Glass fiber reinforced nylon composite material, preparation method and application thereof

By introducing a polymer brush on the surface of the glass fiber to enhance the compatibility between the glass fiber and the nylon matrix, the heat resistance and welding problems of the glass fiber reinforced nylon composite material in the automotive air intake manifold are solved, and the mechanical properties and performance are significantly improved. The high temperature resistance solves the problems of easy deformation of materials and difficulty in welding in the existing technology.

CN118725562APending Publication Date: 2024-10-01SUZHOU SUNWAY POLYMER
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410968218.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing glass fiber reinforced nylon composite materials in automotive air intake manifolds have insufficient heat resistance, are easily deformed, and are difficult to weld and form. They are prone to produce glass fiber debris and affect vehicle performance.

Method used

By introducing a polymer brush on the surface of the glass fiber, the long-chain flexible structure of the polymer brush is used to enhance the interfacial interaction and compatibility between the glass fiber and the nylon matrix, and the polymer brush-modified glass fiber is prepared and extruded through a twin-screw Machine blending, processing and granulation to form glass fiber reinforced nylon composite materials.

Benefits of technology

It significantly improves the mechanical properties and high temperature aging resistance of the material, improves the welding strength, reduces the phenomenon of floating fibers, and improves the overall performance and application value of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a glass fiber reinforced nylon composite material, and a preparation method and application thereof, the glass fiber reinforced nylon composite material comprises (a) a nylon matrix, (b) modified glass fiber, (c) an auxiliary agent, and (d) a color master batch; wherein the modified glass fiber is glass fiber modified by a polymer brush. According to the invention, the polymer brush is introduced to the surface of the glass fiber, and the long-chain flexible structure of the polymer brush is utilized to increase the interfacial interaction and compatibility between the glass fiber and the nylon matrix, so that the mechanical property and temperature resistance of the composite material are enhanced; and the binding force between the polymer brush and nylon acylamino is relatively strong, so that the temperature resistance is further enhanced, the problem of fiber floating on the surface of the material is solved, and the market prospect and the application value are wide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer processing, and in particular to a glass fiber reinforced nylon composite material, a preparation method and application thereof. Background Art

[0002] At present, the main direction and research and development goal of the automobile industry is to reduce weight, so as to achieve energy saving and consumption reduction, increase vehicle speed, reduce emissions and save costs. In the 1990s, the automobile industry began to use plastics to manufacture functional parts. At the same time, because plastics are easy to form, they play an important role in the manufacturing process of complex parts such as automobile engine intake manifolds and fuel tanks. Therefore, strengthening the research on the application and development of plastic automotive intake manifolds and fuel tanks has very important practical significance.

[0003] Glass fiber is cheap, and its strength and Young's modulus are 10 times greater than nylon resin. It has very low water absorption, excellent heat resistance, chemical resistance and mechanical properties, and is an ideal reinforcement material for engineering. However, due to the difference between glass fiber and nylon materials, compatibility issues are prone to occur, and poor surface quality phenomena such as exposed glass fiber (commonly known as floating fiber) occur during the molding process. In addition, the operating temperature of the automotive intake manifold is relatively high, and ordinary glass fiber reinforced nylon composite materials are not heat resistant enough, are easy to deform, and have a high application risk; at the same time, the existing glass fiber reinforced nylon composite materials are difficult to weld and mold due to their high glass fiber content, and glass fiber debris is easily generated during the welding process, affecting the normal use of the intake manifold and thus affecting the performance of the vehicle. Summary of the invention

[0004] In view of the shortcomings of the prior art described above, the purpose of the present invention is to provide a glass fiber reinforced nylon composite material to solve the problems of insufficient heat resistance, easy deformation and difficult welding of the glass fiber reinforced nylon material used for vehicle intake manifolds in the prior art. At the same time, the present invention will also provide a method for preparing the glass fiber reinforced nylon composite material; in addition, the present invention will also provide applications of the glass fiber reinforced nylon composite material.

[0005] In order to achieve the above-mentioned object and other related objects, the present invention provides the following technical solutions: The first aspect of the present invention provides a glass fiber reinforced nylon composite material, comprising (a) a nylon matrix, (b) modified glass fiber, (c) an additive, and (d) a masterbatch; wherein the modified glass fiber is a glass fiber modified by a polymer brush.

[0006] Specifically, the polymer brush is composed of a polymethyl methacrylate (PMMA) molecular chain, an initiator is fixed on the surface of the glass fiber, and one end of the polymethyl methacrylate molecular chain is fixed on the initiator. The glass fiber is a glass fiber modified by a silane coupling agent, and the initiator is fixed on the surface of the glass fiber by coupling with the silane coupling agent.

[0007] The present invention introduces polymer brushes on the surface of glass fiber and utilizes the long-chain flexible structure of the polymer brushes to increase the interface interaction and compatibility between glass fiber and nylon matrix, thereby enhancing the mechanical properties and temperature resistance of the composite material, and has broad market prospects and application value.

[0008] Furthermore, the polymer brush-modified glass fiber is obtained by the following preparation method: (1) Clean the glass fiber and remove organic matter and impurities on the surface of the glass fiber; (2) The cleaned glass fiber is subjected to silanization treatment to introduce a silane coupling agent on its surface; (3) reacting the glass fiber modified with the silane coupling agent with the initiator to fix the initiator on the surface of the glass fiber; (4) The glass fiber after the initiator is fixed is reacted with methyl methacrylate (MMA) monomer by atom transfer radical polymerization (ATRP) to make the molecular chain grow from the initiator fixing point on the surface of the glass fiber to form a dense brush-like structure, thereby obtaining the polymer brush-modified glass fiber.

[0009] In step (1), the glass fiber cleaning process includes: ultrasonically cleaning the glass fiber in acetone, deionized water and ethanol in sequence, each for 5 to 10 minutes, and then drying at 80 to 110°C.

[0010] Preferably, the glass fiber is flat glass fiber, and the ratio of major axis to minor axis is 2:1 to 5:1.

[0011] In step (2), the silanization process includes: immersing the glass fiber in anhydrous ethanol containing a silane coupling agent, reacting at room temperature, and washing and drying after the reaction is completed.

[0012] Wherein, the silane coupling agent is 3-aminopropyltriethoxysilane (APTES); the added concentration of the silane coupling agent is preferably 1-5wt%.

[0013] In step (3), the initiator is 2-bromoisobutyric acid bromide (BiBB). The glass fiber modified with the silane coupling agent is reacted with the initiator in an organic solvent at room temperature. After the reaction, the glass fiber is washed and dried. After such treatment, the surface of the glass fiber will have brominated alkyl ends that can be used for ATRP.

[0014] In step (4), the ATRP reaction is carried out under the action of a transition metal catalyst and a ligand. The catalyst and the ligand work together in the ATRP reaction to achieve fine control over the polymerization reaction, which not only involves the growth of the polymer chain, but also includes the regulation of the polymerization rate, molecular weight and molecular weight distribution.

[0015] The transition metal catalyst is copper (I) bromide (CuBr), copper (I) chloride (CuCl) or copper (I) iodide (CuI); the ligand is N,N,N',N'',N''-pentamethyldiethylenetriamine (PMDETA) or N,N,N',N'',N'',N''-hexamethyltriethylenetetramine (HMTTA).

[0016] Step (4) is specifically as follows: adding MMA monomer, copper (I) catalyst and ligand into an organic solvent, stirring evenly, adding glass fiber fixed with initiator, introducing inert gas protection, heating to 55-70° C., stirring and performing ATRP reaction, after the reaction is completed, filtering, washing and drying to obtain the polymer brush modified glass fiber.

[0017] During the ATRP reaction, the copper (I) catalyst acts on the brominated alkyl end of the initiator to form free radicals and Cu (II) complexes. The generated free radicals react with the MMA monomer to initiate chain growth and form PMMA molecular chains. The active end of the molecular chain can react with the Cu (II) complex to re-form the brominated end and the Cu (I) complex, thereby stopping the polymerization (inactivation) and preventing the molecular chain from continuing to increase in length. The ligand can form a complex with Cu (I) and Cu (II), thereby regulating the conversion between Cu (I) / Cu (II) and increasing the stability and reaction efficiency of the catalyst. By precisely controlling the ratio of Cu (I) / Cu (II), reaction temperature and reaction time, the growth of the molecular chain can be controlled to achieve the desired molecular weight and structure.

[0018] In step (4), the mass ratio of glass fiber, MMA monomer, copper (I) catalyst and ligand is (80-120): (20-100): (2-10): (2-10).

[0019] Preferably, the mass ratio of the copper (I) catalyst to the ligand is 1:1.

[0020] In step (3) and step (4), the organic solvent includes methanol, ethanol or dichloromethane.

[0021] Furthermore, the modified glass fiber accounts for 15-35wt% of the total weight of the glass fiber reinforced nylon composite material.

[0022] Furthermore, the nylon matrix includes at least one of PA6, PA66, PA56, PA612, PA1010, PA1012, PA5T, PA6T, PA10T, and PA6I.

[0023] Furthermore, the nylon matrix is ​​composed of high molecular weight PA10T and high molecular weight distribution width PA10T, and the ratio of the two is 3:1 to 3:4, preferably 3:2.

[0024] Furthermore, the auxiliary agent is a compound of an antioxidant and an internal and external lubricant, and the ratio of the two is 1:1 to 1:5.

[0025] Furthermore, the additive accounts for 0.1-1wt% of the total weight of the glass fiber reinforced nylon composite material.

[0026] Furthermore, the masterbatch accounts for 0.5-2wt% of the total weight of the glass fiber reinforced nylon composite material.

[0027] A second aspect of the present invention provides a method for preparing a glass fiber reinforced nylon composite material, comprising the following steps: S1, mixing nylon matrix, additives and masterbatch uniformly with a high-speed mixer to obtain a mixture A; S2, adding mixed material A to the main feed, adding modified glass fiber to the side feed, and blending and granulating through a twin-screw extruder; S3, melt-extrude through a twin-screw extruder, cool the extrudate in a water tank, and obtain the glass fiber reinforced nylon composite material after traction granulation.

[0028] In step S1, the mixer speed is 200-400 rpm, and the mixing time is 2-10 min.

[0029] In step S2, the temperature range of the twin-screw extruder is 180-310°C, and the screw speed is 350-600 rpm.

[0030] A third aspect of the present invention provides an application of a glass fiber reinforced nylon composite material, wherein the glass fiber reinforced nylon composite material is used to manufacture an intake manifold for a vehicle.

[0031] As described above, the glass fiber reinforced nylon composite material, preparation method and application thereof of the present invention have the following beneficial effects: DETAILED DESCRIPTION The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.

[0032] Example 1 A polymer brush-modified glass fiber, the preparation method of which comprises the following steps: (1) 100 g of glass fiber was ultrasonically cleaned in acetone, deionized water and ethanol for 10 min each time, and then dried at 110 °C; (2) Soak the cleaned glass fiber in 1 L of anhydrous ethanol solution of 1 wt% APTES and react at room temperature for 12 hours. After the reaction, wash with ethanol to remove unreacted APTES and dry at 110°C; (3) adding the above APTES-modified glass fiber and 0.5 g BiBB to dichloromethane for reaction at room temperature for 24 hours. After the reaction, washing the glass fiber with dichloromethane and methanol to remove unreacted BiBB, and drying at 60°C; (4) Add 50 g of MMA monomer, 5 g of CuBr and 5 g of PMDETA to dichloromethane, stir evenly, then add the glass fiber fixed with BiBB, introduce nitrogen protection, heat to 60 °C, and carry out ATRP reaction under stirring. After the reaction, filter out the polymer brush-modified glass fiber, wash with methanol and deionized water to remove unreacted monomer and catalyst, and finally dry at 60 °C.

[0033] Example 2 A glass fiber reinforced nylon composite material, the preparation method of which comprises the following steps: S1, 45 parts by weight of high molecular weight PA10T, 30 parts by weight of high molecular weight distribution width PA10T, 0.5 parts by weight of antioxidant, 0.5 parts by weight of internal and external lubricant, and 1 part by weight of masterbatch were mixed uniformly by a high-speed mixer at a speed of 300 rpm for 3 min to obtain a mixture A; S2, adding mixed material A to the main feed, adding 15 parts by weight of the polymer brush-modified glass fiber prepared in Example 1 to the side feed, and blending and granulating by a twin-screw extruder, with a screw temperature of 260° C. and a screw speed of 350 rpm; S3, melt-extrude through a twin-screw extruder, cool the extrudate in a water tank, and obtain the glass fiber reinforced nylon composite material after traction granulation.

[0034] Example 3 A glass fiber reinforced nylon composite material, the preparation method of which comprises the following steps: S1, 45 parts by weight of high molecular weight PA10T, 30 parts by weight of high molecular weight distribution width PA10T, 0.5 parts by weight of antioxidant, 0.5 parts by weight of internal and external lubricant, and 1 part by weight of masterbatch were mixed uniformly by a high-speed mixer at a speed of 300 rpm for 3 min to obtain a mixture A; S2, adding mixed material A to the main feed, adding 23 parts by weight of the polymer brush-modified glass fiber prepared in Example 1 to the side feed, and blending and granulating by a twin-screw extruder, with a screw temperature of 260° C. and a screw speed of 350 rpm; S3, melt-extrude through a twin-screw extruder, cool the extrudate in a water tank, and obtain the glass fiber reinforced nylon composite material after traction granulation.

[0035] Example 4 A glass fiber reinforced nylon composite material, the preparation method of which comprises the following steps: S1, 45 parts by weight of high molecular weight PA10T, 30 parts by weight of high molecular weight distribution width PA10T, 0.5 parts by weight of antioxidant, 0.5 parts by weight of internal and external lubricant, and 1 part by weight of masterbatch were mixed uniformly by a high-speed mixer at a speed of 300 rpm for 3 min to obtain a mixture A; S2, adding mixed material A to the main feed, adding 35 parts by weight of the polymer brush-modified glass fiber prepared in Example 1 to the side feed, and blending and granulating by a twin-screw extruder, with a screw temperature of 260° C. and a screw speed of 350 rpm; S3, melt-extrude through a twin-screw extruder, cool the extrudate in a water tank, and obtain the glass fiber reinforced nylon composite material after traction granulation.

[0036] Example 5 A glass fiber reinforced nylon composite material, the preparation method of which comprises the following steps: S1, 75 parts by weight of PA10T, 0.5 parts by weight of antioxidant, 0.5 parts by weight of internal and external lubricant, and 1 part by weight of masterbatch were mixed uniformly by a high-speed mixer at a speed of 300 rpm for 3 min to obtain a mixture A; S2, adding mixed material A to the main feed, adding 23 parts by weight of the polymer brush-modified glass fiber prepared in Example 1 to the side feed, and blending and granulating by a twin-screw extruder, with a screw temperature of 260° C. and a screw speed of 350 rpm; S3, melt-extrude through a twin-screw extruder, cool the extrudate in a water tank, and obtain the glass fiber reinforced nylon composite material after traction granulation.

[0037] Comparative Example 1 A glass fiber reinforced nylon composite material, the preparation method of which comprises the following steps: S1, 75 parts by weight of PA10T, 0.5 parts by weight of antioxidant, 0.5 parts by weight of internal and external lubricant, and 1 part by weight of masterbatch were mixed uniformly by a high-speed mixer at a speed of 300 rpm for 3 min to obtain a mixture A; S2, adding mixed material A to the main feed, adding 23 parts by weight of ordinary glass fiber to the side feed, and blending and granulating through a twin-screw extruder, with a screw temperature of 260°C and a screw speed of 350rpm; S3, melt-extrude through a twin-screw extruder, cool the extrudate in a water tank, and obtain the glass fiber reinforced nylon composite material after traction granulation.

[0038] Comparative Example 2 A glass fiber reinforced nylon composite material, the preparation method of which comprises the following steps: S1, 75 parts by weight of PA10T, 0.5 parts by weight of antioxidant, 0.5 parts by weight of internal and external lubricant, and 1 part by weight of masterbatch were mixed uniformly by a high-speed mixer at a speed of 300 rpm for 3 min to obtain a mixture A; S2, adding mixed material A to the main feed, adding 23 parts by weight of glass fiber modified by silane coupling agent to the side feed, and blending and granulating by a twin-screw extruder, with a screw temperature of 260° C. and a screw speed of 350 rpm; S3, melt-extrude through a twin-screw extruder, cool the extrudate in a water tank, and obtain the glass fiber reinforced nylon composite material after traction granulation.

[0039] The glass fiber modified reinforced nylon composite materials prepared in Examples 2 to 5 and Comparative Examples 1 to 2 were dried at 120° C. for 4 h and injection molded to obtain samples. The samples were subjected to tensile tests, bending tests, notch impact tests, welding tests, and tensile retention rate tests after high temperature aging. The experimental results are shown in Table 1.

[0040] Among them, the tensile test is tested according to ISO 527, the bending test is tested according to ISO 178, the notch impact test is tested according to ISO 179, the weld is visually observed for defects in the welding test, and the thermal aging conditions of the tensile retention rate test after high-temperature aging are 120°C and 1000h.

[0041] Table 1 Experimental data of glass fiber modified reinforced nylon composite materials of Examples 2 to 5 and Comparative Examples 1 to 2

[0042] It can be seen from the experimental results of Example 5 and Comparative Examples 1 and 2 that, compared with the traditional silane coupling agent modified glass fiber, the polymer brush modified glass fiber prepared by the present invention has better compatibility with the nylon matrix, and has a stronger bonding with the nylon matrix, can significantly improve the mechanical properties and high temperature aging resistance of the material, has higher welding strength, and does not produce defects.

[0043] It can be seen from the experimental results of Example 3 and Example 5 that the nylon matrix is ​​compounded with nylon materials of different molecular weights and different molecular weight distribution widths, which can significantly improve the welding strength of the composite material and partially improve the mechanical properties.

[0044] In summary, the present invention introduces polymer brushes on the surface of glass fibers and utilizes the long-chain flexible structure of polymer brushes to increase the interface interaction and compatibility between glass fibers and nylon matrix, thereby enhancing the mechanical properties and temperature resistance of the composite material; and the polymer brushes have a strong binding force with nylon amide groups, further enhancing the temperature resistance and improving the problem of floating fibers on the surface of the material, which has broad market prospects and application value. Therefore, the present invention effectively overcomes various shortcomings in the prior art and has a high industrial utilization value.

[0045] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A glass fiber reinforced nylon composite material, comprising (a) a nylon matrix, (b) modified glass fiber, (c) an additive, and (d) a masterbatch; characterized in that: The modified glass fiber is glass fiber modified by a polymer brush.

2. The glass fiber reinforced nylon composite material according to claim 1, characterized in that: The polymer brush is composed of PMMA molecular chains, an initiator is fixed on the surface of the glass fiber, and one end of the PMMA molecular chain is fixed on the initiator.

3. The glass fiber reinforced nylon composite material according to claim 2, characterized in that: The polymer brush modified glass fiber is obtained by the following preparation method: (1) Clean the glass fiber and remove organic matter and impurities on the surface of the glass fiber; (2) The cleaned glass fiber is subjected to silanization treatment to introduce a silane coupling agent on its surface; (3) reacting the glass fiber modified with the silane coupling agent with the initiator to fix the initiator on the surface of the glass fiber; (4) The glass fiber after the initiator is fixed undergoes an atom transfer radical polymerization reaction with the MMA monomer, so that the PMMA molecular chain starts to grow from the initiator fixing point on the surface of the glass fiber to form a dense brush-like structure, thereby obtaining the polymer brush-modified glass fiber.

4. The glass fiber reinforced nylon composite material according to claim 3, characterized in that: In step (2), the silanization process includes: immersing the glass fiber in anhydrous ethanol containing a silane coupling agent, reacting at room temperature, and washing and drying after the reaction is completed; the silane coupling agent is 3-aminopropyltriethoxysilane; the added concentration of the silane coupling agent is 1~5wt%.

5. The glass fiber reinforced nylon composite material according to claim 3, characterized in that: In step (3), the initiator is 2-bromoisobutyric acid bromide.

6. The glass fiber reinforced nylon composite material according to claim 3, characterized in that: In step (4), the ATRP reaction is carried out under the action of a transition metal catalyst and a ligand.

7. The glass fiber reinforced nylon composite material according to claim 6, characterized in that: The transition metal catalyst is copper (I) bromide, copper (I) chloride or copper (I) iodide; the ligand is N,N,N',N'',N''-pentamethyldiethylenetriamine or N,N,N',N'',N'',N''-hexamethyltriethylenetetramine.

8. The glass fiber reinforced nylon composite material according to claim 1, characterized in that: The nylon matrix is ​​composed of high molecular weight PA10T and high molecular weight distribution width PA10T, and the ratio of the two is 3:1-3:

4.

9. A method for preparing a glass fiber reinforced nylon composite material according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1, mixing nylon matrix, additives and masterbatch uniformly with a high-speed mixer to obtain a mixture A; S2, adding mixed material A to the main feed, adding modified glass fiber to the side feed, and blending and granulating through a twin-screw extruder; S3, melt-extrude through a twin-screw extruder, cool the extrudate in a water tank, and obtain the glass fiber reinforced nylon composite material after traction granulation.

10. An application of the glass fiber reinforced nylon composite material according to any one of claims 1 to 8, characterized in that: The glass fiber reinforced nylon composite material is used for manufacturing an intake manifold for a vehicle.