the like can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ZTA ceramic materials, and in particular relates to a method for preparing a carburized ZTA ceramic material. Background Art

[0002] ZTA ceramics have good high-temperature mechanical strength, high hardness, high elastic modulus, high flexural strength, high fracture toughness, thermal shock resistance, wear resistance, oxidation resistance and corrosion resistance. They can be used as structural ceramics for high-efficiency gas turbines, aerospace and automotive parts, corrosion-resistant coatings, ceramic pipe plugs, cutting blades, sealing valves, armor, molds and metal link parts. They have low thermal conductivity, high insulation, good thermal expansion coefficient, special optical properties and good biocompatibility, and can be used in functional ceramics such as electrical insulators, prostheses, piezoelectric ceramics, dental ceramics, ceramic films, high-efficiency filtration, reverse osmosis, gas separation and catalysis.

[0003] In conventional preparation processes, ZTA ceramics are often sintered in an air atmosphere using a muffle furnace. However, the phase change toughening effect of zirconium oxide is affected by the amount of stabilizer added. Usually, when the yttrium content of yttrium-stabilized zirconium oxide increases to more than 5%, c-ZrO2 will easily appear during the preparation process, resulting in poor stability of zirconium oxide. Therefore, the stabilizing effect of yttrium on zirconium oxide is also limited.

[0004] Carburizing technology is a heat treatment process for surface treatment. The method is to place the workpiece in an active carburizing medium, heat it to a certain temperature and keep it warm for a sufficient time, so that the active carbon atoms dispersed in the carburizing medium penetrate into the surface of the steel part, thereby obtaining high carbon on the surface and the core still retains the original composition. According to the different carbon-containing media, carburizing can be divided into gas carburizing, solid carburizing, liquid carburizing and carbonitriding. Solid carburizing is commonly used.

[0005] There is an existing patent application 201410026240.9 on ceramic carburization, which discloses a zirconia-based ceramic and metal connector and its connection method, which describes the corresponding carburizing process, but focuses on the penetration of carbon vapor into the unit cell and the unit cell gap. This patent is about the migration of carbon atoms in pre-fired ceramics to achieve the penetration of carbon atoms, a part of which acts in the zirconia lattice, stabilizing the high-temperature phase of zirconia, so that its stable tetragonal phase can be better retained to room temperature, avoiding transformation to the monoclinic phase, increasing its volume change, and thus avoiding the generation of defects such as cracks in ceramics. The other part stays at the grain boundaries of ceramic particles, which can avoid the generation of abnormal phenomena such as ceramic crack expansion. Moreover, this patent does not involve preheating treatment for carburized workpieces, which is only to improve the wettability of ceramic connectors and nickel-based alloys, while this application is to improve the fracture strength and wear resistance of ceramic materials. Summary of the invention

[0006] The technical problem to be solved by the present invention is: in view of the defect that the fracture strength of ceramic materials cannot be greatly improved under the existing preparation conditions, a method for preparing a carburized ZTA ceramic material is provided, and the ZTA ceramic material prepared by the method has high fracture strength.

[0007] The technical solution adopted by the present invention to solve the technical problem is as follows: a method for preparing a carburized ZTA ceramic material, which includes the following preparation steps: 1) Preparation of ZTA ceramic blanks Powder mixing: using acoustic resonance technology to evenly mix alumina powder, yttrium-stabilized zirconia powder, dispersant and water to obtain a mixed slurry; The acoustic resonance technology has an acceleration of 80G, a mixing time of 10 to 15 minutes, and uses zirconium oxide balls with a particle size of 0.3 to 1.4 mm as an auxiliary mixing medium; Powder granulation: The dispersed mixed slurry is filtered through a sieve, and then a binder and a release agent are added in sequence, and granulated through a granulation tower.

[0008] Dry pressing: The obtained granulated powder is dry pressed to obtain a ceramic green body; Pre-firing: The ceramic blank is placed in a muffle furnace for pre-firing to obtain a ZTA ceramic blank; 2) Carburizing heat treatment A layer of graphite is laid on the bottom of the alumina crucible, and then the ZTA ceramic blank pre-sintered in step 1) is placed in the crucible padded with graphite, and then another layer of graphite is placed to cover the ZTA ceramic blank, and the crucible is covered with a lid, and the blank is placed in a furnace for heat treatment to obtain a ZTA ceramic part; the heat treatment has a sintering temperature of 1450-1550° C., a holding time of 4h-6h, and a heating rate of 2-18° C. / min; 3) Hot isostatic pressing The ZTA ceramic parts after carburization in step 2) are ultrasonically cleaned, dried, placed in a Hip sintering furnace, and subjected to hot isostatic pressing; In terms of weight, the aluminum oxide powder is 70 to 96 parts, the yttrium-stabilized zirconium oxide powder is 4 to 30 parts, the dispersant is 1 to 10 parts, and the mass ratio of the sum of the weight of the aluminum oxide powder and the yttrium-stabilized zirconium oxide powder to water is 1: (1 to 2); the binder is 2 to 3 parts, and the release agent is 0.5 to 1 part; the dispersant is ammonium polyacrylate or ammonium polymethacrylate, the binder is ammonium acrylate or ammonium acrylate salt, and the release agent is vegetable oil.

[0009] Preferably, the alumina powder of the present invention has a particle size of 100-400 nm and a purity of 99.99%; the yttrium-stabilized zirconia powder has a particle size of 30-40 nm and a purity of 99.9%.

[0010] Preferably, the mesh size of the sieve of the present invention is 200-325 meshes; the dry pressing pressure of the dry pressing molding is 1.1-2.3 MPa; the pre-burning temperature of the pre-burning is 800-1300°C, the heating rate is 1.5-15°C / min, and the insulation time is 30-60min.

[0011] Preferably, the hot isostatic pressing treatment of the present invention has a specific process of: a heating rate of 5 to 10°C / min, a holding pressure of 100 to 200 MPa, a maximum temperature of 1350°C to 1400°C, and a holding time of 1 to 3 hours.

[0012] Preferably, the ZTA ceramic blank of the present invention has a diameter of 2.8 mm and a length of 12 mm.

[0013] Preferably, the graphite described in the present invention is high-purity graphite powder with a mass percentage of 99.9% and a mesh size of 100 meshes.

[0014] Compared with the prior art, the technical advantages of the present invention are: 1) The average fracture strength of conventional color ZTA ceramic materials is 1091.4 MPa, while the average fracture strength of ceramic materials after using the method of the present invention is 1349.8 MPa. The fracture strength of the ceramic material is increased by about 20%, and the advantages are also significant in actual wear tests.

[0015] 2) The carburized ZTA ceramic material of the present invention is a product pre-fired at 1200°C, which retains porosity and gives the blank a certain strength. In principle, the present invention realizes the infiltration of carbon atoms by the migration of carbon atoms in the pre-fired ceramics. A part of it acts in the zirconia lattice, stabilizing the high-temperature phase of zirconia, so that its stable tetragonal phase can be better retained to room temperature, avoiding transformation to the monoclinic phase, increasing its volume change, and thus avoiding the generation of defects such as cracks in the ceramic. The other part stays at the grain boundaries of the ceramic particles, which can avoid the occurrence of abnormal phenomena such as ceramic crack expansion. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a microstructure diagram of the ZTA ceramic material prepared in Example 1 of the present invention.

[0017] Figure 2 This is a microstructure diagram of the ZTA ceramic material prepared in Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0018] The present invention will be further described below in conjunction with the embodiments. Example 1

[0019] Preparation of ZTA ceramic blanks Powder mixing: 85 parts of alumina powder, particle size 300nm, purity 99.99%; 20 parts of yttrium-stabilized zirconia powder, particle size 30-40nm, purity 99.9%, 5 parts of ammonium polyacrylate, 210 parts of water, mixing using acoustic resonance technology (80G acceleration, mixing for 10min, using zirconia balls with a particle size of 1mm as an auxiliary mixing medium) to prepare a mixed slurry.

[0020] Powder granulation: The dispersed mixed slurry is filtered through a 300-mesh sieve to remove the zirconium oxide balls, and 3 parts of ammonium acrylate emulsion and 1 part of vegetable oil are added in sequence, and granulation is performed through a granulation tower.

[0021] Dry pressing: The obtained powder is dry pressed at 2.0MPa to obtain a ceramic green body; Pre-firing: The ceramic blank is pre-firing in a muffle furnace to obtain a ZTA ceramic blank. The diameter of the ceramic blank is 2.8 mm, the length is 12 mm, the pre-firing temperature is 1200°C, the heating rate is 10°C / min, and the holding time is 40 min.

[0022] 2) Carburizing heat treatment A 80 mm thick first graphite is laid on the bottom of the alumina crucible. The graphite is high-purity graphite powder with a mass percentage of 99.9% and a mesh size of 100. Then the pre-fired ZTA ceramic blank is gently placed in the crucible padded with graphite (to avoid the ceramic blank directly passing through the graphite pad and contacting the bottom, resulting in poor carburizing effect). After placing the ceramic blank, a 80 mm thick second graphite is placed to cover the ZTA ceramic blank, the crucible is covered, and the crucible is placed in a furnace for heat treatment to obtain a ZTA ceramic part with a sintering temperature of 1500°C, a holding time of 5h, and a heating rate of 10°C / min.

[0023] 3) Hot isostatic pressing The ZTA ceramic parts after carburization in step 2) were thoroughly cleaned by ultrasonic cleaning, dried and placed in a Hip sintering furnace for hot isostatic pressing with a heating rate of 8°C / min, a holding pressure of 150MPa, a maximum temperature of 1380°C and a holding time of 2h.

[0024] The ZTA ceramic part prepared in Example 1 has a microstructure as shown in FIG. Figure 1 As shown, the product performance is as follows: 6pcs of products were tested, and the breaking strength measurement data were: 1439.8MPa, 1257.8MPa, 1455.6MPa, 1444.6MPa, 1151.3MPa, with an average of 1349.8MPa; 3pcs of products were tested, hardness measurement data: 1834HV5, 1862HV5, 1819HV5, 1889HV5, 1885HV5, 1854HV5; 3pcs of products were tested, and the average wear volume of the product wear resistance test was 0.052mm 3 ; Test 3pcs of products, perform wire bonding, and judge the wear resistance by the product life. The product bonding times are 1 million to 1.5 million times. Comparative Example 1

[0025] Without pre-firing, the ceramic blank is directly degummed after dry pressing, and the rest is the same as Example 1. The degumming conditions are as follows: the heating rate is 0.33-0.67°C / min, the maximum temperature is 650°C, and the holding time is 90min. After the degumming is completed, the ceramic blank is directly clamped with tweezers and placed in a crucible filled with graphite. It is found that the blank is fragile during the clamping and moving process. The product after degumming has basically no strength. Therefore, it is necessary to pre-firing to make the ceramic parts have a certain strength to avoid easy breakage in subsequent operations. Comparative Example 2

[0026] Conventional ZTA ceramic products are not carburized and have the following characteristics: 6pcs of products were tested, and the breaking strength measurement data were: 1007.4MPa, 1207.9MPa, 1241.3MPa, 1129.4MPa, 870.9MPa, with an average of 1091.4MPa; 6pcs products were tested, hardness data: 1774HV5, 1793HV5, 1796HV5, 1772HV5, 1760HV5, 1779HV5; 3pcs of products were tested, and the average wear volume of the product wear resistance test was 0.080mm 3 ; 3pcs of products were tested, bonding times: 600,000 to 900,000 times. Comparative Example 3

[0027] Compared with Example 1, the difference is that 3 parts of chromium oxide powder are added to the raw materials. Because after adding 3 parts of chromium oxide powder to the raw materials of conventional ZTA ceramics, the bonding times of the product can be increased. The rest is the same as Example 1. The microstructure of the ZTA ceramic material prepared in Comparative Example 3 is as follows: Figure 2 As shown, it can be seen that the surface void defects increase.

[0028] Product performance of the ZTA ceramic component of comparative example 3: 6 pieces of products were tested, and the breaking strength measurement data were: 926.4 MPa, 961.4 MPa, 1135.1 MPa, 1148.7 MPa, and 1176.7 MPa, with an average of 1069.7 MPa, which was a decrease of 20.75% compared to the optimal conditions of Example 1.

[0029] 6 pieces of products were tested, and the hardness data were: 1699HV5, 1575HV5, 1661HV5, 1640HV5, 1581HV5, 1638HV5, which was a decrease of 11.21% compared to the optimal conditions.

[0030] 3pcs of products were tested, and the average wear volume of the wear resistance test was 0.078mm 3 .

[0031] 3pcs of products were tested, bonding times: 800,000 to 1,000,000 times.

Claims

1. A method for preparing a carburized ZTA ceramic material, Features: The preparation steps include: 1) Preparation of ZTA ceramic blanks Powder mixing: using acoustic resonance technology to evenly mix alumina powder, yttrium-stabilized zirconia powder, dispersant and water to obtain a mixed slurry; the acoustic resonance technology has an acceleration of 80G, a mixing time of 10 to 15 minutes, and uses zirconia balls with a particle size of 0.3 to 1.4 mm as an auxiliary mixing medium; Powder granulation: The dispersed mixed slurry is filtered through a sieve, and then a binder and a release agent are added in sequence, and granulated through a granulation tower; Dry pressing: The obtained granulated powder is dry pressed to obtain a ceramic green body; Pre-firing: The ceramic blank is placed in a muffle furnace for pre-firing to obtain a ZTA ceramic blank; 2) Carburizing heat treatment A layer of graphite is laid on the bottom of the alumina crucible, and then the ZTA ceramic blank pre-sintered in step 1) is placed in the crucible padded with graphite, and then another layer of graphite is placed to cover the ZTA ceramic blank, and the crucible is covered with a lid, and the blank is placed in a furnace for heat treatment to obtain a ZTA ceramic part; the heat treatment has a sintering temperature of 1450-1550° C., a holding time of 4h-6h, and a heating rate of 2-18° C. / min; 3) Hot isostatic pressing The ZTA ceramic parts after carburization in step 2) are ultrasonically cleaned, dried, placed in a Hip sintering furnace, and subjected to hot isostatic pressing; Among them, in terms of weight, the aluminum oxide powder is 70 to 96 parts, the yttrium-stabilized zirconium oxide powder is 4 to 30 parts, the dispersant is 1 to 10 parts, the mass ratio of the sum of the weight of the aluminum oxide powder and the yttrium-stabilized zirconium oxide powder to water is 1: (1 to 2); the binder is 2 to 3 parts, and the release agent is 0.5 to 1 part; the dispersant is ammonium polyacrylate or ammonium polymethacrylate, the binder is ammonium acrylate or ammonium acrylate salt, and the release agent is vegetable oil.

2. The method according to claim 1, Features: The alumina powder has a particle size of 100-400 nm and a purity of 99.99%; the yttrium-stabilized zirconia powder has a particle size of 30-40 nm and a purity of 99.9%.

3. The method according to claim 1, Features: The mesh number of the sieve is 200-325 meshes; the dry pressing pressure of the dry pressing molding is 1.1-2.3 MPa; the pre-burning temperature of the pre-burning is 1100-1300° C., the heating rate is 1.5-15° C. / min, and the insulation time is 30-60 min.

4. The method according to claim 1, Features: The specific process of the hot isostatic pressing treatment is as follows: a heating rate of 5 to 10°C / min, a holding pressure of 100 to 200 MPa, a maximum temperature of 1350°C to 1400°C, and a holding time of 1 to 3 hours.

5. The method according to claim 1, Features: The diameter of the ZTA ceramic blank is 2.8 mm and the length is 12 mm.

6. The method according to claim 1, Features: The graphite is high-purity graphite powder with a mass percentage of 99.9% and a mesh size of 100 meshes.

Citation Information

Patent Citations

  • Zirconia-based ceramic and metal connecting piece and connecting method thereof

    CN104788116A

  • Carburizing method for oxide ceramic

    CN103724051A

  • Anti-static ceramic as well as preparation method and application thereof

    CN107986781A

  • Setter material for sintering

    JP2007084395A

  • Carburized sintered body, and manufacturing method thereof

    JP2012255183A