Modified natural rubber semi-finished product as well as preparation method and application thereof

By using modified natural rubber semi-finished products in PVC electrical tape, the problem of high cost and limited supply of imported materials is solved, the effect of reducing production costs and improving tape performance is achieved, and the dependence on imported materials is reduced.

CN118725205AInactive Publication Date: 2024-10-01SHU GROUP CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410933641.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing technology, the imported graft-modified natural rubber material used in PVC electrical tape has high cost and limited supply, resulting in high production costs and dependence, making it difficult to meet the market's demand for cost reduction and quality improvement.

Method used

By preparing a modified natural rubber semi-finished product, including tobacco rubber, methyl methacrylate, benzoyl peroxide, accelerator and antioxidant, a specific process is used for grafting reaction to form a product with high aging resistance. and cohesive strength modified natural rubber semi-finished products, and apply them to PVC electrical tapes.

Benefits of technology

While maintaining material properties, it reduces production costs, reduces dependence on imported materials, improves the stability and performance of the adhesive, and ensures good bonding performance and weather resistance of the tape.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725205A_ABST
    Figure CN118725205A_ABST
Patent Text Reader

Abstract

The invention discloses a modified natural rubber semi-finished product, a preparation method and application of the modified natural rubber semi-finished product in a PVC electrical adhesive tape. The modified natural rubber semi-finished product is prepared from the following raw materials in parts by weight: 60 to 75 parts of smoke sheet rubber, 25 to 40 parts of methyl methacrylate, 1.2 parts of benzoyl peroxide, 0.4 part of accelerant M, 0.2 part of antioxidant 1010 and 500 to 600 parts of methylbenzene. According to the invention, the natural rubber is grafted with the hard monomer by utilizing the characteristics of more double bonds on the molecular chain segment of the natural rubber and easiness in addition reaction, the hard monomer adopts methyl methacrylate, and the natural rubber adopts smoked sheet rubber, so that the natural rubber can be grafted on the basis of keeping the original performance of the natural rubber; the aging resistance of the natural rubber can be effectively improved, and the cohesive strength is high. The product with stable quality is obtained, the existing raw materials are utilized for grafting reaction in a company, the market circulation link is omitted, the production cost is reduced, the quality can be autonomously controlled, the material performance improvement space is larger, and meanwhile, the dependence on imported materials is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of adhesive tapes, in particular to a modified natural rubber semi-finished product, a preparation method and application thereof in PVC electrical tapes. Background Art

[0002] As market competition becomes increasingly fierce, consumers are demanding lower prices while demanding product quality, which directly involves the cost control of manufacturing companies. To meet this demand, manufacturing companies need to tap potential from all aspects and minimize production costs.

[0003] To ensure product performance, our company uses an imported grafted modified natural rubber in its PVC pressure-sensitive adhesive tape, which can effectively improve the cohesive strength of the tape and enhance the weather resistance of the product. However, there are only a few manufacturers of this raw material in the world, and they are all located abroad. The procurement channels are limited, the material prices are high, and the cost pressure is high.

[0004] In order to reduce material costs and procurement risks, it is necessary to try to produce an intermediate product within the enterprise that can partially or even completely replace this imported material and use it in PVC electrical tape. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art, reduce material costs without changing material properties, provide a modified natural rubber semi-finished product and a preparation method, and apply the semi-finished product to PVC electrical tape to reduce import dependence.

[0006] To achieve the above object, the present invention is implemented through the following technical solutions:

[0007] In a first aspect, the present invention provides a modified natural rubber semi-finished product, comprising the following raw materials in parts by weight: 60-75 parts of smoked sheet rubber, 25-40 parts of methyl methacrylate, 1.2 parts of benzoyl peroxide, 0.4 parts of accelerator M, 0.2 parts of antioxidant 1010, and 500-600 parts of toluene.

[0008] In a second aspect, the present invention further provides a method for preparing the modified natural rubber semi-finished product described above, comprising the following steps:

[0009] S1. Adjust the roller distance of the open mill to 4mm, roughly refine the tobacco sheet rubber 2 to 4 times and let it dry, then adjust the roller distance of the open mill to 2mm, refine it 1 to 3 times and let it dry, the size is about 60cm×40cm;

[0010] S2. Into the first pre-reactor were sequentially injected 2 / 5 methyl methacrylate and 2 / 5 benzoyl peroxide, stirred for 30 minutes to obtain a first mixed solution for standby;

[0011] S3. The remaining methyl methacrylate and benzoyl peroxide were sequentially injected into the second pre-reactor and stirred for 30 minutes to obtain a second mixed solution for standby use;

[0012] S4. Toluene was injected into the main reactor, stirring was started, and the plasticized tobacco sheet was put into the plasticized tobacco sheet, and the stirring was stopped for 4 hours and allowed to stand for 1 hour;

[0013] S5. After standing, the main reactor was added with promoter M and antioxidant 1010, stirred for 5 minutes, then heated to 80 ° C and stabilized for 5 minutes;

[0014] S6. The first mixed solution obtained in the first pre-reactor was added dropwise to the main reactor for 1 hour, and the temperature was maintained at 82 to 84 ° C throughout the process, and then kept at 84 to 86 ° C for 1 hour;

[0015] S7. The second mixed solution obtained in the second pre-reactor was added dropwise to the main reactor for 3 hours, and the temperature was maintained at 84 to 86 ° C throughout the process, and then kept at 86 to 88 ° C for 1 hour;

[0016] S8. Cool to below 40°C, filter the material and obtain a modified natural rubber semi-finished product.

[0017] In a third aspect, the present invention also provides an adhesive application scheme, in which the modified natural rubber semi-finished product described above is combined with natural rubber, a tackifying resin, an antioxidant, etc. to prepare an adhesive for PVC electrical tape.

[0018] In the present invention, the natural rubber molecular chain segments have more double bonds and are easy to undergo addition reactions. By grafting natural rubber (smoked rubber) with a hard monomer (methyl methacrylate), the aging resistance and cohesive strength of natural rubber can be effectively improved while maintaining the original properties of natural rubber. The molecular weight of natural rubber and the content and composition of non-rubber components are affected by the origin and tree species, which in turn affect the stability of the adhesive. The grafted modified natural rubber can effectively reduce this adverse effect and improve the performance of the adhesive.

[0019] In the present invention, the applicant, based on many years of work and research, hopes to obtain a modified natural rubber semi-finished product with a dry glue Mooney viscosity value (ML1+4, 100°C) of 80 to 90 according to the characteristics of the adhesive tape. The adhesive prepared by combining it with other rubbers and a tackifying resin is coated on a PVC film to obtain an adhesive tape with a peel strength of not less than 1.5N / cm, an initial tack ball number between 18 and 25, and a lasting adhesion of not less than 60min. In this way, a PVC electrical tape product with better performance can be obtained. According to experience, if the rubber Mooney viscosity value is too high, the Tg temperature of the adhesive will be too high, the initial adhesion will be poor, and it will have good bonding performance at room temperature (5-40°C), but it will tend to be in a glassy state at low temperatures (below 0°C), which may lead to loss of adhesion or poor adhesion; if the rubber Mooney viscosity value is too low, the Tg temperature of the adhesive will be too low, the sustained adhesion will be poor, and it will have good bonding performance at low temperatures (below 0°C), but it will tend to be in a viscous flow state at room temperature (0-40°C), which may lead to overflow or creep of the adhesive layer. In severe cases, the adhesive will lose its pressure sensitivity and the peel strength will be extremely low. The appropriate Mooney viscosity value can ensure that the three properties of the adhesive, namely peel strength, initial adhesion and sustained adhesion, are in a relatively balanced state, and its weather resistance will be better and the performance will be more stable.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] In the present invention, while obtaining products with stable quality, the company utilizes existing raw materials for grafting reaction, removes the market circulation link, reduces production costs, allows independent quality control, leaves more room for improvement in material performance, and reduces dependence on imported materials.

[0022] In the present invention, the characteristics of natural rubber molecular chain segments having more double bonds and being easy to undergo addition reaction are utilized, and natural rubber is grafted with a hard monomer, wherein the hard monomer is methyl methacrylate and the natural rubber is smoked sheet rubber, so that the aging resistance and cohesive strength of natural rubber can be effectively improved while maintaining the original properties of natural rubber. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a picture of the modified natural rubber semi-finished product obtained in Example 1. DETAILED DESCRIPTION

[0024] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict.

[0025] The invention provides a modified natural rubber semi-finished product, comprising the following raw materials in parts by mass: 60-75 parts of smoked sheet rubber, 25-40 parts of methyl methacrylate, 1.2 parts of benzoyl peroxide, 0.4 parts of accelerator M, 0.2 parts of antioxidant 1010, and 500-600 parts of toluene.

[0026] The raw materials in the present invention, except for the following types, are all common materials on the market. Unless otherwise stated, no specific source manufacturer is specified.

[0027] Styrene butadiene rubber SBR1013: American Lion Company

[0028] Petroleum resin E5637: Exxon Corporation, USA

[0029] Petroleum resin E5600: Exxon Corporation, USA

[0030] Example 1

[0031] This embodiment provides a modified natural rubber semi-finished product, comprising the following raw materials in parts by weight: 60 parts of smoked sheet rubber, 40 parts of methyl methacrylate, 1.2 parts of benzoyl peroxide, 0.4 parts of accelerator M, 0.2 parts of antioxidant 1010, and 560 parts of toluene. The smoked sheet rubber is Thai 1# smoked sheet rubber.

[0032] The method for preparing the modified natural rubber semi-finished product of this embodiment comprises the following steps:

[0033] S1. Adjust the roller distance of the open mill to 4mm, roughly refine the tobacco rubber sheet 2 to 4 times, then adjust the roller distance of the open mill to 2mm, refine 1 to 3 times and let the sheet dry, the size is about 60cm×40cm;

[0034] S2. Into the first pre-reactor were sequentially injected 2 / 5 methyl methacrylate and 2 / 5 benzoyl peroxide, stirred for 30 minutes to obtain a first mixed solution for standby;

[0035] S3. The remaining methyl methacrylate and benzoyl peroxide were sequentially injected into the second pre-reactor and stirred for 30 minutes to obtain a second mixed solution for standby use;

[0036] S4. Toluene was injected into the main reactor, stirring was started, and the plasticized tobacco sheet was put into the plasticized tobacco sheet, and the stirring was stopped for 4 hours and allowed to stand for 1 hour;

[0037] S5. After standing, the main reactor was added with promoter M and antioxidant 1010, stirred for 5 minutes, then heated to 80 ° C and stabilized for 5 minutes;

[0038] S6. The first mixed solution obtained in the first pre-reactor was added dropwise to the main reactor for 1 hour, and the temperature was maintained at 82 to 84 ° C throughout the process, and then kept at 84 to 86 ° C for 1 hour;

[0039] S7. The second mixed solution obtained in the second pre-reactor was added dropwise to the main reactor for 3 hours, and the temperature was maintained at 84 to 86 ° C throughout the process, and then kept at 86 to 88 ° C for 1 hour;

[0040] S8. Cool to below 40°C, filter the material, and obtain a modified natural rubber semi-finished product, such as Figure 1 As shown (the appearance of the rubber semi-finished products in each embodiment is basically the same, the main difference lies in the difference in their inherent properties).

[0041] Note: During the experiment, the temperature may fluctuate slightly, but the temperature is required to always remain within the temperature range required by the above preparation method. The equipment setting value can be set within this range according to the equipment status.

[0042] Embodiment 2-4

[0043] Examples 2-4 respectively provide a modified natural rubber semi-finished product. Compared with Example 1, the contents of benzoyl peroxide, accelerator M, antioxidant 1010, and toluene in the formula remain unchanged, while the contents of smoked sheet rubber and methyl methacrylate are changed. The specific formula is shown in Table 1.

[0044] Table 1

[0045] Example 1 Example 2 Example 3 Example 4 Smoked glue 60 65 70 75 Methyl Methacrylate 40 35 30 25 Benzoyl peroxide 1.2 1.2 1.2 1.2 Accelerator M 0.4 0.4 0.4 0.4 Antioxidant 1010 0.2 0.2 0.2 0.2 Toluene 560 560 560 560

[0046] The modified natural rubber semi-finished product provided in Examples 2-4 is prepared by a method similar to that of Example 1.

[0047] Application Example 1:

[0048] The modified natural rubber semi-finished products obtained in Examples 1-4 were subjected to comparative tests, and the test results are shown in Table 2.

[0049] Table 2

[0050]

[0051]

[0052] Note [1]: When testing odor, the odor produced by toluene as a solvent is considered normal, and odors other than toluene are considered abnormal.

[0053] Note [2]: All viscosity tests were conducted using 15% solid content glue.

[0054] Note [3]: Before the Mooney viscosity test, 80 g of each semi-finished product and imported adhesive solution were taken, placed in release paper, and treated in a constant temperature drying oven at 105°C for 3 hours. The adhesive film was extruded into a sheet of 5 cm long, 5 cm wide, and 0.5-1 cm thick as a sample for testing. The preheating time for the test was 1 minute, and the test was performed after heating for 4 minutes.

[0055] Note [4]: ​​Take 7.5 parts of plasticized tobacco sheet glue, 101315 parts of styrene-butadiene rubber SBR, 15 parts of petroleum resin E5637, 15 parts of petroleum resin E5600, and 0.5 parts of antioxidant 1010, dissolve in 97.5 parts of toluene, and stir evenly until there are no particles. Prepare 4 samples in total, add 50 parts of a semi-finished product of the embodiment to each sample, and stir evenly. The above 6 adhesives are coated on the company's current 0.11mm PVC film (primer has been applied), the thickness of the dry adhesive layer ranges from 16-20um, and after drying, it is made into a roll tape for testing. Then use an electronic peel tester, an initial adhesion tester, and a sustained adhesion tester to test the peel strength, initial adhesion, and sustained adhesion respectively.

[0056] Note [5]: Aging refers to treating the tape roll at a constant temperature of 65°C for 240 hours.

[0057] As can be seen from Table 2, Example 1 has the largest Mooney viscosity, peel strength, and sustained adhesion, but the lowest initial adhesion, and the amount of hard monomer methyl methacrylate used in the formula is relatively large, the adhesive Tg is relatively higher, and the low temperature resistance is the worst; although Example 2 is better than Example 1, the initial adhesion is still low; Example 4 has the best initial adhesion, but the worst Mooney viscosity, peel strength, and sustained adhesion, the amount of hard monomer methyl methacrylate is small, the adhesive Tg is relatively lower, and the high temperature resistance is the worst. The data before and after aging vary greatly, which is also an unstable factor in quality; The various indicators of Example 3 are in a relatively moderate state, meet the expected requirements, and are the best solution.

[0058] Application Example 2:

[0059] The modified natural rubber semi-finished product obtained in Example 3 was subjected to comparative tests with ungrafted tobacco sheet rubber and imported modified natural rubber. The test results are shown in Table 4.

[0060] Table 3

[0061]

[0062]

[0063] Note [1]: Adjust the roller distance of the mixing mill to 4 mm, and roughly refine the tobacco sheet rubber for 2 to 4 times to produce sheets. Then adjust the roller distance of the mixing mill to 2 mm, refine it for 1 to 3 times, cut it into sheets of appropriate size, and mix 15 parts by weight of rubber with 85 parts by weight of toluene in a stirring kettle, stir evenly, and use it for testing.

[0064] Note [2]: Adjust the roller distance of the mixing mill to 4 mm, roughly refine the imported modified natural rubber for 4 to 7 times, and then let the sheets air-dry. Then adjust the roller distance of the mixing mill to 2 mm, refine for 3 to 5 times, cut into sheets of appropriate size, mix 15 parts by mass of rubber with 85 parts by mass of toluene, stir evenly in a stirring kettle, and use for testing.

[0065] Note [3]: All viscosity tests were conducted using 15% solid content glue.

[0066] Note [4]: ​​When testing odor, the odor produced by toluene as a solvent is considered normal, and odors other than toluene are considered abnormal.

[0067] Note [5]: Before the Mooney viscosity test, 80 g of each semi-finished product and imported adhesive solution were taken, placed in release paper, and treated in a constant temperature drying oven at 105°C for 3 hours. The adhesive film was extruded into a sheet of 5 cm long, 5 cm wide, and 0.5-1 cm thick as a sample for testing. The preheating time for the test was 1 minute, and the test was performed after heating for 4 minutes.

[0068] Note [6]: Take 7.5 parts of plasticized tobacco sheet glue, 1315 parts of styrene-butadiene rubber SBR10, 15 parts of petroleum resin E5637, and 15 parts of petroleum resin E5600, dissolve them in 97.5 parts of toluene, and stir them evenly until there are no particles. Prepare 3 samples in total, add 50 parts of a semi-finished product of the embodiment (or imported glue solution) to each sample, and stir them evenly. The above 3 adhesives are respectively coated on the company's current 0.11mm PVC film (primer has been applied), and the thickness of the dry adhesive layer ranges from 16-20um. After drying, it is made into a roll tape for testing. Then use an electronic peel tester, an initial adhesion tester, and a sustained adhesion tester to test the peel strength, initial adhesion, and sustained adhesion.

[0069] Note [7]: Aging refers to treating the tape roll at a constant temperature of 65°C for 240 hours.

[0070] As shown in Table 3, the test data of the tobacco sheet rubber are the worst, especially the stickiness (heat resistance) and peel strength. The comprehensive performance of Example 3 is obviously better than that of the ungrafted tobacco sheet rubber. The data of the imported modified natural rubber are close to those of Example 3, and Example 3 basically meets the expected effect. In the present invention, the natural rubber is modified by grafting hard monomers to obtain properties similar to those of the imported modified natural rubber, which reduces the production cost and, more importantly, reduces the dependence on imported materials.

[0071] The application scheme of the present invention is as follows: 50 parts of modified natural rubber semi-finished product, 7.5 parts of plasticized smoke sheet rubber, 101315 parts of styrene butadiene rubber SBR, 15 parts of petroleum resin E5637, 15 parts of petroleum resin E5600, 0.5 parts of antioxidant 1010, and 97.5 parts of toluene are prepared as an adhesive, which is coated on a PVC film. As shown in Table 3, good tape performance is obtained. Based on this, the formula can be appropriately adjusted according to the specific performance requirements of the tape to obtain the expected effect.

[0072] The technical solution of the present invention is further described below in conjunction with a comparative example (single component).

[0073] Comparative Example 1

[0074] This comparative example provides a modified natural rubber semi-finished product, and the preparation method is similar to that of Example 1; this comparative example provides several formulations, as shown in Table 4.

[0075] Table 4

[0076] Recipe 1 Recipe 2 Recipe 3 Recipe 4 Smoked glue 60 60 60 60 Methyl Methacrylate 40 40 40 40 Benzoyl peroxide 1.2 1.2 1.2 1.2 Accelerator M 0.4 0.4 0.4 0.4 Antioxidant 1010 0.2 0.2 0.2 0.2 Toluene 230 300 350 560

[0077] In the implementation process of Formula 1, Formula 2, and Formula 3, the viscosity of the rubber solution was too high to varying degrees, the equipment load was too large during the stirring process, and the heat generated during the grafting reaction was difficult to dissipate, the temperature control was difficult, and it was not convenient for mass production; Formula 4 achieved the smooth progress of the preparation process, and a solid content of about 15% was a more appropriate state. In the implementation of the invention technology, Formula 4 was used as the basis, the solid content was kept unchanged, and the optimal ratio was obtained by changing the raw material ratio to obtain a modified natural rubber semi-finished product with excellent performance.

[0078] Comparative Example 2

[0079] This comparative example provides a modified natural rubber semi-finished product, using methyl acrylate as a monomer for grafting, and the other formula components and contents are the same as those in Example 3, and the preparation method is similar to that in Example 1; the formula is shown in Table 5.

[0080] Table 5

[0081]

[0082]

[0083] The modified natural rubber semi-finished product obtained in Comparative Example 2 was subjected to comparative tests, and the test results are shown in Table 6.

[0084] Table 6

[0085]

[0086] Notes [1]-[5]: The method is the same as that of Application Example 1.

[0087] As can be seen from Table 6, although methyl acrylate is a hard monomer, its glass transition temperature is only 8°C, which leads to the relatively low glass transition temperature of the modified rubber after grafting, and the cohesive strength (characterized by the stickiness) is still relatively small. Although the performance after grafting is improved compared with the ungrafted tobacco sheet rubber, the improvement is small. By comparing the data before and after aging, the improvement in aging resistance is limited. In view of the test results, it is necessary to select hard monomers with high glass transition temperature, such as styrene (Tg is 80°C) and acrylonitrile (Tg is 97°C), but acrylonitrile is toxic and should not be used.

[0088] Comparative Example 3

[0089] This comparative example provides a modified natural rubber semi-finished product, using styrene as a monomer for grafting, and the other formula components and contents are the same as those in Example 3, and the preparation method is similar to that in Example 1; the formula is shown in Table 7.

[0090] Table 7

[0091] raw materials Ratio (mass parts) Smoked glue 70 Styrene 30 Benzoyl peroxide 1.2 Accelerator M 0.4 Antioxidant 1010 0.2 Toluene 560

[0092] The modified natural rubber semi-finished product obtained in Comparative Example 3 was subjected to comparative tests, and the test results are shown in Table 8.

[0093] Table 8

[0094]

[0095] Notes [1]-[5]: The method is the same as that of Application Example 1.

[0096] As can be seen from Table 8, the performance of styrene-grafted cigarette sheet glue is greatly improved compared with the ungrafted cigarette sheet glue, whether it is aging resistance (the change range of various indicators before and after aging is relatively small) or cohesive strength (maintaining adhesion), but there is still a certain gap compared with methyl methacrylate grafted cigarette sheet glue.

[0097] Comparative Example 4

[0098] This comparative example provides a modified natural rubber semi-finished product, which is grafted with standard rubber (SCR5). Other formula components and contents are the same as those in Example 3, and the preparation method is similar to that in Example 1; the formula is shown in Table 9.

[0099] Table 9

[0100] raw materials Ratio (mass parts) Standard rubber (SCR5) 70 Methyl Methacrylate 30 Benzoyl peroxide 1.2 Accelerator M 0.4 Antioxidant 1010 0.2 Toluene 560

[0101] The modified natural rubber semi-finished product obtained in Comparative Example 4 was subjected to comparative tests, and the test results are shown in Table 10.

[0102] Table 10

[0103]

[0104] Notes [1]-[5]: The method is the same as that of Application Example 1.

[0105] It can be seen from Table 10 that after the standard rubber is grafted, the performance is greatly improved compared with the ungrafted tobacco sheet adhesive, whether it is aging resistance (the change range of various indicators before and after aging is relatively small) or cohesive strength (maintaining adhesion). However, compared with the tobacco sheet adhesive grafted with methyl methacrylate, there is still a certain gap, especially the initial adhesion is not good, which makes the tape difficult to stick to the adherend.

[0106] Comparative Example 5

[0107] This comparative example provides a modified natural rubber semi-finished product, which is grafted with crepe rubber. Other formula components and contents are the same as those in Example 3, and the preparation method is similar to that in Example 1; the formula is shown in Table 11.

[0108] Table 11

[0109] raw materials Ratio (mass parts) Crepe glue 70 Methyl Methacrylate 30 Benzoyl peroxide 1.2 Accelerator M 0.4 Antioxidant 1010 0.2 Toluene 560

[0110] The modified natural rubber semi-finished product obtained in Comparative Example 5 was subjected to comparative tests, and the test results are shown in Table 12.

[0111] Table 12

[0112]

[0113] Notes [1]-[5]: The method is the same as that of Application Example 1.

[0114] It can be seen from Table 12 that after the grafting of crepe sheet glue, the performance is greatly improved compared with the ungrafted smoke sheet glue, whether it is aging resistance (the change range of various indicators before and after aging is relatively small) or cohesive strength (maintaining adhesion), it is basically equivalent to the smoke sheet glue after methyl methacrylate grafting. However, the price of crepe sheet glue is higher than that of smoke sheet glue, and the procurement channels are not as wide as those of smoke sheet glue, which is disadvantageous for cost and the procurement risk is relatively large.

[0115] The benzoyl peroxide used in the formula mainly plays the role of initiating the reaction, and a suitable oily initiator can be used in this formula; the accelerator M mainly plays the role of promoting the reaction, and can also be replaced by similar materials such as DM; the antioxidant 1010 mainly eliminates the adverse effects of oxygen in the reaction process, and can be replaced by similar materials; toluene is a universal solvent, and toluene or other suitable solvents can be selected according to the actual situation of the enterprise.

[0116] The above-mentioned embodiments only express the specific implementation of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A modified natural rubber semi-finished product, characterized in that: The invention comprises the following raw materials in parts by weight: 60-75 parts of tobacco sheet glue, 25-40 parts of methyl methacrylate, 1.2 parts of benzoyl peroxide, 0.4 parts of accelerator M, 0.2 parts of antioxidant 1010 and 500-600 parts of toluene.

2. A modified natural rubber semi-finished product according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 70 parts of tobacco sheet glue, 30 parts of methyl methacrylate, 1.2 parts of benzoyl peroxide, 0.4 parts of accelerator M, 0.2 parts of antioxidant 1010 and 560 parts of toluene.

3. The method for preparing the modified natural rubber semi-finished product according to any one of claims 1 to 2, characterized in that: The following steps are involved: S1. Adjust the roller distance of the open mill to 4mm, roughly refine the tobacco sheet rubber 2 to 4 times, then adjust the roller distance of the open mill to 2mm, refine 1 to 3 times and let the sheet dry, the size is about 60cm×40cm; S2. Into the first pre-reactor were sequentially injected 2 / 5 methyl methacrylate and 2 / 5 benzoyl peroxide, stirred for 30 minutes to obtain a first mixed solution for standby; S3. The remaining methyl methacrylate and benzoyl peroxide were sequentially injected into the second pre-reactor and stirred for 30 minutes to obtain a second mixed solution for standby use; S4. Toluene is injected into the main reactor, stirring is started, and the tobacco sheet glue after plastication in step S1 is put into the reactor, and the stirring is stopped for 4 hours and allowed to stand for 1 hour; S5. After standing, the main reactor was added with promoter M and antioxidant 1010, stirred for 5 minutes, then heated to 80 ° C and stabilized for 5 minutes; S6. The first mixed solution obtained in the first pre-reactor was added dropwise to the main reactor for 1 hour, and the temperature was maintained at 82 to 84 ° C throughout the process, and then kept at 84 to 86 ° C for 1 hour; S7. The second mixed solution obtained in the second pre-reactor was added dropwise to the main reactor for 3 hours, and the temperature was maintained at 84 to 86 ° C throughout the process, and then kept at 86 to 88 ° C for 1 hour; S8. Cool to below 40°C, filter the material and obtain a modified natural rubber semi-finished product.

4. Use of the modified natural rubber semi-finished product according to any one of claims 1 to 2 or the modified natural rubber semi-finished product obtained by the preparation method of the modified natural rubber semi-finished product according to claim 3 in the preparation of PVC electrical tape.

5. According to the use described in claim 4, the modified natural rubber semi-finished product is prepared into an adhesive for PVC electrical tape by mixing natural rubber, tackifying resin and antioxidant.

Citation Information

Patent Citations

  • Three-component composite pressure-sensitive adhesive, preparation method and adhesive tape

    CN114350279A

  • High-thermal-conductivity electronic pressure-sensitive adhesive as well as preparation method and use method thereof

    CN116254081A

  • Primer and pressure-sensitive asdhesive tape

    JP2002146274A

  • High-performance Rubber Damping Material and Method for Preparing the Same

    US20210395423A1