Full-biodegradable thermoplastic bamboo cellulose master batch and preparation method thereof
Through the esterification modification and melt extrusion process of bamboo cellulose, combined with modified nano-silica filler, the problem of poor water absorption and processability of bamboo cellulose during melt processing was solved, and a product with excellent water resistance was prepared. and biodegradable thermoplastic bamboo cellulose masterbatch, suitable for the preparation of plastic films.
Patent Information
- Application Number
- CN202410966884.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-01
AI Technical Summary
Bamboo cellulose has problems with strong water absorption and poor processability during melt processing, making it difficult to use in the preparation of plastic films.
Esterification modification of bamboo cellulose with urea, saturated fatty acid emulsion, 4-dimethylaminopyridine and N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride properties, forming saturated fatty acid esterified bamboo cellulose, and melting and extruding it with polyvinyl alcohol and glycerol in a torque rheometer to prepare thermoplastic bamboo cellulose masterbatch, adding modified nano-silica as a filler to improve water resistance properties and melt processability.
The biodegradability, water resistance and melt processability of bamboo cellulose are achieved, which can meet the melt processing process requirements of traditional plastic films, reduce the swelling rate and improve the performance of the material.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of plastic masterbatches, and more specifically, relates to a fully biodegradable thermoplastic bamboo cellulose masterbatch and a preparation method thereof. Background Art
[0002] Traditional non-biodegradable plastics have caused great harm to the environment. The use of fully biodegradable plastics is an effective way to solve the environmental hazards of non-biodegradable plastics. Bamboo has a fast growth cycle and the bamboo industry has negative carbon emissions. Therefore, bamboo cellulose is an ideal material for the preparation of fully biodegradable plastics. However, bamboo cellulose has poor melt processability and strong water absorption, which is not conducive to the melt processing of plastic films. Therefore, the development of fully biodegradable, melt-processable film-forming masterbatch is an effective way to achieve large-scale preparation of bamboo cellulose plastics. Summary of the invention
[0003] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.
[0004] In order to achieve these purposes and other advantages according to the present invention, a method for preparing a fully biodegradable thermoplastic bamboo cellulose masterbatch is provided, comprising the following steps:
[0005] Step 1, dispersing bamboo cellulose in water, adding urea, saturated fatty acid emulsion, 4-dimethylaminopyridine and N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride, reacting at a certain temperature for a certain time and then stopping the reaction, adding anhydrous ethanol in an equal volume to water to the reactant system to precipitate the reaction product, repeatedly washing the precipitate with anhydrous ethanol for several times, and obtaining saturated fatty acid esterified bamboo cellulose after drying;
[0006] Step 2: Add saturated fatty acid esterified bamboo cellulose, polyvinyl alcohol and glycerol into a torque rheometer at the same time, and prepare thermoplastic bamboo cellulose masterbatch by melt extrusion under certain temperature conditions.
[0007] Preferably, in the step 1, the saturated fatty acid emulsion is any one of gluconic acid emulsion, lauric acid emulsion and stearic acid emulsion or a mixture thereof.
[0008] Preferably, in the step 1, the method for preparing the saturated fatty acid emulsion is to heat the saturated fatty acid until it is completely melted, then add hot water, and stir to prepare the saturated fatty acid emulsion.
[0009] Preferably, the mixture comprises, by weight: 5 parts of saturated fatty acid and 95 parts of hot water.
[0010] Preferably, the temperature of the hot water is greater than 70°C.
[0011] Preferably, the stirring speed is 1000 to 3000 rpm, and the stirring time is 30 to 60 minutes.
[0012] Preferably, in step 1, the following components are included by weight: 5 to 10 parts of bamboo cellulose, 100 parts of water, 5 parts of urea, 10 parts of saturated fatty acid emulsion, 1 part of 4-dimethylaminopyridine and 1 part of N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride.
[0013] Preferably, in the step 1, the reaction temperature is 50-70° C. and the reaction time is 24-72 hours.
[0014] Preferably, in the step 2, the ingredients include, by weight: 100 parts of fatty acid esterified bamboo cellulose, 10 to 30 parts of polyvinyl alcohol and 10 to 20 parts of glycerol.
[0015] Preferably, in the step 2, the melt extrusion temperature is 100-130°C.
[0016] In order to improve the water resistance of the fully biodegradable thermoplastic bamboo cellulose masterbatch and reduce the swelling rate of the fully biodegradable thermoplastic bamboo cellulose masterbatch, in step 2, while adding saturated fatty acid esterified bamboo cellulose, polyvinyl alcohol and glycerol into the torque rheometer, modified nano silicon dioxide is added as filler, and the amount of modified nano silicon dioxide is 12-20% of the mass of saturated fatty acid esterified bamboo cellulose; the preparation method of modified nano silicon dioxide is:
[0017] S11, adding nano-silicon dioxide powder and polyvinyl pyrrolidone to deionized water, ultrasonically dispersing to obtain a nano-silicon dioxide suspension, ultrasonically dispersing for 1 to 2.5 hours, and the ultrasonic frequency is 60 to 120 kHz; wherein the mass volume ratio of the nano-silicon dioxide powder, polyvinyl pyrrolidone and deionized water is 10 to 20 g: 0.3 to 1 g: 100 to 300 mL;
[0018] S12. Dodecyltrimethoxysilane and 3-propyleneoxypropyltrimethoxysilane are mixed in a mass ratio of 1:2 to obtain a mixed modified liquid; the nano-silica suspension is stirred at a high speed of 2400-3600 rpm, and the mixed modified liquid is added dropwise to the nano-silica suspension while stirring, and the amount of the mixed modified liquid added is 5-10% of the nano-silica powder; after the addition is completed, the mixed system is rotated to a high-temperature and high-pressure reactor, pressurized to 2-6 MPa, heated to 110-160°C, and reacted for 2-4 hours; cooled to room temperature, and dried to obtain modified nano-silica.
[0019] The present invention has at least the following beneficial effects:
[0020] The present invention uses bamboo cellulose as a substrate, first esterifies bamboo cellulose, and realizes esterification modification of bamboo cellulose by long-chain alkanes in an aqueous environment to obtain saturated fatty acid esterified bamboo cellulose, and then mixes the saturated fatty acid esterified bamboo cellulose with polyvinyl alcohol and glycerol to prepare a fully biodegradable thermoplastic bamboo cellulose masterbatch. The problem that bamboo cellulose has strong water absorption and cannot be melt-processed is solved. The thermoplastic bamboo cellulose masterbatch prepared by the present invention can meet the melt processing technology of general plastic films, and has excellent water resistance, melt processing and biodegradability, and can be used in traditional plastic melt processing technology.
[0021] Among them, urea used for esterification modification of bamboo cellulose is used to expose more active groups of cellulose and destroy the strong hydrogen bonding between cellulose molecular chains; saturated fatty acid emulsion is used as a modifier to obtain saturated fatty acid esterified bamboo cellulose through esterification reaction between saturated fatty acid carboxyl (-COOH) and cellulose hydroxyl (-OH). The modified saturated fatty acid esterified bamboo cellulose, the long-chain alkane introduced by the saturated fatty acid can give the bamboo cellulose melt fluidity, that is, melt processability. 4-Dimethylaminopyridine and N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride are both catalysts for esterification reactions. Polyvinyl alcohol and glycerol are both plasticizers used to increase the toughness of thermoplastic bamboo cellulose masterbatch.
[0022] When preparing the fully biodegradable thermoplastic bamboo cellulose masterbatch, the present invention also uses modified nano silicon dioxide as a filler, firstly prepares the nano silicon dioxide into a uniformly dispersed suspension, then uses dodecyl trimethoxysilane and 3-propyleneoxypropyl trimethoxysilane under high pressure conditions, raises the temperature to 110-160° C. to hydrophobically modify the nano silicon dioxide; the hydrophobically modified modified nano silicon dioxide is used as a filler, and is melt-extruded together with saturated fatty acid esterified bamboo cellulose, polyvinyl alcohol and glycerol to obtain the fully biodegradable thermoplastic bamboo cellulose masterbatch, thereby further improving the water resistance of the fully biodegradable thermoplastic bamboo cellulose masterbatch and reducing the swelling rate of the fully biodegradable thermoplastic bamboo cellulose masterbatch.
[0023] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. DETAILED DESCRIPTION
[0024] The present invention is described in further detail below so that those skilled in the art can implement it according to the description.
[0025] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0026] Embodiment 1:
[0027] This embodiment provides a method for preparing a fully biodegradable thermoplastic bamboo cellulose masterbatch, comprising:
[0028] 5kg of bamboo cellulose was dispersed in 100kg of water, and 5kg of urea, 10kg of grape acid emulsion, 1kg of 4-dimethylaminopyridine and 1kg of N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride were added. The reaction was stopped after 48 hours at 60°C. The product was precipitated with 50% ethanol aqueous solution, washed repeatedly several times and dried to obtain saturated fatty acid esterified bamboo cellulose. 100kg of saturated fatty acid esterified bamboo cellulose, 10kg of polyvinyl alcohol and 20kg of glycerol were taken and added to the torque rheometer at the same time, and the thermoplastic cellulose masterbatch was prepared by melt extrusion at 110°C.
[0029] Wherein, the preparation method of saturated fatty acid emulsion is:
[0030] 5 kg of saturated fatty acid was heated until completely melted, and then 95 kg of hot water (temperature greater than 70° C.) was added, and the mixture was stirred at 3000 rpm for 60 minutes to prepare a saturated fatty acid emulsion.
[0031] Embodiment 2:
[0032] This embodiment provides a method for preparing a fully biodegradable thermoplastic bamboo cellulose masterbatch, comprising:
[0033] 5 kg of bamboo cellulose was dispersed in 100 kg of water, and 5 kg of urea, 10 kg of lauric acid emulsion, 1 kg of 4-dimethylaminopyridine and 1 kg of N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride were added. The reaction was stopped after 48 hours at 60°C. The product was precipitated with 50% ethanol aqueous solution, washed repeatedly several times and dried to obtain saturated fatty acid esterified bamboo cellulose. 100 kg of saturated fatty acid esterified bamboo cellulose, 10 kg of polyvinyl alcohol and 20 kg of glycerol were taken and added to the torque rheometer at the same time, and the thermoplastic cellulose masterbatch was prepared by melt extrusion at 120°C.
[0034] Embodiment 3:
[0035] This embodiment provides a method for preparing a fully biodegradable thermoplastic bamboo cellulose masterbatch, comprising:
[0036] 5kg of bamboo cellulose was dispersed in 100kg of water, and 5kg of urea, 10kg of stearic acid emulsion, 1kg of 4-dimethylaminopyridine and 1kg of N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride were added. The reaction was stopped after 48 hours at 60°C. The product was precipitated with 50% ethanol aqueous solution, washed repeatedly several times and dried to obtain saturated fatty acid esterified bamboo cellulose. 100kg of saturated fatty acid esterified bamboo cellulose, 10kg of polyvinyl alcohol and 20kg of glycerol were taken and added to the torque rheometer at the same time, and the thermoplastic cellulose masterbatch was prepared by melt extrusion at 130°C.
[0037] Embodiment 4:
[0038] This embodiment provides a method for preparing a fully biodegradable thermoplastic bamboo cellulose masterbatch, comprising:
[0039] 5kg of bamboo cellulose was dispersed in 100kg of water, and 5kg of urea, 10kg of lauric acid and stearic acid mixed emulsion, 1kg of 4-dimethylaminopyridine and 1kg of N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride were added. The reaction was stopped after 48 hours at 60°C. The product was precipitated with 50% ethanol aqueous solution, washed repeatedly several times and dried to obtain saturated fatty acid esterified bamboo cellulose. 100kg of saturated fatty acid esterified bamboo cellulose, 20kg of polyvinyl alcohol and 20kg of glycerol were taken and added to the torque rheometer at the same time, and the thermoplastic cellulose masterbatch was prepared by melt extrusion at 125°C.
[0040] Embodiment 5:
[0041] This embodiment provides a method for preparing a fully biodegradable thermoplastic bamboo cellulose masterbatch, comprising:
[0042] 5kg of bamboo cellulose was dispersed in 100kg of water, and 5kg of urea, 10kg of mixed emulsion of gluconic acid and stearic acid, 1kg of 4-dimethylaminopyridine and 1kg of N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride were added. The reaction was stopped after 48 hours at 60°C, and the product was precipitated with 50% ethanol aqueous solution, washed repeatedly several times, and dried to obtain saturated fatty acid esterified bamboo cellulose. 100kg of saturated fatty acid esterified bamboo cellulose, 20kg of polyvinyl alcohol and 10kg of glycerol were taken and added to the torque rheometer at the same time, and melt extruded at 120°C to obtain thermoplastic cellulose masterbatch.
[0043] Example 6
[0044] This embodiment provides a method for preparing a fully biodegradable thermoplastic bamboo cellulose masterbatch. Compared with Example 2, 100 kg of saturated fatty acid esterified bamboo cellulose, 10 kg of polyvinyl alcohol and 20 kg of glycerol are taken and added to the torque rheometer at the same time, and modified nano silicon dioxide is also added thereto as a filler. The rest of the preparation method and process parameters are the same as those in Example 2; the amount of modified nano silicon dioxide is 12 kg; the preparation method of modified nano silicon dioxide is:
[0045] S11, adding 15 kg of nano-silicon dioxide powder and 0.3 kg of polyvinyl pyrrolidone into 100 L of deionized water, and performing ultrasonic dispersion to obtain a nano-silicon dioxide suspension, and performing ultrasonic dispersion for 1 h at an ultrasonic frequency of 60 kHz;
[0046] S12, 0.3 kg of dodecyltrimethoxysilane and 0.6 kg of 3-propyleneoxypropyltrimethoxysilane are mixed to obtain a mixed modified liquid; the nano-silica suspension is stirred at a high speed of 2400 rpm, and the mixed modified liquid is added dropwise to the nano-silica suspension while stirring; after the addition is completed, the mixed system is rotated to a high-temperature and high-pressure reactor, pressurized to 3 MPa, heated to 110°C, and reacted for 4 hours; cooled to room temperature, and dried to obtain modified nano-silica.
[0047] Example 7
[0048] This embodiment provides a method for preparing a fully biodegradable thermoplastic bamboo cellulose masterbatch. Compared with Example 2, 100 kg of saturated fatty acid esterified bamboo cellulose, 10 kg of polyvinyl alcohol and 20 kg of glycerol are taken and added to the torque rheometer at the same time, and modified nano silicon dioxide is also added thereto as a filler. The rest of the preparation method and process parameters are the same as those in Example 2; the amount of modified nano silicon dioxide is 15 kg; the preparation method of modified nano silicon dioxide is:
[0049] S11, adding 20 kg of nano silicon dioxide powder and 0.6 kg of polyvinyl pyrrolidone into 120 L of deionized water, and performing ultrasonic dispersion to obtain a nano silicon dioxide suspension, and performing ultrasonic dispersion for 2.5 h at an ultrasonic frequency of 120 kHz;
[0050] S12, 0.6 kg of dodecyltrimethoxysilane and 1.2 kg of 3-propyleneoxypropyltrimethoxysilane are mixed to obtain a mixed modified liquid; the nano-silica suspension is stirred at a high speed of 3600 rpm, and the mixed modified liquid is added dropwise to the nano-silica suspension while stirring; after the dropwise addition is completed, the mixed system is rotated to a high-temperature and high-pressure reactor, pressurized to 4 MPa, heated to 130°C, and reacted for 3 hours; cooled to room temperature, and dried to obtain modified nano-silica.
[0051] Comparative Example 1
[0052] This comparative example provides a method for preparing a fully biodegradable thermoplastic bamboo cellulose masterbatch. Compared with the example, when 100 kg of saturated fatty acid esterified bamboo cellulose, 10 kg of polyvinyl alcohol and 20 kg of glycerol are added to a torque rheometer at the same time, 12 kg of nano-silicon dioxide is also added thereto as a filler, and the rest of the preparation method and process parameters are the same as those in Example 2.
[0053] Comparative Example 2
[0054] This comparative example provides a method for preparing a fully biodegradable thermoplastic bamboo cellulose masterbatch. Compared with the example, when 100 kg of saturated fatty acid esterified bamboo cellulose, 10 kg of polyvinyl alcohol and 20 kg of glycerol are added to a torque rheometer at the same time, 15 kg of nano-silicon dioxide is also added thereto as a filler, and the rest of the preparation method and process parameters are the same as those in Example 2.
[0055] The fully biodegradable thermoplastic bamboo cellulose masterbatch prepared in Examples 1 to 7 and Comparative Examples 1 and 2 was subjected to water swelling resistance test, melting temperature test and full biodegradability test. The test results are shown in the following table:
[0056] sample Swelling rate (%) Melting temperature(℃) Total biodegradation cycle (days) Example 1 2.02±0.02 111 93 Example 2 1.87±0.02 121 98 Example 3 2.01±0.01 127 100 Example 4 2.12±0.01 122 102 Example 5 1.98±0.02 118 105 Example 6 1.66±0.01 124 101 Example 7 1.61±0.01 122 103 Comparative Example 1 2.04±0.02 126 105 Comparative Example 2 2.00±0.01 129 106
[0057] It can be seen from the above table that the fully biodegradable thermoplastic bamboo cellulose masterbatch prepared in the above examples has excellent water resistance, melt processability and fully biodegradable performance, and can be used in traditional plastic melt processing technology to prepare the production of fully biodegradable plastic film.
[0058] At the same time, compared with the technical solutions of Examples 1 to 5, Examples 6 and 7 use hydrophobically modified modified nano-silicon dioxide as filler, which further improves the water resistance of the fully biodegradable thermoplastic bamboo cellulose masterbatch and reduces the swelling rate of the fully biodegradable thermoplastic bamboo cellulose masterbatch. Comparative Examples 1 and 2 use unmodified nano-silicon dioxide as filler, and the prepared fully biodegradable thermoplastic bamboo cellulose masterbatch has similar water resistance, melt processing performance and fully biodegradable performance as Examples 1 to 5; but the swelling rate of the fully biodegradable thermoplastic bamboo cellulose masterbatch prepared by Comparative Examples 1 and 2 is higher than that of Example 2, and significantly lower than that of Examples 6 and 7, indicating that compared with unmodified nano-silicon dioxide, the swelling rate of the fully biodegradable thermoplastic bamboo fiber masterbatch prepared by using hydrophobically modified nano-silicon dioxide as filler has been significantly reduced.
[0059] The number of devices and processing scales described here are used to simplify the description of the present invention. Applications, modifications and variations of the present invention will be obvious to those skilled in the art.
[0060] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the examples shown and described herein.
Claims
1. A method for preparing a fully biodegradable thermoplastic bamboo cellulose masterbatch, characterized in that: The following steps are involved: Step 1, dispersing bamboo cellulose in water, adding urea, saturated fatty acid emulsion, 4-dimethylaminopyridine and N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride, reacting at a certain temperature for a certain time and then stopping the reaction, adding anhydrous ethanol in an equal volume to water to the reactant system to precipitate the reaction product, repeatedly washing the precipitate with anhydrous ethanol for several times, and obtaining saturated fatty acid esterified bamboo cellulose after drying; Step 2: Add saturated fatty acid esterified bamboo cellulose, polyvinyl alcohol and glycerol into a torque rheometer at the same time, and prepare thermoplastic bamboo cellulose masterbatch by melt extrusion under certain temperature conditions.
2. The method for preparing the fully biodegradable thermoplastic bamboo cellulose masterbatch according to claim 1, characterized in that: In the step 1, the saturated fatty acid emulsion is any one of gluconic acid emulsion, lauric acid emulsion and stearic acid emulsion or a mixture thereof.
3. The method for preparing the fully biodegradable thermoplastic bamboo cellulose masterbatch according to claim 1, characterized in that: In the step 1, the method for preparing the saturated fatty acid emulsion is to heat the saturated fatty acid until it is completely melted, then add hot water, and stir to prepare the saturated fatty acid emulsion.
4. The method for preparing the fully biodegradable thermoplastic bamboo cellulose masterbatch according to claim 3, characterized in that: By weight, it comprises: 5 parts of saturated fatty acid and 95 parts of hot water.
5. The method for preparing the fully biodegradable thermoplastic bamboo cellulose masterbatch according to claim 3, characterized in that: The temperature of the hot water is greater than 70°C.
6. The method for preparing the fully biodegradable thermoplastic bamboo cellulose masterbatch according to claim 3, characterized in that: The stirring speed is 1000 to 3000 rpm, and the stirring time is 30 to 60 minutes.
7. The method for preparing the fully biodegradable thermoplastic bamboo cellulose masterbatch according to claim 1, characterized in that: In the step 1, the following are included by weight: 5 to 10 parts of bamboo cellulose, 100 parts of water, 5 parts of urea, 10 parts of saturated fatty acid emulsion, 1 part of 4-dimethylaminopyridine and 1 part of N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride.
8. The method for preparing the fully biodegradable thermoplastic bamboo cellulose masterbatch according to claim 1, characterized in that: In the step 1, the reaction temperature is 50-70° C. and the reaction time is 24-72 hours.
9. The method for preparing the fully biodegradable thermoplastic bamboo cellulose masterbatch according to claim 1, characterized in that: In the step 2, the following are included by weight: 100 parts of fatty acid esterified bamboo cellulose, 10 to 30 parts of polyvinyl alcohol and 10 to 20 parts of glycerol.
10. The method for preparing the fully biodegradable thermoplastic bamboo cellulose masterbatch according to claim 1, characterized in that: In the step 2, the melt extrusion temperature is 100-130°C.