Preparation method and application of green luminous hybrid manganese halide crystal

By designing the reaction between organic cations and manganese halides to prepare green-emitting zero-dimensional hybrid manganese halide crystals, the problem of light conversion efficiency and preparation difficulty of existing X-ray scintillator materials has been solved, and efficient X-ray imaging performance and flexibility have been achieved.

CN118724909AActive Publication Date: 2024-10-01SUN YAT SEN UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410741320.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-01
Estimated Expiration
2044-06-11

AI Technical Summary

Technical Problem

Existing X-ray scintillator materials have shortcomings in light conversion efficiency and preparation difficulty, and cannot meet the needs of flexible electronic products. Especially in X-ray imaging, the irradiation luminescence intensity is weak and the imaging effect is poor.

Method used

By designing organic cations and using a simple volatilization method to prepare green luminescent zero-dimensional hybrid manganese halide crystals, ethylphenyltriethylenediamine bromide is used as an organic ligand to react with the manganese halide to form a high quantum yield and low self-contained material. Absorbing organic-inorganic hybrid crystals of manganese halides and applying them to X-ray imaging.

Benefits of technology

It achieves high quantum yield and good radioluminescence performance. The light yield far exceeds that of commercial materials. It also has good air stability and flexibility, making it suitable for high-quality X-ray imaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724909A_ABST
    Figure CN118724909A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of light-emitting materials, and particularly discloses a preparation method of a green light-emitting hybrid manganese halide crystal, zero-dimensional hybrid manganese-based halide with excellent light-emitting performance is prepared by skillfully designing organic cations and utilizing a simple volatilization method, the zero-dimensional hybrid manganese-based halide has high quantum yield and negligible self-absorption, and the green light-emitting hybrid manganese-based halide can be used as a green light-emitting hybrid manganese halide crystal. According to the present invention, the luminescent material has the extraordinary radiation luminescence property, the light yields are respectively 61809 ph / MeV and 55569 ph / MeV, and are far beyond the 25000 ph / MeV of the commercial LuAG: Ce, and the luminescent material can be used in X-ray imaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of luminescent materials, and in particular relates to a preparation method and application of green luminescent hybrid manganese halide crystals. Background Art

[0002] X-ray scintillators are an important component of medical imaging, nondestructive testing, environmental monitoring and safety inspection. Scintillators absorb X-rays and convert them into visible light radiation, and then a visible light camera can be used to obtain a projected image of the object. The most widely used commercial scintillators are NaI(Tl), CsI(Na), LYSO and PbWO4. Despite decades of intensive research, scintillators are still imperfect. First, the conversion efficiency of light is still very limited. In addition, almost all commercial scintillators are prepared under high temperature and high pressure, which increases their cost and difficulty of preparation. Moreover, the inherent stiffness cannot meet the growing demand for flexible electronics.

[0003] In recent years, metal halide perovskites have been widely used in X-ray sensors due to their high photoluminescence quantum yield (PLQY), strong absorption, long carrier diffusion length, high defect tolerance, and friendly processing environment. In addition, the soft properties of perovskites make them potential candidates for flexible integration of imaging sensors. To date, many new technologies have been developed to prepare perovskite X-ray detectors. Henning et al. used inkjet printing technology to prepare flexible perovskite X-ray detectors. The advantages of this technology are high reproducibility and strong stability. Huang et al. reported that the good connectivity and crystallinity of perovskite crystals in perovskite-filled films for large-area detector arrays created a smooth surface, resulting in good imaging quality. Polymer encapsulation can also be used to prepare flexible films for X-ray detectors, realizing stable and efficient X-ray detectors. Lead-free perovskite single crystals, such as Cs2AgBiBr6, Cs3Bi2I9, and Cs3Cu2I5, have also been used for X-ray detection. However, the fabrication process of high-quality scintillator films is usually complicated, which may hinder their large-scale production.

[0004] Flexible scintillators are usually prepared by combining perovskite nanocrystal powder with polymers. For example, Zeng et al. prepared large-area thin films by adding CsPbBr3@Cs4PbBr6 powders into polystyrene / toluene solution; Liang et al. introduced BA2PbBr4:Mn(II) solid powder into polymethyl methacrylate / dichloromethane to achieve scintillators with high-resolution X-ray imaging.

[0005] In recent years, manganese-based metal halides have shown high emission performance and good stability, making them the most advanced scintillating materials. Tao and colleagues 2+A temperature-dependent tunable dual emission was found in the 0D hybrid (C4H9NH3)2MnI4, i.e., the additional emission centers come from STEs, which are the main sources of 0D Mn 2+ Unfortunately, most manganese halide complexes are not ideal for X-ray imaging because they produce weaker luminescence intensity under X-ray irradiation than commercial scintillators, resulting in poor imaging results.

[0006] Therefore, providing an organic-inorganic hybrid manganese-based metal halide that can be used as an X-ray scintillator material and has high fluorescence quantum yield and good air stability is a problem that needs to be urgently solved in the prior art. Summary of the invention

[0007] In order to solve the above technical problems, the present invention proposes a method for preparing green luminescent hybrid manganese halide crystals. Through the ingenious design of organic cations and the use of a simple volatilization method, a zero-dimensional hybrid manganese-based halide with excellent luminescence performance is prepared. The zero-dimensional hybrid manganese-based halide has high quantum yield and negligible self-absorption, and has extraordinary radioluminescence performance. The light yields are 61809ph / MeV and 55569ph / MeV, respectively, which far exceed the 25000ph / MeV of commercial LuAG:Ce, and are applied to X-ray imaging.

[0008] In order to achieve the above object, the present invention is achieved through the following technical solutions:

[0009] In one aspect, the present invention provides a method for preparing a green luminescent hybrid manganese halide crystal, comprising the following steps:

[0010] S1: dissolving 1,4-diazabicyclo[2,2,2]octane in an organic solvent, adding 2-bromoethylbenzene, stirring to form a white precipitate, and then treating to obtain an organic ligand of ethylphenyltriethylenediamine bromide;

[0011] S2: adding manganese halide and ethylphenyltriethylenediamine bromide organic ligand into an organic solvent, fully mixing, and heating and volatilizing to obtain manganese halide organic-inorganic hybrid crystals.

[0012] Preferably, the molar ratio of 1,4-diazabicyclo[2,2,2]octane to 2-bromoethylbenzene in S1 is 1:1.

[0013] Preferably, the concentration of 1,4-diazabicyclo[2,2,2]octane in the organic solvent in S1 is 1 mmol / (1-2) mL.

[0014] Preferably, in S1, 1,4-diazabicyclo[2,2,2]octane is dissolved in an organic solvent, 2-bromoethylbenzene is added under stirring, and the mixture is stirred for 3 hours to form a white precipitate, which is then centrifuged, washed and dried to obtain an organic ligand of ethylphenyltriethylenediamine bromide.

[0015] Preferably, the molar ratio of manganese halide to ethylphenyltriethylenediamine bromide organic ligand in S2 is 1:(2-2.2).

[0016] Preferably, the concentration of the manganese halide in the organic solvent in S2 is 1 mmol / (10-15) mL, and the concentration of the ethylphenyltriethylenediamine bromide organic ligand in the organic solvent is 2 mmol / (20-25) mL.

[0017] Preferably, in S2, manganese halide and ethylphenyltriethylenediamine bromide organic ligand are added to an organic solvent respectively, filtered respectively, mixed thoroughly, heated and volatilized to obtain manganese halide organic-inorganic hybrid crystals.

[0018] Preferably, the temperature of the heating treatment in S2 is 55-75° C., and the time of the heating treatment is 6-10 hours.

[0019] In another aspect, the present invention provides the use of the manganese halide organic-inorganic hybrid crystal prepared by the above method for preparing an X-ray scintillator.

[0020] Preferably, the method for preparing an X-ray scintillator from the manganese halide organic-inorganic hybrid crystal comprises the following steps:

[0021] S1: firstly grinding manganese halide organic-inorganic hybrid crystals into powder, and then ultrasonically dispersing the powder in a dichloromethane solution to obtain a mixture of manganese-based metal organic-inorganic hybrid halides;

[0022] S2: mixing a solution containing a manganese-based metal organic-inorganic hybrid halide and polydimethylsiloxane (PDMS), wherein the mass ratio of the manganese halide powder to the polydimethylsiloxane (PDMS) is 1:(1-2), and then performing ultrasonic stirring to obtain a colloidal solution;

[0023] S3: The obtained colloidal solution is dropped onto a glass sheet by spin coating, and heated at 120° C. for 12 h to finally obtain a scintillator film.

[0024] The beneficial effects of the present invention are:

[0025] The molecular formula of the organic-inorganic hybrid manganese halide crystal provided by the present invention is (pe-ted)2MnX4; pe-ted +is an ethylphenyl triethylene diamine cation; X is at least one of Cl and Br, and belongs to ethylphenyl triethylene diammonium salt. The benzene ring connected by N on the ethylphenyl triethylene diammonium salt cation in the structure enhances the interaction between atoms inside the material and reduces the defect state density, thereby improving the overall stability and luminescence efficiency of the manganese-based metal organic-inorganic hybrid metal halide crystal. It exhibits excellent crystallinity, high quantum yield and negligible self-absorption, and has extraordinary radioluminescence performance. The light yields are 61809ph / MeV and 55569ph / MeV, respectively, far exceeding the 25000ph / MeV of commercial LuAG:Ce, which is conducive to its application in high-quality X-ray imaging. In addition, due to pe-ted + Due to their high hydrophobicity, the Mn-based metal-organic-inorganic hybrid crystals show good air stability and can maintain stable luminescence and radiation properties after storage in ambient air for more than 1 month, which is much better than the recently reported all-inorganic compound Cs3MnI. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0027] Figure 1 is the mass spectrum of the organic ligand pet-ted ligand;

[0028] Figure 2 It is the NMR image of the organic ligand pe-ted ligand;

[0029] Figure 3 It is a schematic diagram of the structure of the organic ligand pet-ted ligand;

[0030] Figure 4 It is a schematic diagram of the unit cell structure of the compound (pe-ted)2MnBr4;

[0031] Figure 5 For the compound (pe-ted) 2MnCl 2.06 Br 1.94 Schematic diagram of the unit cell structure;

[0032] Figure 6 For the compound (pe-ted) 2MnBr4 and the compound (pe-ted) 2MnCl 2.06 Br 1.94 Powder diffraction pattern and single crystal structure simulated X-ray diffraction pattern;

[0033] Figure 7Thermogravimetric and microanalytical thermogravimetric diagrams of the compound (pe-ted) 2MnBr4;

[0034] Figure 8 For the compound (pe-ted) 2MnCl 2.06 Br 1.94 Thermogravimetric and microanalytical thermogravimetric diagrams;

[0035] Fig. 9 For the compound (pe-ted) 2MnBr4 and the compound (pe-ted) 2MnCl 2.06 Br 1.94 Excitation emission spectrum of

[0036] Fig.10 is the quantum yield diagram of the compound (pe-ted)2MnBr4;

[0037] Fig.11 For the compound (pe-ted) 2MnCl 2.06 Br 1.94 Quantum yield diagram of ;

[0038] Fig.12 The compound (pe-ted) 2MnBr4 and the compound (pe-ted) 2MnCl 2.06 Br 1.94 and the radiant luminescence intensity diagram of the scintillator LuAG:Ce;

[0039] Fig.13 The compound (pe-ted) 2MnBr4 and the compound (pe-ted) 2MnCl 2.06 Br 1.94 Radiation intensity diagram during two-hour high-dose rate exposure;

[0040] Fig.14 Radiation intensity diagram for the compound (pe-ted) 2MnBr4 after five hundred cycles of switching;

[0041] Fig.15 For the compound (pe-ted) 2MnCl 2.06 Br 1.94 Radiation intensity diagram after 500 switching cycles;

[0042] Fig.16 The compound (pe-ted) 2MnBr4 and the compound (pe-ted) 2MnCl 2.06 Br 1.94 and the linear relationship between the signal-to-noise ratio of the scintillator LuAG:Ce and the dose rate;

[0043] Fig.17 Radiation intensity diagram for flexible membranes at two hours of high dose rate irradiation;

[0044] Fig.18 This is the radiation intensity diagram of the flexible membrane switch after five hundred cycles;

[0045] Fig.19 This is the linear relationship between the signal-to-noise ratio of the flexible film and the scintillator LuAG:Ce and the dose rate. DETAILED DESCRIPTION

[0046] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0047] 1. The materials used in the following embodiments are as follows:

[0048] The raw materials used in the examples of the present invention were all provided by MacLean Reagent Company: manganese bromide hydrate (purity: 98%), manganese chloride (purity: 99.0%), 1,4-diazabicyclo[2,2,2]octane (purity: 98%), 2-bromoethylbenzene (purity: 98%), and acetone (Xilong, purity: 99.5%).

[0049] 2. Instruments and testing methods:

[0050] The crystal structure was tested by X-ray single crystal diffractometer (Rigaku, Japan, XtaLAB SynergyCustom);

[0051] Powder diffraction was tested by X-ray powder diffractometer (Bruker D8 ADVANCE);

[0052] The UV-visible absorption spectrum was tested by UV-visible spectrophotometer (PerkinElmer Lambda 900);

[0053] The PL spectra and lifetime decay curves were tested by Edinburgh FLS1000 fluorescence spectrometer;

[0054] A commercially available X-ray tube (TUB00154-9I-W06, MOXTEK, tungsten target, maximum power 12 W) was used as the X-ray source. The spectral signals were collected using Edinburgh FLS1000 and PMT900 photomultiplier tubes;

[0055] A commercial camera (Canon EOS M50Mark II M50) was used to capture images of a flexible large-area X-ray imaging screen;

[0056] Thermal stability was tested by thermogravimetric analysis (TGA) using a Netzsch TG 209F1 Libra.

[0057] Example 1

[0058] Preparation of PE-TED

[0059] S1: Synthesis of 2-ethylbenzene-1,4-diazabicyclo[2,2,2]octan-1-ium (pe-ted ligand):

[0060] 2.24 g 1,4-diazabicyclo[2,2,2]octane (Ted) (20 mmol) was dissolved in 25 mL acetone, 3.70 g 2-bromoethylbenzene (20 mmol) was added under magnetic stirring, and the mixture was stirred for two hours. A large amount of white precipitate was generated. The precipitate was collected by centrifugation and washed three times with acetonitrile. Finally, 4.98 g of the product pe-ted ligand was obtained by vacuum drying. Figure 1 and Figure 2 The mass spectrum and NMR of the organic ligand PET-TED successfully proved the purity of the synthesized organic ligand. Figure 3 is a schematic diagram of the structure of the organic ligand (red ball: manganese; purple ball: nitrogen; gray ball: carbon);

[0061] S2: Synthesis of (pe-ted) 2MnBr4 crystals:

[0062] 0.28g manganese bromide hydrate (1mmol) was dissolved in 10mL N,N-dimethylformamide, 0.59g pe-ted ligand (1mmol) was dissolved in 20mL methanol, the two solutions were filtered into clear beakers respectively, heated at 55°C for 8 hours, transparent block crystals were precipitated, and the mass of the obtained crystal product was 0.81g; the unit cell structure diagram of the compound (pe-ted) 2MnBr4 crystal is shown as follows Figure 4 shown.

[0063] Example 2

[0064] (pe-ted)2MnCl 2.06 Br 1.94 Preparation

[0065] S1: Synthesis of 2-ethylbenzene-1,4-diazabicyclo[2,2,2]octan-1-ium (pe-ted ligand):

[0066] 2.24 g 1,4-diazabicyclo[2,2,2]octane (Ted) (20 mmol) was dissolved in 25 mL acetone, 3.70 g 2-bromoethylbenzene (20 mmol) was added under magnetic stirring, and the mixture was stirred for two hours. A large amount of white precipitate was generated. The precipitate was collected by centrifugation, washed three times with acetonitrile, and finally dried in vacuum to obtain 5.23 g of the product pe-ted ligand;

[0067] S2: (pe-ted)2MnCl2.06 Br 1.94 Crystal synthesis:

[0068] 0.16g manganese chloride (1mmol) was dissolved in 10mL N,N-dimethylformamide, 0.59g pe-ted ligand (1mmol) was dissolved in 20mL methanol, the two solutions were filtered into clear beakers, heated at 65℃ for 6 hours, transparent block crystals precipitated, and the crystal product mass was 0.63g. (pe-ted)2MnCl 2.06 Br 1.94 The unit cell structure of a crystal is shown in the figure below: Figure 5 shown.

[0069] Comparative Example 1

[0070] In contrast to Example 1, the preparation of (pe-ted) 2MnBr4

[0071] S1: Synthesis of 2-ethylbenzene-1,4-diazabicyclo[2,2,2]octan-1-ium (pe-ted ligand):

[0072] 1.12 g 1,4-diazabicyclo[2,2,2]octane (Ted) (10 mmol) was dissolved in 10 mL acetonitrile, 1.85 g 2-bromoethylbenzene (10 mmol) was added under magnetic stirring, and the mixture was stirred for two hours. A large amount of white precipitate was generated. The precipitate was collected by centrifugation and washed three times with acetone. Finally, 2.63 g of the product pe-ted ligand was obtained by vacuum drying.

[0073] S2: Synthesis of (pe-ted) 2MnBr4 crystals:

[0074] 0.28g of manganese bromide hydrate (1mmol) was dissolved in 10mL of N,N-dimethylformamide, and 0.59g of pe-ted ligand (1mmol) was dissolved in 20mL of ethanol. The two solutions were filtered into clear beakers respectively, and heated at 65°C for 6 hours. Transparent block crystals precipitated, and the mass of the obtained crystal product was 0.78g. Compared with Example 1, the solvents used for pe-ted ligand and (pe-ted)2MnBr4 crystals were different, but both could obtain the corresponding products.

[0075] In summary, the results of the above embodiments and comparative examples show that:

[0076] Figure 6 For the compound (pe-ted) 2MnBr4 and the compound (pe-ted) 2MnCl 2.06 Br 1.94The powder diffraction pattern and the single crystal structure simulated X-ray diffraction pattern are highly consistent, and there are no other obvious impurity peaks, indicating that the compounds (pe-ted) 2MnBr4 and (pe-ted) 2MnCl 2.06 Br 1.94 The crystals have high purity and composition homogeneity.

[0077] Figure 7 and Figure 8 For the compound (pe-ted) 2MnBr4 and the compound (pe-ted) 2MnCl 2.06 Br 1.94 The thermogravimetric and microanalytical thermogravimetric diagrams show that the synthesized manganese-based metal halide is stable before 265°C and loses the organic cation first as the temperature increases.

[0078] Fig. 9 For the compound (pe-ted) 2MnBr4 and the compound (pe-ted) 2MnCl 2.06 Br 1.94 The asymmetric absorption can be attributed to the excitation emission spectrum of Mn 2+ The odd-even forbidden d→d transition. Under the excitation of 230-500nm wavelength, it shows strong narrow spectrum emission, with the emission wavelength covering 450 to 650nm. This emission feature can be attributed to Mn 2+ Typical dd orbitals of ions 4 T1→ 6 A1 transition. The half-peak width is about 50nm and the Stokes shift is about 70nm.

[0079] Fig.10 and Fig.11 For the compound (pe-ted) 2MnBr4 and the compound (pe-ted) 2MnCl 2.06 Br 1.94 Quantum yield diagram of the compound (pe-ted) 2MnBr4, with the inset being a crystal photo under natural light and ultraviolet light. The quantum yield of the compound (pe-ted) 2MnCl is as high as 95.29%. 2.06 Br 1.94 The PL value of the films is 80.32%, indicating that they have high PL performance and good application potential in WLEDs and displays.

[0080] Fig.12 For the compound (pe-ted) 2MnBr4 and the compound (pe-ted) 2MnCl 2.06 Br 1.94The radiative emission intensity diagram of the compound (pe-ted) 2MnBr4 and the compound (pe-ted) 2MnCl is estimated based on the comprehensive radiative emission spectrum area and light yield of LuAG:Ce (25000ph / MeV) and the photoluminescence intensity diagram of the compound (pe-ted) 2MnBr4 and the compound (pe-ted) 2MnCl. 2.06 Br 1.94 The light outputs are approximately 61809ph / MeV and 55569ph / MeV respectively.

[0081] Fig.13 For the compound (pe-ted) 2MnBr4 and the compound (pe-ted) 2MnCl 2.06 Br 1.94 The stability of long-term radiation at high dose rates indicates the radiation stability of the synthesized compound, which is expected to be made into flexible films for medical testing.

[0082] Fig.14 and Fig.15 For the compound (pe-ted) 2MnBr4 and the compound (pe-ted) 2MnCl 2.06 Br 1.94 The cyclic radiation intensity diagram after 500 cycles of switching on and off shows good repeatability and stability in the response under X-ray irradiation.

[0083] Detection limit is another key parameter for evaluating the performance of X-ray scintillators. Fig.16 For the compound (pe-ted) 2MnBr4 and the compound (pe-ted) 2MnCl 2.06 Br 1.94 The linear relationship between the signal-to-noise ratio and the dose rate of the scintillator LuAG:Ce was studied, and the response radiation emission spectrum under the X-ray dose rate range of 200-700μGy / s was performed, showing a linear RL response of the luminescence intensity to the dose rate. When the signal-to-noise ratio is 3, the X-ray detection limit corresponding to the compound (pe-ted) 2MnBr4 is calculated to be 1.376μGy / s, and the compound (pe-ted) 2MnCl 2.06 Br 1.94 This corresponds to 1.440 μGy / s, both of which are lower than the dose rate required for medical X-ray diagnosis (5.5 μGy / s) and the commercial scintillator LuAG:Ce (8.583 μGy / s).

[0084] By spin coating a colloidal solution of PDMS containing metal halides, a flexible film is obtained. Fig.17 The flexible membrane was irradiated with radiation intensity at a high dose rate for two hours, and the radiation intensity remained stable.

[0085] Fig.18 This is a graph of radiation intensity after 500 cycles of the flexible membrane switch, indicating that the membrane has good durability and stability in practical applications.

[0086] Fig.19 The linear relationship between the signal-to-noise ratio of the flexible film and the scintillator LuAG:Ce and the dose rate is shown. Through linear fitting, the detection limit of the film is 5.173 μGy / s, which is better than 8.583 μGy / s of the commercial scintillator LuAG:Ce.

[0087] The (pe-ted)2MnX4 (X=Cl, Br) single crystal materials prepared in the embodiment and the comparative example both achieved a fluorescence yield of more than 80%; (pe-ted)2MnBr4, as an X-ray scintillator, has a high quantum yield of 95.29% and high crystal stability, and has broad application prospects; (pe-ted)2MnBr4 has efficient X-ray imaging capability, with a light yield of up to 61809ph / MeV and a detection limit as low as 1.376μGy / s, both of which are superior to commercial LuGG:Ce scintillator materials; and (pe-ted)2MnBr4 crystals have good solution processability and film-forming properties, and a uniform and dense luminescent thin film can be obtained by a simple spin coating method while maintaining the excellent luminescence properties of the crystal.

[0088] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all details in detail, nor do they limit the invention to only the specific embodiments described. Obviously, many modifications and changes can be made according to the content of this specification.

Claims

1. A method for preparing green luminescent hybrid manganese halide crystals, characterized in that: The following steps are involved: S1: dissolving 1,4-diazabicyclo[2,2,2]octane in an organic solvent, adding 2-bromoethylbenzene, stirring to form a white precipitate, and then treating to obtain an organic ligand of ethylphenyltriethylenediamine bromide; S2: adding manganese halide and ethylphenyltriethylenediamine bromide organic ligand into an organic solvent, fully mixing, and heating and volatilizing to obtain manganese halide organic-inorganic hybrid crystals.

2. The method for preparing the green luminescent hybrid manganese halide crystal according to claim 1, characterized in that: The molar ratio of 1,4-diazabicyclo[2,2,2]octane to 2-bromoethylbenzene in S1 is 1:

1.

3. The method for preparing the green luminescent hybrid manganese halide crystal according to claim 1, characterized in that: The concentration of 1,4-diazabicyclo[2,2,2]octane in the organic solvent in S1 is 1 mmol / (1-2) mL.

4. The method for preparing the green luminescent hybrid manganese halide crystal according to claim 1, characterized in that: In the S1, 1,4-diazabicyclo[2,2,2]octane is dissolved in an organic solvent, 2-bromoethylbenzene is added under stirring conditions, and the mixture is stirred for 3 hours to form a white precipitate, which is then centrifuged, washed, and dried to obtain an organic ligand of ethylphenyltriethylenediamine bromide.

5. The method for preparing the green luminescent hybrid manganese halide crystal according to claim 1, characterized in that: The molar ratio of manganese halide to ethylphenyltriethylenediamine bromide organic ligand in S2 is 1:(2-2.2).

6. The method for preparing green luminescent hybrid manganese halide crystals according to claim 1, characterized in that: The concentration of the manganese halide in the organic solvent in S2 is 1 mmol / (10-15) mL, and the concentration of the organic ligand of ethylphenyltriethylenediamine bromide in the organic solvent is 2 mmol / (20-25) mL.

7. The method for preparing green luminescent hybrid manganese halide crystals according to claim 1, characterized in that: In the step S2, manganese halide and ethylphenyltriethylenediamine bromide organic ligand are added to an organic solvent respectively, filtered respectively, mixed sufficiently, and heated for volatilization to obtain manganese halide organic-inorganic hybrid crystals.

8. The method for preparing green luminescent hybrid manganese halide crystals according to claim 7, characterized in that: The temperature of the heating treatment in S2 is 55-75° C., and the time of the heating treatment is 6-10 hours.

9. Use of the manganese halide organic-inorganic hybrid crystal prepared by the method according to any one of claims 1 to 8 in preparing an X-ray scintillator.

10. The use of the organic-inorganic hybrid manganese halide crystal in the preparation of an X-ray scintillator according to claim 9, characterized in that: A method for preparing an X-ray scintillator from a manganese halide organic-inorganic hybrid crystal comprises the following steps: S1: firstly grinding manganese halide organic-inorganic hybrid crystals into powder, and then ultrasonically dispersing the powder in a dichloromethane solution to obtain a mixture of manganese-based metal organic-inorganic hybrid halides; S2: mixing a solution containing a manganese-based metal organic-inorganic hybrid halide and polydimethylsiloxane (PDMS), wherein the mass ratio of the manganese halide powder to the polydimethylsiloxane (PDMS) is 1:(1-2), and then performing ultrasonic stirring to obtain a colloidal solution; S3: The obtained colloidal solution is dropped onto a glass sheet by spin coating, and heated at 120° C. for 12 h to finally obtain a scintillator film.

Citation Information

Patent Citations

  • Organic-inorganic hybrid manganese halide luminescent material and preparation method thereof

    CN112961162A

  • Zero-dimensional manganese-based metal halide, preparation method thereof and application of zero-dimensional manganese-based metal halide in high-resolution flexible X-ray scintillator imaging

    CN115894256A

  • Manganese-based metal organic-inorganic hybrid halide as well as preparation method and application thereof

    CN116478684A

  • Scintillation materials and methods

    WO2024020501A1