Lower-layer tread rubber with low rolling resistance coefficient, preparation method of lower-layer tread rubber, tire and rolling resistance coefficient evaluation method
By using ultra-high amounts of silica black and silane coupling agent in the lower tread compound, combined with new carbon black and anti-vulcanization reversion agent, the lower tread compound with a low rolling resistance coefficient is designed and evaluated using the tanδ/G'2 value This method solves the problem of performance loss of the lower tread rubber when reducing rolling resistance, and achieves the simultaneous effect of reducing rolling resistance and improving performance.
Patent Information
- Application Number
- CN202410967919.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-01
AI Technical Summary
When the rolling resistance coefficient of the existing tread lower layer is reduced, the elongation product and tear strength are reduced, which affects the performance. Moreover, the traditional evaluation method is not highly correlated with the rolling resistance coefficient of the finished tire, making it difficult to accurately guide formula design.
Using a combination of ultra-high amounts of silica and silane coupling agent, combined with new low-hysteresis high-reinforcement carbon black and anti-vulcanization reversion agent, the lower tread rubber with low rolling resistance coefficient is designed, and passed the tanδ/G'2 value evaluation method Improve the correlation between the hysteresis performance of the semi-finished rubber compound and the rolling resistance coefficient of the finished tire.
The rolling resistance coefficient of the tire is reduced by about 5%, while maintaining the tensile strength product greater than 14,000 and the tear strength greater than 110. It does not affect other performance, reduces the heat generated by the tire during operation, and improves the service life.
Smart Images

Figure CN118725424A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of tires, and in particular to a low rolling resistance coefficient lower tread rubber and a preparation method thereof, a tire and a rolling resistance coefficient evaluation method. Background Art
[0002] The domestic and international markets have lower and lower requirements for the rolling resistance coefficient of tires. Since the tread rubber has a large impact on rolling resistance, between 30% and 50%, the early research on materials for reducing rolling resistance of tires focused on the tread formulation, especially the tread upper layer rubber formulation, which accounts for a higher proportion. However, the tread upper layer rubber also bears the performance of wear, grip, and cut resistance. Excessive reduction of its rolling resistance coefficient may lead to the loss of other properties. On the contrary, compared with the tread upper layer rubber, the tread lower layer rubber is less restricted and there is still a lot of room for exploration.
[0003] However, when the rolling resistance coefficient of the current tread rubber is reduced, the strength-extension product and tear strength are also reduced accordingly, thus affecting its performance; in addition, in the traditional evaluation of the hysteresis performance of rubber, the tanδ of the DMA test is mainly used, supplemented by compression heat generation or rebound. However, in actual research and application, it is found that these evaluation methods are not highly correlated with the rolling resistance coefficient of the finished tire in the improvement of the tread rubber, and it is difficult to accurately guide the formulation design. Summary of the invention
[0004] In view of this, the present invention proposes a lower tread rubber with a low rolling resistance coefficient and a preparation method thereof, a tire and a rolling resistance coefficient evaluation method to solve the technical defects existing in the prior art.
[0005] In a first aspect, the present invention provides a low rolling resistance coefficient lower tread rubber, comprising the following components in parts by weight:
[0006] 100 parts of natural rubber, 5-20 parts of carbon black, 30-45 parts of white carbon black, 3-4 parts of zinc oxide, 1-3 parts of stearic acid, 2-4 parts of antioxidant, 3.95-5.1 parts of silane coupling agent, 0.5-2.3 parts of accelerator, 0.5-1 part of anti-reversion agent, 0.5-1 part of sulfur.
[0007] Preferably, the antioxidant includes antioxidant RD and / or antioxidant 6PPD.
[0008] Preferably, the silane coupling agent includes Si75 and / or Si69;
[0009] And / or, the accelerator includes accelerator D and / or accelerator NS;
[0010] And / or, the anti-reversion agent is 1,6-bis(N,N-dibenzothiazolecarbamoyl disulfide)-hexane.
[0011] Preferably, the following components are included in weight:
[0012] 100 parts of natural rubber, 5-20 parts of carbon black, 30-45 parts of white carbon black, 3.5 parts of zinc oxide, 2 parts of stearic acid, 3 parts of antioxidant, 3.95-5.1 parts of silane coupling agent, 0.5 parts of accelerator D, 0.5-1 parts of anti-reversion agent, 1.3-1.8 parts of sulfur, and 1.3-1.8 parts of accelerator NS.
[0013] In a second aspect, the present invention further provides a method for preparing the low rolling resistance coefficient lower tread rubber, comprising the following steps:
[0014] Add natural rubber into a meshing internal mixer, mix, then add accelerator D, white carbon black, and silane coupling agent, continue mixing, and then discharge the rubber to obtain a masterbatch;
[0015] Adding a first-stage masterbatch, carbon black, antioxidant, zinc oxide and stearic acid into an intermeshing internal mixer, mixing, lifting the plug, and then pressing the plug, mixing and discharging the glue to obtain a second-stage masterbatch;
[0016] Add the second-stage masterbatch into the intermeshing internal mixer, mix, then add sulfur, accelerator NS, anti-vulcanization reversion agent, continue mixing, lift the plug, then press the plug, mix and discharge the rubber to obtain the final mixed rubber, which is the lower tread rubber.
[0017] Preferably, the method for preparing the lower tread rubber with low rolling resistance coefficient comprises the following steps:
[0018] Add natural rubber to an intermeshing internal mixer, set the mixer speed to 40-50 rpm, mix for 20-30 seconds, then add accelerator D, white carbon black, and silane coupling agent, continue mixing until the temperature reaches 140-160°C, and then discharge the rubber to obtain a masterbatch;
[0019] Add the first-stage masterbatch, carbon black, antioxidant, zinc oxide and stearic acid into the intermeshing internal mixer, set the internal mixer speed to 40-50 rpm, mix for 120-140 seconds, lift the plug, keep for 15-25 seconds, then press the plug and mix to 140-160°C, then discharge the glue to obtain the second-stage masterbatch;
[0020] Add the second-stage masterbatch into the intermeshing internal mixer, set the mixer speed to 25-35 rpm, mix for 60-70 seconds, then add sulfur, accelerator NS, and anti-vulcanization reversion agent, continue mixing for 130-140 seconds, lift the plug, then press the plug and mix to 100-120°C before discharging the rubber to obtain the final mixed rubber, which is the lower tread rubber.
[0021] In a third aspect, the present invention further provides a method for preparing the low rolling resistance coefficient lower tread rubber, comprising the following steps:
[0022] Add natural rubber into a meshing internal mixer, mix, then add accelerator D, white carbon black, and silane coupling agent, continue mixing, and then discharge the rubber to obtain a masterbatch;
[0023] Add a section of masterbatch, carbon black, antioxidant, zinc oxide and stearic acid into a meshing internal mixer, mix, lift the plug, then press the plug. After mixing, discharge the rubber onto an open mixer, turn over, add sulfur, accelerator NS and anti-vulcanization reversion agent, then turn over thinly, cool the lower sheet to room temperature, and obtain the lower tread rubber.
[0024] Preferably, the method for preparing the lower tread rubber with low rolling resistance coefficient comprises the following steps:
[0025] Add natural rubber to an intermeshing internal mixer, set the mixer speed to 40-50 rpm, mix for 20-30 seconds, then add accelerator D, white carbon black, and silane coupling agent, continue mixing until the temperature reaches 140-160°C, and then discharge the rubber to obtain a masterbatch;
[0026] Add a masterbatch, carbon black, antioxidant, zinc oxide and stearic acid into a meshing internal mixer, set the mixer speed to 40-50 rpm, mix for 120-140 s, lift the plug, hold for 15-25 s, then press the plug and mix to 140-160 ℃, then discharge the rubber onto an open mixer, refining and cooling to 90-100 ℃, adding sulfur, accelerator NS and anti-vulcanization reversion agent, and then thin-pass refining for 280-320 s. Cool the lower sheet to room temperature to obtain the lower tread rubber.
[0027] In a fourth aspect, the present invention further provides a tire, which is prepared using the low rolling resistance coefficient lower tread rubber described above or the low rolling resistance coefficient lower tread rubber prepared by the preparation method described above.
[0028] In a fifth aspect, the present invention further provides a method for evaluating the rolling resistance coefficient of a tire, comprising the following steps:
[0029] Providing the low rolling resistance coefficient lower tread rubber or the low rolling resistance coefficient lower tread rubber prepared by the preparation method;
[0030] Testing the storage modulus G' and loss modulus G" of the lower tread rubber;
[0031] Calculate the tanδ value, wherein tanδ=G" / G';
[0032] Calculation of tanδ / G' 2 value;
[0033] tanδ / G' 2The value is linearly related to the rolling resistance coefficient of the tire, which can be calculated using tanδ / G' 2 The value predicts the rolling resistance coefficient of the tire.
[0034] The low rolling resistance coefficient lower tread rubber and its preparation method, tire and rolling resistance coefficient evaluation method of the present invention have the following beneficial effects compared with the prior art:
[0035] 1. The low rolling resistance coefficient lower tread rubber of the present invention breaks through the design concept of traditional natural rubber formula and adopts a combination of ultra-high amount of white carbon black and silane coupling agent to achieve simultaneous improvement of high reinforcement and low heat generation performance; new materials, new low hysteresis and high reinforcement MH363 carbon black and 1,6-bis(N,N-dibenzothiazolecarbamoyl disulfide)-hexane are used to further reduce the hysteresis performance of the rubber material, while ensuring other physical properties such as strong tear; the low rolling resistance coefficient lower tread rubber of the present invention can reduce the rolling resistance coefficient of the tire by about 5%, while the strength-elongation product is greater than 14000 and the tear strength is greater than 110, so that it not only does not affect other performance characteristics, but also can reduce the heat generated by the tire during operation and increase the service life of the tire.
[0036] 2. The present invention studies the stress and deformation mechanism of the crown rubber during tire operation and deduces the factors that affect the hysteresis of the lower tread rubber. The factors are not only related to the traditional indicators of rubber hysteresis performance such as tanδ, compression heat generation or rebound, but also have a great relationship with the stiffness of the rubber. Based on this, combined with product development and verification, an evaluation method with a higher correlation with the rolling resistance coefficient of the finished tire is explored - tanδ / G' 2 The present invention aims at reducing the rolling resistance coefficient of the tire and the evaluation method of the hysteresis performance of the lower layer rubber of the tread, thereby improving the correlation between the hysteresis performance of the semi-finished rubber product and the rolling resistance coefficient of the finished tire. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the prior art descriptions. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0038] Figure 1 It is the linear relationship diagram between tanδ and the rolling resistance coefficient of the tire;
[0039] Figure 2 is tanδ / G' 2 Linear relationship diagram with the rolling resistance coefficient of the tire. DETAILED DESCRIPTION
[0040] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] The present application provides a low rolling resistance coefficient lower tread rubber, comprising the following components in parts by weight:
[0042] 100 parts of natural rubber, 5-20 parts of carbon black, 30-45 parts of white carbon black, 3-4 parts of zinc oxide, 1-3 parts of stearic acid, 2-4 parts of antioxidant, 3.95-5.1 parts of silane coupling agent, 0.5-2.3 parts of accelerator, 0.5-1 part of anti-reversion agent, and 1.3-1.8 parts of sulfur.
[0043] In some embodiments, the antioxidant includes antioxidant RD and / or antioxidant 6PPD.
[0044] Specifically, antioxidant RD, also known as antioxidant RD, antioxidant 224, has a molecular formula of C 12 H 17 N; Antioxidant 6PPD, namely N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, molecular formula: C 18 H 24 N2.
[0045] In some embodiments, the silane coupling agent includes Si75 and / or Si69; specifically, Si75 bis-[γ-(triethoxysilyl)propyl]-disulfide (Si75); silane coupling agent Si-69, chemically named bis-[γ-(triethoxysilyl)propyl]tetrasulfide.
[0046] In some embodiments, the promoter includes promoter D and / or promoter NS; promoter D, also known as diphenylguanidine, has a molecular formula of C 13 H 13 N3; Accelerator NS, chemical name: N-tert-butyl-2-benzothiazole xanthamide, molecular formula C 11 H 14 N2S2.
[0047] In some embodiments, the anti-reversion agent is 1,6-bis(N,N-dibenzothiazolecarbamoyl disulfide)-hexane.
[0048] In some embodiments, the natural rubber is natural rubber NR10, i.e., 10# standard natural rubber; the carbon black includes carbon black N375 and / or carbon black MH363; the carbon black MH363 is a new type of low hysteresis and high reinforcement MH363 carbon black (iodine absorption value: 63-73 mg / g; DBP absorption value: 131-141 ml / 100 g, purchased from Jiangxi Black Cat Carbon Black Co., Ltd.); the carbon black N375 is black cat carbon black N375, purchased from Jiangxi Black Cat Carbon Black Co., Ltd.; the white carbon black is white carbon black VN3, i.e., Degussa VN3 precipitated silica.
[0049] In some embodiments, the low rolling resistance coefficient lower tread rubber comprises the following components in parts by weight:
[0050] 100 parts of natural rubber, 5-20 parts of carbon black, 30-45 parts of white carbon black, 3.5 parts of zinc oxide, 2 parts of stearic acid, 3 parts of antioxidant, 3.95-5.1 parts of silane coupling agent, 0.5 parts of accelerator D, 0.5-1 parts of anti-reversion agent, 1.3-1.8 parts of sulfur, and 1.3-1.8 parts of accelerator NS.
[0051] The low rolling resistance coefficient lower tread rubber of the present invention breaks through the design concept of traditional natural rubber formula, adopts a combination of ultra-high amount of white carbon black and silane coupling agent to achieve simultaneous improvement of high reinforcement and low heat generation performance; new materials, new low hysteresis and high reinforcement MH363 carbon black and 1,6-bis(N,N-dibenzothiazolecarbamoyl disulfide)-hexane are adopted to further reduce the hysteresis performance of the rubber material, while ensuring other physical properties such as strong tear; the low rolling resistance coefficient lower tread rubber of the present invention can reduce the rolling resistance coefficient of the tire by about 5%, while the strength-elongation product is greater than 14000 and the tear strength is greater than 110, so that it not only does not affect other use performance, but also can reduce the heat generated by the tire during operation and increase the service life of the tire.
[0052] Based on the same inventive concept, the present invention also provides a method for preparing the above-mentioned lower tread rubber with a low rolling resistance coefficient, comprising the following steps:
[0053] S1. Add natural rubber into an intermeshing internal mixer, mix, then add accelerator D, white carbon black, and silane coupling agent, continue mixing, and then discharge the rubber to obtain a masterbatch;
[0054] S2, adding a first-stage masterbatch, carbon black, antioxidant, zinc oxide, and stearic acid into an intermeshing internal mixer, mixing, lifting the plug, and then pressing the plug, mixing, and then discharging the glue to obtain a second-stage masterbatch;
[0055] S3. Add the second-stage masterbatch into the intermeshing internal mixer, mix, then add sulfur, accelerator NS, anti-vulcanization reversion agent, continue to mix, lift the plug, then press the plug, mix and discharge the rubber to obtain the final rubber, which is the lower tread rubber.
[0056] In some embodiments, a method for preparing a lower tread rubber layer with a low rolling resistance coefficient comprises the following steps:
[0057] S1. Add natural rubber to an intermeshing internal mixer, set the mixer speed to 40-50 rpm, mix for 20-30 seconds, then add accelerator D, white carbon black, and silane coupling agent, continue mixing until the temperature reaches 140-160°C, and then discharge the rubber to obtain a masterbatch;
[0058] S2, add a first-stage masterbatch, carbon black, antioxidant, zinc oxide, and stearic acid into an intermeshing internal mixer, set the mixer speed to 40-50 rpm, mix for 120-140 seconds, lift the plug, hold for 15-25 seconds, then press the plug and mix to 140-160°C before discharging the glue to obtain a second-stage masterbatch;
[0059] S3. Add the second-stage masterbatch into the intermeshing internal mixer, set the mixer speed to 25-35 rpm, mix for 60-70 seconds, then add sulfur, accelerator NS, and anti-vulcanization reversion agent, continue mixing for 130-140 seconds, lift the plug, then press the plug and mix to 100-120°C, then discharge the rubber to obtain the final mixed rubber, which is the lower tread rubber.
[0060] Based on the same inventive concept, the present invention also provides a method for preparing the above-mentioned lower tread rubber with a low rolling resistance coefficient, comprising the following steps:
[0061] S1. Add natural rubber into an intermeshing internal mixer, mix, then add accelerator D, white carbon black, and silane coupling agent, continue mixing, and then discharge the rubber to obtain a masterbatch;
[0062] S2. Add a masterbatch, carbon black, antioxidant, zinc oxide and stearic acid into a meshing internal mixer, mix, lift the plug, and then press the plug. After mixing, discharge the rubber onto an open mixer, turn over, add sulfur, accelerator NS and anti-vulcanization reversion agent, and then turn over thinly. Cool the lower sheet to room temperature to obtain the lower tread rubber.
[0063] In some embodiments, a method for preparing a lower tread rubber layer with a low rolling resistance coefficient comprises the following steps:
[0064] S1. Add natural rubber to an intermeshing internal mixer, set the mixer speed to 40-50 rpm, mix for 20-30 seconds, then add accelerator D, white carbon black, and silane coupling agent, continue mixing until the temperature reaches 140-160°C, and then discharge the rubber to obtain a masterbatch;
[0065] S2. Add a masterbatch, carbon black, antioxidant, zinc oxide and stearic acid into a meshing internal mixer, set the mixer speed to 40-50 rpm, mix for 120-140 seconds, lift the plug, hold for 15-25 seconds, then press the plug and mix to 140-160°C, then discharge the rubber onto an open mixer, reheat and cool to 90-100°C, add sulfur, accelerator NS and anti-vulcanization reversion agent, then reheat for 280-320 seconds, cool the lower sheet to room temperature, and the lower tread rubber is obtained.
[0066] Based on the same inventive concept, the present invention also provides a tire, which is prepared using the above-mentioned low rolling resistance coefficient lower tread rubber or the low rolling resistance coefficient lower tread rubber prepared by the above-mentioned preparation method.
[0067] Based on the same inventive concept, the present invention also provides a method for evaluating a rolling resistance coefficient of a tire, comprising the following steps:
[0068] S1. providing the above-mentioned lower tread rubber with low rolling resistance coefficient or the lower tread rubber with low rolling resistance coefficient prepared by the above-mentioned preparation method;
[0069] S2. Test the storage modulus G' and loss modulus G" of the lower tread rubber;
[0070] S3. Calculate the tanδ value, tanδ=G" / G';
[0071] S4. Calculation of tanδ / G' 2 value;
[0072] S5, tanδ / G' 2 The value is linearly related to the rolling resistance coefficient of the tire in the absence of other variables, which can be calculated using tanδ / G' 2 The value predicts the rolling resistance coefficient of the tire.
[0073] In some embodiments, the rolling resistance coefficient of the tire is y, y = 8077.7x + 3.6533, where x = tan δ / G' 2 .
[0074] Specifically, the storage modulus G' and loss modulus G", are tested by DMA (Dynamic mechanical analysis), and the test conditions are: test shear mode: strain: 0.25%, frequency: 10HZ, temperature: 30-100°C, heating rate: 2°C / min; the temperature of G' and G" is 60°C;
[0075] The present invention studies the stress and deformation mechanism of the crown rubber during tire operation and deduces the factors that affect the hysteresis of the lower tread rubber. The factors are not only related to the traditional indicators of rubber hysteresis performance such as tanδ, compression heat generation or rebound, but also have a great relationship with the stiffness of the rubber. Based on this, combined with product development and verification, an evaluation method with a higher correlation with the rolling resistance coefficient of the finished tire is explored - tanδ / G' 2 ;
[0076] The present invention aims at reducing the rolling resistance coefficient of a tire and the evaluation method of the hysteresis performance of the rubber under the tread, and improves the correlation between the hysteresis performance of the semi-finished rubber product and the rolling resistance coefficient of the finished tire.
[0077] The following further describes the low rolling resistance coefficient lower tread rubber of the present application and its preparation method with specific examples. This section further describes the content of the present invention in conjunction with specific examples, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0078] Table 1 below provides the formulations of the lower tread rubber with low rolling resistance coefficient shown in Examples 1 to 5 and Comparative Example 1. The formulation data in Table 1 are all in parts by weight.
[0079] Table 1 - Low rolling resistance coefficient lower tread rubber formulations of different embodiments
[0080]
[0081]
[0082] Among them, the natural rubber in Table 1 is natural rubber NR10, that is, 10# standard natural rubber; white carbon black is white carbon black VN3; the antioxidant is a combination of antioxidant RD and antioxidant 6PPD, and the mass ratio of antioxidant RD to antioxidant 6PPD is 1:1; the silane coupling agent is silane coupling agent Si75; the anti-reversion agent is 1,6-bis(N,N-dibenzothiazolecarbamoyl disulfide)-hexane; the mass ratio of antioxidant RD to antioxidant 6PPD is 1:1; zinc oxide, stearic acid, accelerator D, sulfur, and accelerator NS are all conventional market products.
[0083] The method for preparing the above-mentioned lower tread rubber with low rolling resistance coefficient comprises the following steps:
[0084] S1. Add natural rubber to an intermeshing internal mixer, set the mixer speed to 40 rpm, mix for 25 seconds, then add accelerator D, white carbon black, and silane coupling agent, continue mixing to 150°C, and then discharge the rubber to obtain a masterbatch;
[0085] S2, add the first stage masterbatch, carbon black, antioxidant, zinc oxide and stearic acid into the intermeshing internal mixer, set the speed of the internal mixer to 45 rpm, mix for 130 seconds, lift the plug, hold for 20 seconds, then press the plug and mix to 150°C and then discharge the glue to obtain the second stage masterbatch;
[0086] S3. Add the second-stage masterbatch into the intermeshing internal mixer, set the mixer speed to 30 rpm, mix for 65 seconds, then add sulfur, accelerator NS, and anti-vulcanization reversion agent, continue mixing for 135 seconds, lift the plug, then press the plug and mix to 110°C, then discharge the rubber to obtain the final mixed rubber, which is the lower tread rubber.
[0087] The performance of the lower tread rubber formulations in the above Examples 1 to 5 and Comparative Example 1 was tested, and the results are shown in Table 2 below.
[0088] Table 2 - Performance of the low rolling resistance coefficient lower tread rubber formulations of different embodiments
[0089]
[0090]
[0091] Note: 1. Curing conditions: 151℃×20min; different lower tread rubbers are cured at 151℃ for 20min before corresponding performance tests.
[0092] 2. G' and G" were tested by DMA (Dynamic mechanical analysis), and the test conditions were as follows: test shear mode: strain: 0.25%, frequency: 10HZ, temperature: 30-100℃, heating rate: 2℃ / min; the temperature of G' and G" was 60℃;
[0093] 3. Other performance test methods: Rebound resilience is tested according to GB / T1681; bottom and middle heat generation is tested according to GB / T1687.3; hardness is tested according to GB / T531.1; 100%, 300% elongation, tensile strength and elongation at break are tested according to GB / T528; tearing is tested according to GB / T529; Mooney viscosity is tested according to GB / T1232.1;
[0094] 4. Strength-extension product is the product of tensile strength and elongation at break;
[0095] Comparative Example 1 is a conventional TBR tire tread lower layer rubber formula.
[0096] From Examples 1 to 6, it can be seen that Tanδ / G', which characterizes the heat generation hysteresis performance, 2 , resilience, bottom heat generation, and middle heat generation are all better than those in comparative example 1, but Tanδ is not necessarily the case;
[0097] It can be seen from Examples 1 to 6 that the strength-elongation products are all greater than 14,000, which is close to that of Comparative Example 1;
[0098] It can be seen from Examples 1 to 6 that the tear strength is greater than 110, which is slightly better than Comparative Example 1.
[0099] Furthermore, the lower tread rubber formulations in Example 2 and Comparative Example 1 were selected to produce tires with other components unchanged, and the tire indoor rolling resistance test was carried out (tested according to GB / T29040-2012). The rolling resistance coefficient was reduced by 5.65% compared with that of Comparative Example 1. The detailed results are shown in Table 3 below.
[0100] Table 3 - Indoor rolling resistance test results
[0101]
[0102]
[0103] In the above Table 3, three tires were prepared using Comparative Example 1 as the lower tread rubber, and the rolling resistance coefficients of the tested tires were 4.65, 4.60, and 4.56, respectively, while the rolling resistance coefficients of the tires prepared using Example 2 as the lower tread rubber were 4.38, 4.32, and 4.33. Compared with Comparative Example 1, the rolling resistance coefficient of the tire decreased by 5.65%.
[0104] After years of research on rolling resistance, the applicant found that the correlation between tanδ of the lower tread rubber and the rolling resistance coefficient of the tire is not good. In order to conduct in-depth research, a series of tests were conducted and the following conclusions were found:
[0105] 1. The tanδ of the lower tread rubber has a poor correlation with the rolling resistance coefficient of the tire. The specific data is shown in the figure below. Figure 1 shown.
[0106] 2. After trying and analyzing various combinations, it was found that the rolling resistance coefficient of the tire is related to the tanδ / G' of the lower tread rubber. 2 The correlation is very high, the specific data is as follows Figure 2 shown.
[0107] from Figure 2 It can be seen that the rolling resistance coefficient of the tire is y, y = 8077.7x + 3.6533, where x = tanδ / G' 2 , there is a linear relationship between y and x, and the correlation coefficient is R 2 =0.9181, much higher than the correlation coefficient R using tanδ 2 =0.5911.
[0108] The above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A low rolling resistance coefficient lower tread rubber, It is characterized in that It comprises the following components in parts by weight: 100 parts of natural rubber, 5-20 parts of carbon black, 30-45 parts of white carbon black, 3-4 parts of zinc oxide, 1-3 parts of stearic acid, 2-4 parts of antioxidant, 3.95-5.1 parts of silane coupling agent, 0.5-2.3 parts of accelerator, 0.5-1 part of anti-reversion agent, and 1.3-1.8 parts of sulfur.
2. The low rolling resistance coefficient lower tread rubber according to claim 1, It is characterized in that The antioxidant includes antioxidant RD and / or antioxidant 6PPD.
3. The low rolling resistance coefficient lower tread rubber according to claim 1, It is characterized in that The silane coupling agent includes Si75 and / or Si69; And / or, the accelerator includes accelerator D and / or accelerator NS; And / or, the anti-reversion agent is 1,6-bis(N,N-dibenzothiazolecarbamoyl disulfide)-hexane.
4. The low rolling resistance coefficient lower tread rubber according to any one of claims 1 to 3, It is characterized in that It comprises the following components in parts by weight: 100 parts of natural rubber, 5-20 parts of carbon black, 30-45 parts of white carbon black, 3.5 parts of zinc oxide, 2 parts of stearic acid, 3 parts of antioxidant, 3.95-5.1 parts of silane coupling agent, 0.5 parts of accelerator D, 0.5-1 parts of anti-reversion agent, 1.3-1.8 parts of sulfur, and 1.3-1.8 parts of accelerator NS.
5. A method for preparing a lower tread rubber with a low rolling resistance coefficient as claimed in any one of claims 1 to 4, It is characterized in that The following steps are involved: Add natural rubber into a meshing internal mixer, mix, then add accelerator D, white carbon black, and silane coupling agent, continue mixing, and then discharge the rubber to obtain a masterbatch; Adding a first-stage masterbatch, carbon black, antioxidant, zinc oxide and stearic acid into an intermeshing internal mixer, mixing, lifting the plug, and then pressing the plug, mixing and discharging the glue to obtain a second-stage masterbatch; Add the second-stage masterbatch into the intermeshing internal mixer, mix, then add sulfur, accelerator NS, anti-vulcanization reversion agent, continue mixing, lift the plug, then press the plug, mix and discharge the rubber to obtain the final mixed rubber, which is the lower tread rubber.
6. The method for preparing the lower tread rubber with low rolling resistance coefficient as claimed in claim 5, It is characterized in that The following steps are involved: Add natural rubber to an intermeshing internal mixer, set the mixer speed to 40-50 rpm, mix for 20-30 seconds, then add accelerator D, white carbon black, and silane coupling agent, continue mixing until the temperature reaches 140-160°C, and then discharge the rubber to obtain a masterbatch; Add the first-stage masterbatch, carbon black, antioxidant, zinc oxide and stearic acid into the intermeshing internal mixer, set the internal mixer speed to 40-50 rpm, mix for 120-140 seconds, lift the plug, keep for 15-25 seconds, then press the plug and mix to 140-160°C, then discharge the glue to obtain the second-stage masterbatch; Add the second-stage masterbatch into the intermeshing internal mixer, set the mixer speed to 25-35 rpm, mix for 60-70 seconds, then add sulfur, accelerator NS, and anti-vulcanization reversion agent, continue mixing for 130-140 seconds, lift the plug, then press the plug and mix to 100-120°C before discharging the rubber to obtain the final mixed rubber, which is the lower tread rubber.
7. A method for preparing a lower tread rubber with a low rolling resistance coefficient as claimed in any one of claims 1 to 4, It is characterized in that The following steps are involved: Add natural rubber into a meshing internal mixer, mix, then add accelerator D, white carbon black, and silane coupling agent, continue mixing, and then discharge the rubber to obtain a masterbatch; Add a section of masterbatch, carbon black, antioxidant, zinc oxide and stearic acid into a meshing internal mixer, mix, lift the plug, then press the plug. After mixing, discharge the rubber onto an open mixer, turn over, add sulfur, accelerator NS and anti-vulcanization reversion agent, then turn over thinly, cool the lower sheet to room temperature, and obtain the lower tread rubber.
8. The method for preparing the lower tread rubber with low rolling resistance coefficient as claimed in claim 7, It is characterized in that The following steps are involved: Add natural rubber to an intermeshing internal mixer, set the mixer speed to 40-50 rpm, mix for 20-30 seconds, then add accelerator D, white carbon black, and silane coupling agent, continue mixing until the temperature reaches 140-160°C, and then discharge the rubber to obtain a masterbatch; Add a masterbatch, carbon black, antioxidant, zinc oxide and stearic acid into a meshing internal mixer, set the mixer speed to 40-50 rpm, mix for 120-140 s, lift the plug, hold for 15-25 s, then press the plug and mix to 140-160 ℃, then discharge the rubber onto an open mixer, refining and cooling to 90-100 ℃, adding sulfur, accelerator NS and anti-vulcanization reversion agent, and then thin-pass refining for 280-320 s. Cool the lower sheet to room temperature to obtain the lower tread rubber.
9. A tire, It is characterized in that The method is prepared by using the low rolling resistance coefficient lower tread rubber as claimed in any one of claims 1 to 4 or the low rolling resistance coefficient lower tread rubber prepared by the preparation method as claimed in any one of claims 5 to 8.
10. A method for evaluating the rolling resistance coefficient of a tire, It is characterized in that The following steps are involved: Providing a low rolling resistance coefficient lower tread rubber as claimed in any one of claims 1 to 4 or a low rolling resistance coefficient lower tread rubber prepared by the preparation method as claimed in any one of claims 5 to 8; Testing the storage modulus G' and loss modulus G" of the lower tread rubber; Calculate the tanδ value, wherein tanδ=G" / G'; Calculation of tanδ / G' 2 value; tanδ / G' 2 The value is linearly related to the rolling resistance coefficient of the tire, which can be calculated using tanδ / G' 2 The value predicts the rolling resistance coefficient of the tire.