Crosslinked polythiophene derivative electrochromic material and preparation method thereof

Through the preparation of cross-linked polythiophene derivative electrochromic materials and the electrochemical copolymerization of c-EDT and ProDOT-Me, the problems of long response time and poor stability of electrochromic materials in the existing technology are solved, and high optical properties are achieved. contrast and fast response time, and significantly improves the material’s cycling stability.

CN118725262APending Publication Date: 2024-10-01LIAOCHENG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410686136.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing technology, conjugated polymer electrochromic materials with a variety of good electrochromic parameters are relatively scarce, and the degradation problem of cross-linked conjugated polymers due to volume shrinkage/expansion during the redox process has not been effectively addressed. solve.

Method used

By preparing cross-linked polythiophene derivative electrochromic materials, electrochemical copolymerization of c-EDT monomer and ProDOT-Me is used to control their mass ratio and cross-linking density, and the electrochromic material is deposited on the surface of the working electrode using a potentiostatic method. , achieving a material with short response time, high optical contrast and high cycle stability.

Benefits of technology

The electrochromic material has a response time of 0.5 seconds, an optical contrast of 70%, and maintains 81% activity after 1,000 cycles, significantly improving the stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725262A_ABST
    Figure CN118725262A_ABST
Patent Text Reader

Abstract

The invention discloses a cross-linked polythiophene derivative electrochromic material and a preparation method thereof, and belongs to the technical field of electrochromism. The cross-linked polythiophene derivatives are poly (1, 10), poly (1, 5), poly (1, 2) and poly (1, 1). According to the invention, the mass ratio of two monomers (c-EDT and ProDOT-Me) is changed, electrochemical copolymerization is carried out to obtain the polythiophene derivative electrochromic material with different crosslinking densities, and the microtopography, the electrochemical behavior, the spectroelectrochemistry and the electrochromic performance of the four polymers are systematically studied. The optical contrast of the cross-linked polythiophene derivative prepared by the method reaches 70%, the response time is as low as 0.5 second, and the photochemical stability is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrochromic technology, in particular to a cross-linked polythiophene derivative electrochromic material and a preparation method thereof. Background Art

[0002] Electrochromic materials exhibit different light absorption characteristics under different redox states, making them widely used in flexible displays, camouflage materials, buildings and automotive smart glass. Currently reported electrochromic materials can be divided into organic materials (polymers and small organic molecules), inorganic materials (WO3, TiO2, NiO, etc.) and organic / inorganic composite materials. As an organic electrochromic material, conjugated polymers have many unique advantages over other materials, such as good flexibility, light weight, rich colors, fast response time, etc. After the unremitting efforts of researchers, a series of high-performance conjugated polymers have been reported as electrochromic materials, such as black-transparent polymers, multicolor change polymers, near-infrared responsive polymers, etc. It must be pointed out that conjugated polymers with multiple good electrochromic parameters are still very scarce. Therefore, how to prepare conjugated polymer electrochromic materials with multiple good electrochromic parameters is a problem that needs to be solved urgently.

[0003] In recent years, researchers have used a variety of strategies to improve the electrochromic properties of conjugated polymers, such as constructing donor-acceptor type molecular structures, optimizing side chain lengths, and constructing cross-linked molecules with a network structure. Due to the presence of intramolecular pores, cross-linked conjugated polymers have high ion transport capabilities and have become a hot topic of research. For example, Bein et al. prepared a series of electrochromic materials based on two-dimensional covalent organic frameworks (COFs). Due to the presence of intramolecular nanopores, their response time was as low as 0.2s and the color rendering efficiency reached 858cm 2 C -1 . Qin et al. designed an ether chain-modified cross-linked polythiophene derivative, which exhibited faster response time and higher color development efficiency than PEDOT. On the other hand, the network structure of the cross-linked conjugated polymer has higher stability than that of the polymer with linear molecular structure, which can effectively reduce the degradation of the conjugated polymer caused by volume shrinkage / expansion during the redox process. In short, the network structure makes the cross-linked conjugated polymer show great advantages in electrochromic performance over linear conjugated polymers.

[0004] Polythiophene and its derivatives have the advantages of low working potential, rich apparent colors, and high cycle stability. As electrochromic materials, they have attracted widespread attention from researchers. Among the reported polythiophene derivatives, PEDOT and its analogs have become a class of star electrochromic polymers due to their excellent properties, such as high transmittance, fast response time, and high optical contrast. For example, PEDOT can achieve a color transition from dark blue to highly transparent blue during oxidation. Moreover, due to the strong electron donating ability of ethylene, the redox potential window of PEDOT can be extended to the negative potential region, making it an ideal cathode material for electrochromic devices. These excellent electrochromic properties give PEDOT and its derivatives broad application prospects in the field of electrochromism. Therefore, introducing cross-linked structures into PEDOT derivatives is expected to further enhance their electrochromic properties. Summary of the invention

[0005] In order to solve the problems existing in the prior art, the present invention provides a cross-linked polythiophene derivative electrochromic material and a preparation method thereof. The material prepared by the present invention has a short response time, a high optical contrast and a high cycle stability.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] In one aspect, the present invention provides a cross-linked polythiophene derivative electrochromic material, the electrochromic material having the following structural formula:

[0008]

[0009] Among them, m is 1-10, and the side chain n is 620-670.

[0010] On the other hand, the present invention also provides a method for preparing the cross-linked polythiophene derivative electrochromic material, comprising:

[0011] (1) preparing c-EDT monomer;

[0012] (2) c-EDT and 3,4-(2,2-dimethylpropylenedioxy)thiophene (ProDOT-Me) were dissolved in dichloromethane, and then a supporting electrolyte was added and mixed evenly;

[0013] (3) Using platinum wire or ITO conductive glass as the working electrode, platinum wire as the counter electrode, and Ag / AgCl as the reference electrode, a constant potential method is used to electro-deposit at a potential of 1.8 V for 10 to 20 seconds to obtain an electrochromic material deposited on the surface of the working electrode.

[0014] Preferably, the step (1) is specifically:

[0015] (11) EDT-Cl (3.00 g), methacrylic acid (2.84 g), K2CO3 (5.44 g) and KI (0.052 g) were dissolved in dimethyl sulfoxide (10 ml), reacted at 120° C. for 4 h, then extracted with dichloromethane and purified by silica gel column to obtain light yellow crystalline EDT-c; the structural formula of EDT-Cl is as follows:

[0016]

[0017] (12) ETD-c (2.00 g) and azobisisobutyronitrile (1.37 g) were dissolved in 7 ml of tetrahydrofuran, refluxed for 24 h, cooled to room temperature, and added with excess methanol to obtain a white solid, which was washed thoroughly with methanol and dried in vacuo.

[0018] Furthermore, in the step (2), the mass ratio of c-EDT to ProDOT-Me is 1:1-1:10, preferably, the mass ratio of c-EDT to ProDOT-Me is 1:10.

[0019] Preferably, the total concentration of c-EDT and ProDOT-Me is 1 to 3 g·L -1 ;

[0020] Preferably, the supporting electrolyte is tetrabutylammonium hexafluorophosphate (Bu4NPF6) with a concentration of 0.1 to 0.2 mol·L -1 .

[0021] In the preparation process of the cross-linked polythiophene derivative electrochromic material of the present invention, the reaction equation is as follows:

[0022]

[0023] The preparation formula of c-EDT is as follows:

[0024]

[0025] Among them, n is 620~670.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The present invention prepares a series of electrochromic materials with different crosslinking densities through two steps: first, the c-EDT monomer is prepared by free radical polymerization of the flexible side chain (methacrylate), and then the mass ratio of c-EDT and ProDOT-Me is adjusted to achieve copolymerization through an electrochemical method. The point-value color-changing material prepared by the present invention has a high optical contrast (70%) and a fast response time (0.5s), and has high optical stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is the linear scanning curve of two monomers with different mass ratios;

[0029] Figure 2 Cyclic voltammetry curves of two monomers with different mass ratios: (a) the mass ratio of c-EDT and ProDOT-Me is 1:10; (b) the mass ratio of c-EDT and ProDOT-Me is 1:5; (c) the mass ratio of c-EDT and ProDOT-Me is 1:2; (d) the mass ratio of c-EDT and ProDOT-Me is 1:1;

[0030] Figure 3 Infrared characterization images of poly(1,10), poly(1,5), poly(1,2) and poly(1,1);

[0031] Figure 4 (a) is the SEM photograph of poly(1,10), (b) is poly(1,5), (c) is poly(1,2) and (d) is poly(1,1);

[0032] Figure 5 Cyclic voltammetry curves of polymers at different scan rates and the relationship between redox peak current density and scan rate; (a, b) are poly(1,10), (c, d) are poly(1,5), (e, f) are poly(1,2) and (g, h) are poly(1,1);

[0033] Figure 6 (a) is the spectroelectrochemical curve of poly(1,10), (b) is poly(1,5), (c) is poly(1,2) and (d) is poly(1,1);

[0034] Figure 7 (a) is the time-transmittance curve of poly(1,10), (b) is poly(1,5), (c) is poly(1,2) and (d) is poly(1,1) tested with different switching times; poly(1,10): 565nm; poly(1,5): 564nm; poly(1,2): 564nm; poly(1,1): 564nm;

[0035] Figure 8 Response times for (a) poly(1,10), (b) poly(1,5), (c) poly(1,2), and (d) poly(1,1);

[0036] Fig. 9Cyclic voltammetry curves of (a) poly(ProDOT-Me); (b) poly(1,10); (c) poly(1,5); (d) poly(1,2); (e) poly(1,1); and (f) poly(2,1). DETAILED DESCRIPTION

[0037] In order to make the technical problems to be solved, technical solutions and advantages of the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.

[0038] In the present invention, the materials and reagents used can be obtained from commercial sources unless otherwise specified. EDT-Cl was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0039] The present invention provides a cross-linked polythiophene derivative electrochromic material and a preparation method thereof, and specific embodiments are as follows.

[0040] Example 1

[0041] A method for preparing a cross-linked polythiophene derivative electrochromic material, comprising:

[0042] (1) preparing c-EDT monomer;

[0043] (11) EDT-Cl (3.00 g), methacrylic acid (2.84 g), K2CO3 (5.44 g) and KI (0.052 g) were dissolved in dimethyl sulfoxide (10 ml), reacted at 120°C for 4 h, and then extracted with dichloromethane. The product was purified by silica gel column to obtain light yellow crystalline EDT-c with a yield of 67%.

[0044] (12) ETD-c (2.00 g) and azobisisobutyronitrile (1.37 g) were dissolved in 7 ml of tetrahydrofuran, refluxed for 24 h, cooled to room temperature, and added with excess methanol to obtain a white solid, which was washed thoroughly with methanol and dried in vacuo. Yield: 83%.

[0045] (2) Dissolve the two monomers c-EDT (5 mg) and ProDOT-Me (5 mg) in 5 mL of dichloromethane solution. Then add the supporting electrolyte tetrabutylammonium hexafluorophosphate (Bu4NPF6) into the dichloromethane solution. The supporting electrolyte concentration is 0.1 mol L -1 . Mix well.

[0046] (3) Electrochemical polymerization was carried out on an electrochemical workstation equipped with a three-electrode electrolytic cell. A platinum wire (1 mm in diameter) or ITO conductive glass (50 mm in length and 7 mm in width) was used as the working electrode, a platinum wire (1 mm in diameter) was used as the counter electrode, and an Ag / AgCl electrode was used as the reference electrode. Electrodeposition was performed at a potential of 1.8 V for 10 s using a constant potential method to obtain an electrochromic material deposited on the surface of the working electrode, which was named poly(1,1).

[0047] Example 2

[0048] In this embodiment, the mass ratio of c-EDT to ProDOT-Me is 1:2, and the amounts used are 5 mg and 10 mg respectively, which are dissolved in 7.5 mL of dichloromethane solution; the other conditions are the same as those in Example 1, and the obtained electrochromic material is named poly(1,2).

[0049] Example 3

[0050] In this embodiment, the mass ratio of c-EDT to ProDOT-Me is 1:5, and the amounts are 1 mg and 5 mg respectively, dissolved in 3 mL of dichloromethane solution; the other conditions are the same as in Example 1, and the obtained electrochromic material is named poly(1,5).

[0051] Example 4

[0052] In this embodiment, the mass ratio of c-EDT to ProDOT-Me is 1:10, and the amounts used are 1 mg and 10 mg respectively, dissolved in 5.5 mL of dichloromethane solution; the other conditions are the same as in Example 1, and the obtained electrochromic material is named poly(1,10).

[0053] In order to further illustrate the beneficial effects of the present invention, the following comparative example was constructed.

[0054] Comparative Example 1

[0055] In this comparative example, c-EDT was replaced by an equal amount of ProDOT-Me, and the other conditions were the same as those in Example 1, and the product was named poly(ProDOT-Me).

[0056] Comparative Example 2

[0057] In this comparative example, the mass ratio of c-EDT to ProDOT-Me is 2:1, and the amounts used are 10 mg and 5 mg respectively, which are dissolved in 7.5 mL of dichloromethane solution; the other conditions are the same as those in Example 1, and the obtained electrochromic material is named poly(2,1).

[0058] Comparative Example 3

[0059] This comparative example prepares PET-(1,9) according to CN202311508711.5.

[0060] The performance test of the electrochromic material prepared in the above embodiment is carried out as follows.

[0061] The prepared electrochromic material was tested by linear sweep voltammetry and cyclic voltammetry curves. The results are shown in Figure 1-2 .Depend on Figure 1 It can be seen that the initial oxidation potentials of the prepared electrochromic materials with different crosslinking densities are not much different, ranging from 1.39 to 1.42 V. Figure 2 It can be seen that in the first 10 cycles, the current density in the mixed monomer gradually increased with the increase of scanning cycles, indicating that c-EDT and ProDOT-Me copolymerized. It can also be observed that dark blue polymers are deposited on the surface of the working electrode. These results show that the cross-linked copolymer has a higher conductivity.

[0062] The structure and morphology of the prepared electrochromic material were characterized. Figure 3-4 .

[0063] Depend on Figure 3 The infrared characterization graph shows that with the increase of crosslinking density, the -1 The relative intensity of the absorption peaks at 1732 cm -1 Except for the peak at 1488cm, the six conjugated polymers have similar absorption peaks, which is consistent with the molecular structure of the prepared conjugated polymers. -1 and 1332cm -1 The peak at 1170 cm-1 is attributed to the C=C stretching vibration of the thiophene ring. -1 The peak at 1046 cm is attributed to the deformation vibration in the =CH plane. -1 and 1024cm -1 These peaks at are attributed to the CO stretching vibrations, indicating that conjugated polymers with different cross-linking densities were successfully prepared.

[0064] Depend on Figure 4 It can be seen from the SEM images that with the increase of c-EDT content in the polymer, the fiber structure becomes more and more dense and has a regular network structure, which is convenient for subsequent film formation.

[0065] The present invention also conducts performance tests on the prepared electrode materials, and the results are as follows.

[0066] The working electrode was ITO conductive glass (50 mm long and 7 mm wide), and the other conditions were the same as in Examples 1-4, and poly(1,1), poly(1,2), poly(1,5), and poly(1,10) were prepared respectively.

[0067] 1. Electrochemical performance study

[0068] The platinum wire (1 mm in diameter) with polymer film deposited prepared in Example 1-4 was used as the working electrode, the platinum wire (1 mm in diameter) was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode. The electrolyte solution was a 0.1 mol / L phosphorus hexafluoride tetrabutylamine acetonitrile solution, and the cyclic voltammetry curves at different scan rates and the relationship between the redox peak current density and the scan rate were obtained. The results are shown in Figure 5 .Depend on Figure 5 It can be seen that the linear relationship between the redox peak current density and the scan rate confirms that the redox process of the polymer is non-diffusion controlled.

[0069] 2. Spectroelectrochemical research

[0070] The prepared ITO conductive glass (50 mm long and 7 mm wide) with polymer film deposition was used as the working electrode, the platinum wire (1 mm in diameter) was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode. The electrolyte solution was 0.1 mol / L phosphorus hexafluoride tetrabutylamine acetonitrile solution, and the spectroelectrochemical curve was obtained as shown in Figure 6 As shown by Figure 6 It can be seen that in the neutral state, the polymer has an absorption peak at around 564nm, and the color of the neutral polymer is wine red; after the polymer is oxidized, the optical absorption at around 564nm weakens, the absorption in the near-infrared region increases, and the color of the oxidized polymer is light blue.

[0071] 3. Kinetics study

[0072] The ITO conductive glass (50 mm long and 7 mm wide) with polymer film deposited prepared in Examples 1-4 was used as the working electrode, the platinum wire (1 mm in diameter) was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode. The electrolyte solution was a 0.1 mol / L phosphorus hexafluoride tetrabutylamine acetonitrile solution, and the kinetic characteristics were characterized by the time-transmittance curve, see Figure 7 , the transmittance of the polymer film in different states was measured by a spectrophotometer, and the optical contrast and response time of the polymer were calculated, see Table 1.

[0073] Figure 8 Figure 7 is the time-transmittance curve for 10s, and the response time data is shown in Table 1.

[0074] Table 1

[0075]

[0076] As can be seen from Table 1, at 565nm, the response time of the oxidation process of poly(1,10) is 0.6s, and the response time of the reduction process is 0.5s; at 564nm, the response time of the oxidation process of poly(1,5) is 0.9s, and the response time of the reduction process is 2.0s; at 564nm, the response time of the oxidation process of poly(1,2) is 1s, and the response time of the reduction process is 2.9s; at 564nm, the response time of the oxidation process of poly(1,1) is 1.5s, and the response time of the reduction process is 5.9s, that is, poly(1,10) has the fastest response time, which indicates that in the concentrated copolymer, the doped ions can quickly migrate into the polymer film at this dosage ratio.

[0077] As can be seen from Table 1, the difference between the transmittance (oxidized state) and the transmittance (reduced state) of the electrochromic material prepared by the present invention is relatively large, the optical contrast can reach 70%, and the color change is obvious.

[0078] The performance of the materials prepared in the above comparative examples 1-4 was tested, and the results are shown in Table 2.

[0079] Table 2

[0080]

[0081] As shown in Table 2, in Comparative Example 1, ProDOT-Me was used for polymerization to obtain poly(ProDOT-Me), which also had good optical properties.

[0082] In Comparative Example 2, the ratio of c-EDT to ProDOT-Me was adjusted so that the amount of c-EDT far exceeded that of ProDOT-Me. The wavelength of the prepared poly(2,1) was 509 nm, the optical contrast was relatively small, and the response time of the reduction process was relatively long at 44 s. In Comparative Example 3, the optical contrast of PET-(1,9) was smaller than that of Example 1.

[0083] 4. Stability study

[0084] The ITO conductive glass (50 mm long and 7 mm wide) with polymer film deposited prepared in Examples 1-4 and Comparative Examples 1-2 was used as the working electrode, a platinum wire (1 mm in diameter) was used as the counter electrode, and an Ag / AgCl electrode was used as the reference electrode. The electrolyte solution was a 0.1 mol / L phosphorus hexafluoride tetrabutylamine acetonitrile solution, and the cyclic voltammetry curve was obtained as shown in FIG. Fig. 9 After 1000 cycles, poly(ProDOT-Me) maintained 71% of its activity; poly(1,10) in the present invention maintained 81% of its activity, an increase of 14%, that is, the material prepared in the present invention has higher stability.

[0085] In summary, the present invention utilizes c-EDT and ProDOT-Me and adjusts the usage ratio between the two to obtain electrochromic materials with different crosslinking densities. The crosslinked polythiophene derivative prepared by the present invention can achieve an optical contrast of 70%, a response time as low as 0.5 seconds, and high optical stability.

[0086] The above is a preferred embodiment of the present invention. For ordinary technicians in this technical field, making several improvements and modifications without departing from the principles of the present invention should also be regarded as within the protection scope of the present invention.

Claims

1. A method for preparing a cross-linked polythiophene derivative electrochromic material, characterized in that: include: (1) preparing c-EDT monomer; (2) c-EDT and 3,4-(2,2-dimethylpropylenedioxy)thiophene (ProDOT-Me) were dissolved in dichloromethane, and then a supporting electrolyte was added and mixed evenly; (3) Using platinum wire or ITO conductive glass as the working electrode, platinum wire as the counter electrode, and Ag / AgCl as the reference electrode, a constant potential method is used to electro-deposit at a potential of 1.8 V for 10 to 20 seconds to obtain an electrochromic material deposited on the surface of the working electrode.

2. The preparation method according to claim 1, characterized in that: The step (1) is specifically: (11) EDT-Cl, methacrylic acid, K2CO3 and KI were dissolved in dimethyl sulfoxide, reacted at 120°C for 4 hours, then extracted with dichloromethane, and purified by silica gel column to obtain light yellow crystalline EDT-c; the structural formula of the EDT-Cl is as follows: (12) ETD-c and azobisisobutyronitrile were dissolved in tetrahydrofuran, refluxed for 24 h, cooled to room temperature, and added with excess methanol to obtain a white solid, which was washed thoroughly with methanol and dried in vacuo to obtain c-EDT monomer.

3. The preparation method according to claim 2, characterized in that: In the step (2), the mass ratio of c-EDT to ProDOT-Me is 1:1-1:

10.

4. The preparation method according to claim 3, characterized in that: The mass ratio of c-EDT to ProDOT-Me is 1:

10.

5. The preparation method according to claim 4, characterized in that: The total concentration of c-EDT and ProDOT-Me is 1 to 3 g·L -1 .

6. The preparation method according to claim 5, characterized in that: The supporting electrolyte is tetrabutylammonium hexafluorophosphate (Bu4NPF6) with a concentration of 0.1-0.2 mol·L -1 .

7. A cross-linked polythiophene derivative electrochromic material, characterized in that: Prepared by any method of claims 1-6.