Bio-based high-damping rubber material and preparation method thereof

By combining itaconate rubber, natural rubber, polynorbornene rubber and damping additive A, a high-performance bio-based high-damping rubber material is formed, which solves the problem of difficulty in balancing the damping performance and fatigue performance of traditional rubber materials and improves the performance of rubber. improve the mechanical and damping properties of the material and reduce carbon emissions.

CN118725426AActive Publication Date: 2024-10-01ZHUZHOU TIMES NEW MATERIAL TECHNOLOGY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411062490.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-01
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

It is difficult to balance the damping performance and fatigue performance of traditional bio-based itaconate rubber and natural rubber, and has poor compatibility with high-damping polar rubber, resulting in poor mechanical properties of the rubber and unable to meet product use needs.

Method used

Itaconate rubber and natural rubber are used as raw rubber, and polynorbornene rubber with high damping properties and damping additive A are added to improve compatibility through vulcanizing agent cross-linking and chemical reaction, combined with bio-based carbon black and Vegetable oil-based plasticizer to form high-performance bio-based high-damping rubber material.

Benefits of technology

It significantly improves the damping performance and fatigue performance of the rubber, solves the problems of unstable damping performance and poor compatibility, improves the mechanical properties and service life of the rubber, and reduces carbon emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725426A_ABST
    Figure CN118725426A_ABST
Patent Text Reader

Abstract

The invention discloses a bio-based high-damping rubber material and a preparation method thereof. The bio-based high-damping rubber material comprises 100 parts of raw rubber; 3 to 10 parts of zinc oxide; 1-3 parts of stearic acid; 10 to 60 parts of a reinforcing filler; 2-20 parts of a plasticizer; 4 to 10 parts of an anti-aging agent; 2-15 parts of a damping material; 1.5 to 6 parts of a vulcanization system; the rubber is itaconate rubber or a mixture of the itaconate rubber and natural rubber, and the damping material comprises polynorbornene rubber and a damping auxiliary agent A. The rubber material disclosed by the invention solves the problems that the damping performance and the fatigue performance of a traditional damping rubber material cannot be considered at the same time, and the damping performance is unstable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rubber materials, and in particular relates to a bio-based high-damping rubber material and a preparation method thereof. Background Art

[0002] Bio-based itaconate rubber is a new type of rubber material prepared by low-temperature emulsion polymerization using green and environmentally friendly biomass itaconate as the main monomer. It is the first bio-based synthetic rubber variety in the world. Compared with natural rubber, itaconate rubber has better damping performance and flexural performance, especially flexural performance. When itaconate rubber is used to replace part of natural rubber as the main raw rubber, in order to improve the damping performance of itaconate rubber and / or natural rubber, some high-damping raw rubber (such as chloroprene rubber, nitrile rubber, etc.) or some high-damping materials (such as AO-80, antioxidant 1010 or some damping resin) are usually used together. Because itaconate rubber and natural rubber are non-polar raw rubbers, when they are used together with polar rubbers with high damping characteristics (such as chloroprene rubber, nitrile rubber, etc.), the compatibility between the two is poor, and the mechanical properties of the rubber are poor, which cannot meet the product use requirements. Summary of the invention

[0003] In order to overcome the problems in the prior art, the present invention provides a bio-based high damping rubber material and a preparation method thereof. The prepared damping material has good compatibility with raw rubber and will not have precipitation problems during actual use, thereby solving the problem of instability of damping performance of traditional damping rubber materials and products, and at the same time solving the difficult problem that damping performance and fatigue performance of traditional damping materials cannot be taken into account at the same time.

[0004] In order to solve the above technical problems, the technical solutions proposed by the present invention are as follows:

[0005] The invention provides a bio-based high-damping rubber material, comprising the following raw materials in parts by mass: raw rubber: 100 parts; zinc oxide: 3-10 parts; stearic acid: 1-3 parts; reinforcing filler: 10-60 parts; plasticizer: 2-20 parts; antioxidant: 4-10 parts; damping material: 2-15 parts; vulcanization system: 1.5-6 parts; the rubber is itaconate rubber, or a mixture of itaconate rubber and natural rubber, and the damping material comprises polynorbornene rubber.

[0006] In the present invention, itaconate rubber and natural rubber are used as raw rubbers. Compared with natural rubber, itaconate rubber has better damping performance and flexural performance, especially flexural performance. The combination of the two can greatly improve fatigue performance while ensuring damping performance. At the same time, polynorbornene rubber (PNR) with high damping properties is added. It has both cis and trans structures, can avoid crystallization, has a glass transition temperature of 35-37°C, has high shock absorption and damping properties, and a loss factor of up to 3 or even higher, which can convert most of the vibration energy into heat energy; in addition, its molecular chain contains C=C double bonds, which can react chemically with the C=C double bonds in the itaconate / natural rubber molecular chain, thereby organically combining the polynorbornene rubber and itaconate / natural rubber through the cross-linking effect of the vulcanizer, improving the compatibility of the two, and thus greatly improving the damping performance of itaconate / natural rubber.

[0007] As an optional embodiment, in the bio-based high damping rubber material provided by the present invention, the damping material further includes a damping aid A, and the structural formula of the damping aid A is shown in the following formula (1):

[0008]

[0009] In order to further improve the damping performance of itaconate rubber and / or natural rubber, a damping aid A is added in the present invention. The molecular structure of the damping aid A contains a large number of benzene ring structures, which can increase the steric hindrance effect and further significantly improve the damping performance of the rubber. In addition, the carboxyl group in the molecular structure of the novel damping aid can react chemically or form hydrogen bonds with the hydroxyl group on the surface of the filler or the epoxy group in the molecular structure of the plasticizer under certain conditions to form chemical and / or physical bonding bonds. The amino group in the molecular structure can react chemically with the double bond in the rubber molecular chain under high temperature and condensation agent conditions, thereby organically combining the rubber molecular chain with the filler / plasticizer, fundamentally solving the problem of damping agent precipitation.

[0010] As an optional embodiment, in the bio-based high damping rubber material provided by the present invention, the itaconate rubber is selected from one or more of binary itaconate rubber and ternary itaconate rubber; the natural rubber is selected from one or more of smoked sheet rubber, constant viscosity rubber and full latex.

[0011] Furthermore, the itaconate rubber is preferably ternary itaconate rubber; and the natural rubber is preferably smoked sheet rubber.

[0012] As an optional embodiment, in the bio-based high damping rubber material provided by the present invention, the polynorbornene rubber in the damping material is 2-12 parts, and the damping aid A is 1-10 parts.

[0013] As an optional embodiment, in the bio-based high damping rubber material provided by the present invention, the damping aid A is obtained by catalytic reaction of 5-amino-2,4,6-triiodoisophthalic acid and triarylimidazole.

[0014] As an optional embodiment, in the bio-based high damping rubber material provided by the present invention, the synthesis process of the damping aid A is as follows: 5-amino-2,4,6-triiodoisophthalic acid and triaryl imidazole are placed in a reaction container, cuprous iodide and ligand L-proline are added, and the reaction is stirred in a solvent at 60-80°C under a nitrogen atmosphere for 12-48 hours, and then filtered, the clear liquid is taken, the solvent is concentrated, and vacuum drying is performed to obtain the damping aid A.

[0015] As an optional embodiment, in the bio-based high damping rubber material provided by the present invention, the molar ratio of the 5-amino-2,4,6-triiodoisophthalic acid to the triarylimidazole is (1-1.1): (3.1-4).

[0016] In the present invention, the ratio of 5-amino-2,4,6-triiodoisophthalic acid and triarylimidazole is controlled to be (1-1.1): (3.1-4). If the ratio exceeds this range, small molecular substances may remain in the prepared damping additive A, thus affecting the damping effect.

[0017] As an optional embodiment, in the bio-based high damping rubber material provided by the present invention, the solvent is selected from one of N,N-dimethylformamide, N,N-dimethylacetamide or dimethyl sulfoxide.

[0018] As an optional embodiment, in the bio-based high damping rubber material provided by the present invention, the reinforcing filler is selected from one or more of bio-based carbon black, rice husk ash white carbon black, bio-based calcium carbonate, white carbon black, kaolin, qiangwei powder and montmorillonite.

[0019] Further, bio-based carbon black, rice husk ash white carbon black and bio-based calcium carbonate are preferred.

[0020] The present invention adopts bio-based carbon black, rice husk ash white carbon black and bio-based calcium carbonate, wherein the bio-based carbon black is prepared from three raw materials: methane, carbon dioxide and vegetable oil, and the carbon emission is greatly reduced compared with the traditional carbon black; the rice husk ash white carbon black is prepared from rice husk ash which is a by-product of rice processing; the bio-based calcium carbonate is prepared from oyster shells, and can replace up to 80% of the carbon black in rubber products, thereby reducing the carbon emission by 80%-90%.

[0021] As an optional embodiment, in the bio-based high damping rubber material provided by the present invention, the plasticizer is selected from one or more of soybean oil, castor oil, epoxidized soybean oil, epoxy cardanol laurate, epoxy cardanol acetate, and epoxy castor oil.

[0022] Furthermore, it is preferably one or more of epoxidized soybean oil, epoxy cardanol laurate, epoxy cardanol acetate, and epoxy castor oil.

[0023] In the present invention, plant oil-based plasticizers are used to replace petroleum-based plasticizers (including cycloalkane oil, paraffin oil, aromatic oil, etc.). The plasticizing effect of plant oil-based plasticizers is basically equivalent to that of petroleum-based plasticizers, but they are derived from plants, are renewable resources, and meet environmental protection requirements.

[0024] As an optional embodiment, in the bio-based high damping rubber material provided by the present invention, the antioxidant is selected from one or more of quinolines, p-phenylenediamines, protective waxes and ultraviolet absorbers.

[0025] Furthermore, antioxidants RD, 4020, microcrystalline wax and UV-531 are preferred.

[0026] As an optional embodiment, in the bio-based high damping rubber material provided by the present invention, the vulcanization system includes a vulcanizing agent and an accelerator.

[0027] As an optional embodiment, in the bio-based high damping rubber material provided by the present invention, the vulcanizing agent is selected from one or more of sulfur, insoluble sulfur and sulfur carriers; the accelerator is selected from one or more of thiazole accelerators, sulfonamide accelerators and thiuram accelerators.

[0028] Furthermore, the vulcanizing agent is preferably sulfur and insoluble sulfur. The accelerator is preferably thiazole or sulfenamide, such as accelerator DM and accelerator NOBS.

[0029] As an optional embodiment, in the bio-based high damping rubber material provided by the present invention, the zinc oxide is selected from one of direct zinc oxide and indirect zinc oxide.

[0030] Furthermore, indirect zinc oxide is preferred.

[0031] Based on the same technical concept, the present invention also provides a method for preparing the above-mentioned bio-based high damping rubber material, comprising the following steps:

[0032] Add itaconate rubber and natural rubber into an internal mixer, mix at 50-70°C for 1-2 minutes, then add reinforcing filler and plasticizer, mix for 1-2 minutes, add zinc oxide, stearic acid, antioxidant and damping material, mix evenly, cool to below 70°C, add vulcanizer and accelerator, remove from the sheet and cool naturally to obtain rubber compound, and vulcanize the rubber compound after it is left to stand.

[0033] As an optional embodiment, in the preparation method provided by the present invention, during the vulcanization process, the vulcanization temperature is 140° C.-160° C., the vulcanization pressure is 10-20 MPa, and the vulcanization time is 10-30 minutes.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] (1) The bio-based itaconate rubber of the present invention partially or completely replaces natural rubber, which can simultaneously improve the damping performance and fatigue performance of the rubber, solving the technical problem that the damping performance and fatigue performance of the traditional rubber cannot be taken into account at the same time. At the same time, the use of PNR to replace polar damping rubber (such as nitrile rubber) can further significantly improve the mechanical properties, damping performance and fatigue performance of the rubber, and solve the problem of poor compatibility between natural rubber / itaconate and polar damping rubber, which can further improve the performance and service life of the rubber.

[0036] (2) The present invention adopts damping agent A to replace the traditional polar damping agent (such as AO-80), which solves the technical problem that the traditional damping agent is easy to precipitate, resulting in unstable damping performance of the rubber and the product, and further improves the mechanical, damping and fatigue properties of the rubber. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0038] Figure 1 This is the NMR spectrum of the damping aid A prepared in Example 1. DETAILED DESCRIPTION

[0039] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.

[0040] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0041] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0042] Example

[0043] The preparation process of damping agent A is as follows:

[0044] 5-amino-2,4,6-triiodoisophthalic acid (1-1.1 eq, relative molecular weight 558.84) and triaryl imidazole (3.1-4 eq, relative molecular weight 296.4) are placed in a reaction vessel, and cuprous iodide (1.5-6.0 eq, relative molecular weight 190.5) is added, and ligand L-proline (1.5-6.0 eq, relative molecular weight 115.1) is added, and one of potassium carbonate, sodium carbonate or cesium carbonate (6.0-12.0 eq, relative molecular weights are 138.2, 106.0, 325.8, respectively) is added, and then one of N,N-dimethylformamide (DMF) or N,N-dimethylacetamide (DMAC) or dimethyl sulfoxide (DMSO) (300-1000 eq) is added. After bubbling nitrogen and purging oxygen for 30 minutes, the reaction is stirred at 60-80°C under a nitrogen atmosphere for 12-48 hours. Filter, take out the clear liquid, concentrate the solvent and dry in vacuum.

[0045] The NMR spectrum of the prepared damping aid A is shown in the attached figure. Figure 1 shown.

[0046] The synthetic formula is as follows:

[0047]

[0048] The raw material components and composition ratio of the bio-based high damping rubber material are as follows: raw rubber: 100 parts; zinc oxide: 3-10 parts; stearic acid: 1-3 parts; reinforcing filler: 10-60 parts; plasticizer: 2-20 parts; antioxidant: 4-10 parts; damping material: 2-15 parts; vulcanization system: 1.5-6 parts.

[0049] The rubber compound mixing and vulcanization process is as follows:

[0050] (1) Rubber mixing process

[0051] Add raw rubber (one or more of natural rubber and itaconate rubber) into an internal mixer, mix at 50-70°C for 1-2 minutes, then add reinforcing filler, mix for 1-2 minutes, add plasticizer, zinc oxide, stearic acid, antioxidant and damping material, mix well, cool to below 70°C, add vulcanizer and accelerator, remove from the sheet and cool naturally.

[0052] (2) Rubber vulcanization process

[0053] After the rubber compound is left standing for 16 hours, the vulcanization temperature is controlled at 140°C-160°C, the vulcanization pressure is controlled at 10-20MPa, and the vulcanization time is controlled at 10-30 minutes to obtain a high-performance rubber material with high bio-based content, high damping and fatigue resistance.

[0054] The samples of Examples 1 to 6 and Comparative Examples 1 to 3 were prepared according to the above operation. The specific addition amount of each Example and Comparative Example is as shown in Table 1 below:

[0055] Table 1 Formula table of embodiments and comparative examples (parts by mass)

[0056]

[0057]

[0058] The properties of the rubber materials and products corresponding to the above embodiments and comparative examples were tested, and the parameter results were shown in Table 2:

[0059] Table 2: Detection performance parameters

[0060]

[0061]

[0062] From the comparison between Comparative Example 1 and Example 1 and Example 2, it can be seen that after using bio-based itaconate rubber, although the tensile strength and elongation at break of the rubber are slightly reduced, the loss factor and fatigue performance of the rubber are significantly improved, which solves the technical problem that the damping performance and fatigue performance of the traditional rubber cannot be taken into account at the same time; from the comparison between Comparative Example 2 and Example 3, it can be seen that after adding high damping polynorbornene rubber (PNR) to the rubber, the damping performance of the rubber is greatly improved, and other properties remain basically the same; from the comparison between Comparative Example 3 and Example 4, it can be seen that when polar nitrile rubber is used in combination, due to the large difference in polarity between natural rubber / itaconate rubber and it, when the two are used in combination, the compatibility is poor, and the mechanical properties of the rubber are poor. The mechanical properties, damping properties and fatigue properties of the rubber are all poor. When non-polar high-damping polybornene rubber (PNR) is used in combination, the mechanical properties, damping properties and fatigue properties of the rubber are all better than those of Comparative Example 3, which solves the problem that polar rubber can improve the damping properties of natural rubber / itaconate rubber but has an adverse effect on the mechanical properties and fatigue properties; from the comparison between Comparative Example 4 and Example 5, it can be seen that when damping aid A is used, the mechanical properties, damping properties and fatigue properties of the rubber are all better than those of damping aid AO-80 and the technical problem of easy precipitation of AO-80 is solved at the same time; from the comparison between Example 5 and Example 6, it can be seen that increasing the amount of damping aid A can further improve the damping properties of the rubber, and has basically no effect on the mechanical properties and fatigue properties.

[0063] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the scope of protection of the present invention.

Claims

1. A bio-based high damping rubber material, It is characterized in that The invention comprises the following raw materials in parts by weight: raw rubber: 100 parts; zinc oxide: 3-10 parts; Stearic acid: 1-3 parts; reinforcing filler: 10-60 parts; Plasticizer: 2-20 parts; Anti-aging agent: 4-10 parts; Damping material: 2-22 parts; Vulcanization system: 1.5-6 parts; the rubber is itaconate rubber, or a mixture of itaconate rubber and natural rubber, and the damping material includes polynorbornene rubber.

2. The bio-based high damping rubber material according to claim 1, It is characterized in that The damping material also includes a damping aid A, and the structural formula of the damping aid A is shown in the following formula (1):

3. The bio-based high damping rubber material according to claim 1, It is characterized in that The itaconate rubber is selected from one or more of binary itaconate rubber and ternary itaconate rubber; the natural rubber is selected from one or more of smoked sheet rubber, permanent viscous rubber and full latex.

4. The bio-based high damping rubber material according to claim 2, It is characterized in that The damping material contains 2-12 parts of polynorbornene rubber and 1-10 parts of damping aid A.

5. The bio-based high damping rubber material according to claim 2, It is characterized in that The damping auxiliary agent A is obtained by catalytic reaction of 5-amino-2,4,6-triiodoisophthalic acid and triaryl imidazole.

6. The bio-based high damping rubber material according to claim 5, It is characterized in that The synthesis process of the damping auxiliary agent A is as follows: 5-amino-2,4,6-triiodoisophthalic acid and triaryl imidazole are placed in a reaction container, cuprous iodide and ligand L-proline are added, and the reaction is stirred in a solvent at a temperature of 60-80° C. for 12-48 hours under a nitrogen atmosphere, and then filtered to take out the clear liquid, concentrate the solvent, and vacuum dry to obtain the damping auxiliary agent A.

7. The bio-based high damping rubber material according to claim 5 or 6, It is characterized in that The molar ratio of the 5-amino-2,4,6-triiodoisophthalic acid to the triarylimidazole is (1-1.1):(3.1-4).

8. The bio-based high damping rubber material according to claim 1, It is characterized in that The reinforcing filler is selected from one or more of bio-based carbon black, rice husk ash white carbon black, bio-based calcium carbonate, white carbon black, kaolin, Qiangwei powder and montmorillonite; the plasticizer is selected from one or more of soybean oil, castor oil, epoxidized soybean oil, epoxy cardanol laurate, epoxy cardanol acetate, and epoxy castor oil; the antioxidant is selected from one or more of quinoline, p-phenylenediamine, protective wax and ultraviolet absorber; the vulcanization system includes a vulcanizing agent and an accelerator, and the vulcanizing agent is selected from one or more of sulfur, insoluble sulfur and sulfur carrier; the accelerator is selected from one or more of thiazole accelerators, sulfonamide accelerators and thiuram accelerators.

9. The method for preparing the bio-based high damping rubber material according to any one of claims 1 to 8, It is characterized in that The following steps are involved: Add itaconate rubber and natural rubber into an internal mixer, mix at 50-70°C for 1-2 minutes, then add reinforcing filler and plasticizer, mix for 1-2 minutes, add zinc oxide, stearic acid, antioxidant and damping material, mix evenly, cool to below 70°C, add vulcanizer and accelerator, remove from the sheet and cool naturally to obtain rubber compound, and vulcanize the rubber compound after it is left to stand.

10. The method for preparing the bio-based high damping rubber material according to claim 9, It is characterized in that During the vulcanization process, the vulcanization temperature is 140°C-160°C, the vulcanization pressure is 10-20MPa, and the vulcanization time is 10-30 minutes.

Citation Information

Patent Citations

  • Itaconate based bioengineering rubber damping material and preparation method thereof

    CN103951924A

  • Biodegradable polymer

    CN112313267A

  • Divalent platinum complexes, preparation method thereof and application of divalent platinum complexes in aspect of luminescent materials

    CN112940045A

  • Preparation and application of diagnosis and treatment integrated nanoprobe for rheumatoid arthritis

    CN113069558A

  • High-damping shock-absorbing material for automobile body suspension and preparation method and application thereof

    CN113234262A