Asphalt pavement patching material and preparation method thereof
By using SBS modifiers, polyethylene wax, fiber and other components in asphalt pavement repair materials, combined with homogeneous mixing and vacuum forming processes, the problems of high temperature sensitivity and poor support performance are solved, and the high temperature resistance of the material is significantly improved. Stability and low-temperature crack resistance extend the service life of the pavement.
Patent Information
- Application Number
- CN202410959160.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-01
AI Technical Summary
Existing asphalt pavement repair materials have problems such as high temperature sensitivity and poor support performance, resulting in unsatisfactory repair results and short service life.
Using a combination of asphalt, modifier, stabilizer, anti-flaking agent and reinforcing fiber, SBS modifier and polyethylene wax are used to reduce temperature sensitivity, polypropylene fiber and glass fiber are used to improve support performance, and homogeneous The mixing and vacuum forming process ensures even distribution and density of the material.
It significantly improves the high-temperature stability, low-temperature crack resistance and spalling resistance of asphalt mixtures, extends the service life of the pavement, reduces the frequency of maintenance and repair, and improves the quality and economic benefits of the road.
Smart Images

Figure CN118725592A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of asphalt pavement repair, in particular to an asphalt pavement repair material and a preparation method thereof. Background Art
[0002] Asphalt pavement repair is an indispensable part of road maintenance. It involves selecting high-quality repair materials to ensure that the repaired pavement can restore its original smoothness and durability. During the repair process, a professional construction team will accurately assess the degree of pavement damage and select the most suitable repair materials, such as high-polymer modified asphalt or specially formulated asphalt mixtures. These materials not only have excellent skid resistance and wear resistance, but can also maintain stable performance under extreme temperatures. Through meticulous construction operations, the repaired asphalt pavement will be completely renewed, providing a safe and comfortable environment for driving, while extending the service life of the road and reducing maintenance costs.
[0003] Existing asphalt pavements are widely used in road engineering. During long-term use, asphalt pavements are affected by traffic loads and the natural environment, and are prone to cracks, potholes and other defects. Existing asphalt repair materials have problems such as high temperature sensitivity and poor support performance during use, resulting in unsatisfactory repair effects and short service life. In order to solve these problems, it is necessary to develop a new asphalt pavement repair material that can reduce temperature sensitivity, improve support performance, and thus extend the service life of the repair material. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the deficiencies in the prior art, the present invention provides an asphalt pavement repair material and a preparation method thereof, which significantly reduces the temperature sensitivity of the asphalt material and improves the supporting performance of the asphalt mixture.
[0006] (II) Technical solution
[0007] To achieve the above object, the present invention provides the following technical solution: an asphalt pavement repair material and a preparation method thereof, comprising the following components in parts by weight:
[0008] 100 parts of asphalt, 10-20 parts of modifier, 5-15 parts of stabilizer, 2-5 parts of anti-stripping agent, 1-3 parts of reinforcing fiber, 50-100 parts of mineral powder.
[0009] Preferably, the modifier is at least one of SBS (styrene-butadiene-styrene block copolymer) or SBR (styrene-butadiene rubber).
[0010] Preferably, the stabilizer is at least one of polyethylene wax or EVA (ethylene-vinyl acetate copolymer).
[0011] Preferably, the anti-stripping agent is at least one of lime or calcium hydroxide.
[0012] Preferably, the reinforcing fiber is at least one of polypropylene fiber or glass fiber.
[0013] Preferably, the mineral powder is at least one of calcium carbonate powder or talcum powder.
[0014] Preferably, the steps include:
[0015] S1: Material preparation, weigh each component in proportion;
[0016] S2: Material mixing: asphalt, modifier, stabilizer, anti-stripping agent, reinforcing fiber and mineral powder are added into the mixer in sequence;
[0017] S3: heating, heating the mixed material to 160-180°C;
[0018] S4: Stirring. During the heating process, continue stirring for 30-60 minutes until the materials are evenly mixed;
[0019] S5: Forming: pour the evenly mixed material into the mold and compact it into shape;
[0020] S6: Cooling, cooling the material in the mold to room temperature, and taking out the molded repair material.
[0021] Preferably, the heating process adopts intermittent heating, with each heating lasting 10-20 minutes and an interval of 5-10 minutes.
[0022] Preferably, the stirring process adopts high-speed stirring, and the stirring speed is 300-500 rpm.
[0023] Preferably, the cooling process adopts natural cooling or air cooling.
[0024] (III) Beneficial effects
[0025] Compared with the prior art, the present invention provides an asphalt pavement repair material and a preparation method thereof, which have the following beneficial effects:
[0026] 1. By introducing SBS modifier and polyethylene wax, we can significantly improve the performance of asphalt, especially in terms of high temperature stability and low temperature crack resistance;
[0027] SBS modifier plays a core role in the asphalt modification process. This modifier effectively enhances the elasticity and toughness of asphalt through its unique molecular chain cross-linking mechanism. Under high temperature conditions, SBS modifier can significantly reduce the fluidity of asphalt materials, thereby maintaining the stability and durability of the road surface. This cross-linking effect enables asphalt to maintain its structural integrity at high temperatures and is not easy to soften or deform.
[0028] At the same time, the addition of polyethylene wax also brings significant performance improvement to asphalt. Through its unique chemical properties, polyethylene wax can change the crystal structure of asphalt and make it more stable. This change not only improves the heat resistance of asphalt, but also reduces its sensitivity to temperature. In low temperature environment, the effect of polyethylene wax is particularly significant. It can effectively prevent the brittle cracking of asphalt due to sudden temperature drop and maintain the integrity and safety of the road surface.
[0029] The combined use of SBS modifier and polyethylene wax has brought about a comprehensive performance improvement for asphalt materials. This modified asphalt can not only maintain stability at high temperatures, but also resist the formation of cracks at low temperatures, greatly extending the service life of the road surface. This advanced modification technology provides strong technical support for modern road construction.
[0030] 2. When polypropylene fibers or glass fibers are added to asphalt mixtures, their addition significantly enhances the supporting properties of the mixture, thus bringing multiple benefits to the pavement structure. These high-performance fibers are interwoven into a strong three-dimensional network structure within the asphalt. This structure not only enhances the overall strength and rigidity of the material, but also improves its internal cohesion, allowing the asphalt mixture to exhibit a higher bearing capacity when subjected to external loads.
[0031] Specifically, polypropylene fibers, with their excellent heat resistance, chemical corrosion resistance and high modulus, play the role of reinforcing bars in asphalt mixtures. They can effectively disperse and withstand the stress and pressure on the road surface, thereby significantly reducing the deformation and cracking of the road surface. In addition, polypropylene fibers can also improve the fatigue resistance of asphalt mixtures and extend the service life of the road surface.
[0032] Similarly, glass fibers play an indispensable role in asphalt mixtures with their excellent strength, durability and stability. They are closely combined with asphalt to form a stable whole, which enhances the shear strength and rutting resistance of the mixture. This three-dimensional network structure can effectively inhibit the fluidity of asphalt at high temperatures and maintain the flatness and stability of the road surface.
[0033] In general, the addition of polypropylene fiber and glass fiber brings excellent supporting performance to asphalt mixture, which not only improves the bearing capacity and stability of the road surface, but also reduces the frequency of road maintenance and repair. The application of these high-performance fibers is an indispensable part of modern road construction and is of great significance to improving road quality and extending service life.
[0034] 3. When anti-stripping agents, such as lime or calcium hydroxide, are introduced into asphalt mixtures, they significantly enhance the adhesion between asphalt and aggregate, providing a solid guarantee for the stability and durability of the road surface. The mechanism of action of these chemical additives is that they can react chemically with the polar components in asphalt to form a strong and stable chemical bonding layer;
[0035] Specifically, the anti-stripping agent can react with the acidic components (such as carboxylic acid) in asphalt to generate salt compounds. These salt compounds not only enhance the polarity of asphalt, but also promote the adhesion of asphalt to the surface of aggregate. Through this chemical reaction, a strong chemical bond is formed between asphalt and aggregate, which significantly improves the anti-stripping performance of asphalt mixture.
[0036] In addition, the addition of anti-stripping agent can also improve the water stability of asphalt mixture. In a humid environment, water can easily penetrate between asphalt and aggregate, resulting in reduced adhesion and causing pavement peeling. However, anti-stripping agent can react with hydrogen ions in water to reduce the acid value of asphalt, thereby reducing the effect of water on the adhesion between asphalt and aggregate. This improved water stability allows asphalt mixture to maintain good performance under harsh climatic conditions.
[0037] In summary, the addition of anti-stripping agents is one of the important means to improve the performance of asphalt mixtures. They significantly improve the stability and durability of the road surface by enhancing the adhesion between asphalt and aggregate and improving water stability. The application of these chemical additives not only extends the service life of the road surface, but also brings higher economic and social benefits to road construction and maintenance.
[0038] 4. The use of homogenous mixing and vacuum forming technology can ensure the uniform distribution of raw materials and reduce material waste. At the same time, vacuum forming can remove bubbles in the mixture, improve the density and molding quality of the material, and reduce the residue and loss of raw materials.
[0039] 5. The careful matching and synergistic effect of each component produce a significant enhancement effect in the material, thereby significantly improving the overall performance of the material. Specifically, when the SBS modifier and polypropylene fiber are combined, their respective advantages are complementary, and together they bring excellent elasticity and strength to the material. The SBS modifier significantly improves the elasticity and toughness of the material through the cross-linking effect of its molecular chain, so that the material can better restore its original state when subjected to external forces, reducing deformation and cracks. The polypropylene fiber forms a three-dimensional network structure inside the material, increasing the strength and rigidity of the material, and effectively preventing deformation and damage to the road surface. This synergistic effect significantly improves the elasticity and strength of the material, providing a strong guarantee for the stability and durability of the road surface.
[0040] On the other hand, the combined use of anti-stripping agent and polyethylene wax also demonstrated excellent synergistic effects. The anti-stripping agent enhanced the adhesion between asphalt and aggregate by reacting with the polar components in asphalt, effectively preventing the occurrence of pavement peeling, while polyethylene wax improved the material's heat resistance and temperature stability by changing the crystal structure of asphalt. This combination not only enhanced the material's adhesion, but also significantly improved its heat resistance, allowing the material to maintain good performance in high temperature environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 The present invention is a flowchart of the preparation process of an asphalt pavement repair material. DETAILED DESCRIPTION
[0042] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0043] Asphalt is a high molecular organic compound, a hydrocarbon substance mainly composed of carbon, hydrogen, oxygen and other elements. The polarity of asphalt refers to the number of charged parts in its molecules. Since asphalt is a non-polar molecule, there are no large number of polar functional groups in its molecules, so its polarity is relatively low. However, asphalt still contains some polar components, which mainly include:
[0044] Carboxylic acids: Asphalt may contain some polar functional groups containing oxygen, such as carboxylic acid groups. These groups exhibit certain polarity due to the presence of negatively charged oxygen atoms and positively charged hydrogen atoms.
[0045] Ketones and Aldehydes: Asphalt may produce some ketone and aldehyde compounds during processing and use, and these compounds also have certain polarity;
[0046] Sulfur compounds: Asphalt may contain some sulfur compounds, such as hydrogen sulfide, mercaptans, etc. These compounds are also polar;
[0047] When anti-stripping agents (such as lime or calcium hydroxide) are mixed with asphalt, they can react chemically with these polar components in the asphalt. Specifically, the cations (such as calcium ions) in the anti-stripping agent can react with the anions such as carboxylate ions in the asphalt to generate salt compounds. These salt compounds can enhance the polarity of asphalt, improve the adhesion between asphalt and aggregate, and prevent pavement peeling.
[0048] In addition, anti-stripping agents may also improve the polarity of asphalt and promote physical and chemical adsorption between asphalt and aggregate surface, thereby further improving the adhesion between asphalt and aggregate. This improvement in adhesion not only helps prevent pavement spalling, but also enhances the stability and durability of the pavement.
[0049] In summary, anti-stripping agents chemically react with polar components in asphalt (such as carboxylic acids, ketones, aldehydes and sulfur compounds) to enhance the polarity of asphalt and improve the adhesion between asphalt and aggregate, thereby preventing pavement spalling and improving the stability and durability of the pavement.
[0050] Embodiment 1:
[0051] An asphalt pavement repair material and a preparation method thereof, specifically comprising the following steps:
[0052] S1: Material preparation, weigh the following components by weight: 100 parts of asphalt, 15 parts of SBS modifier, 10 parts of polyethylene wax, 3 parts of lime, 2 parts of polypropylene fiber, and 75 parts of calcium carbonate powder;
[0053] S2: Material mixing: heat the asphalt to 150°C, add SBS modifier, polyethylene wax, lime, polypropylene fiber and calcium carbonate powder in sequence, and stir evenly;
[0054] S3: heating, heating the mixed material to 180°C and maintaining for 30 minutes;
[0055] S4: Stirring: During the heating process, continue stirring for 30 minutes to ensure that the materials are evenly mixed;
[0056] S5: Forming: pour the evenly mixed material into the mold and compact it into shape;
[0057] S6: Cooling, cooling the material in the mold to room temperature, and taking out the molded repair material.
[0058] Embodiment 2:
[0059] An asphalt pavement repair material and a preparation method thereof, specifically comprising the following steps:
[0060] S1: Material preparation, weigh the following components by weight: 100 parts of asphalt, 10 parts of SBS modifier, 5 parts of polyethylene wax, 2 parts of lime, 1 part of polypropylene fiber, and 50 parts of calcium carbonate powder;
[0061] S2: Material mixing: heat the asphalt to 150°C, add SBS modifier, polyethylene wax, lime, polypropylene fiber and calcium carbonate powder in sequence, and stir evenly;
[0062] S3: heating, heating the mixed material to 170°C and maintaining for 30 minutes;
[0063] S4: Stirring: During the heating process, continue stirring for 45 minutes to ensure that the materials are evenly mixed;
[0064] S5: Forming: pour the evenly mixed material into the mold and compact it into shape;
[0065] S6: Cooling, cooling the material in the mold to room temperature, and taking out the molded repair material.
[0066] Embodiment three:
[0067] An asphalt pavement repair material and a preparation method thereof, specifically comprising the following steps:
[0068] S1: Material preparation: weigh the following components by weight: 100 parts of asphalt, 20 parts of SBS modifier, 15 parts of polyethylene wax, 5 parts of lime, 3 parts of polypropylene fiber, and 100 parts of calcium carbonate powder;
[0069] S2: Material mixing: heat the asphalt to 150°C, add SBS modifier, polyethylene wax, lime, polypropylene fiber and calcium carbonate powder in sequence, and stir evenly;
[0070] S3: heating, heating the mixed material to 160°C and maintaining for 30 minutes;
[0071] S4: Stirring: During the heating process, continue stirring for 65 minutes to ensure that the materials are evenly mixed;
[0072] S5: Forming: pour the evenly mixed material into the mold and compact it into shape;
[0073] S6: Cooling, cooling the material in the mold to room temperature, and taking out the molded repair material.
[0074] Embodiment 4:
[0075] An asphalt pavement repair material and a preparation method thereof, specifically comprising the following steps:
[0076] S1: Material preparation, weigh the following components by weight: 100 parts of asphalt, 12 parts of SBR modifier, 7 parts of EVA, 2.5 parts of calcium hydroxide, 1.5 parts of glass fiber, and 60 parts of talc;
[0077] S2: Material mixing: heat the asphalt to 150°C, add SBR modifier, EVA, calcium hydroxide, glass fiber and talcum powder in sequence, and stir evenly;
[0078] S3: heating, heating the mixed material to 160°C and maintaining for 30 minutes;
[0079] S4: Stirring: During the heating process, continue stirring for 65 minutes to ensure that the materials are evenly mixed;
[0080] S5: Forming: pour the evenly mixed material into the mold and compact it into shape;
[0081] S6: Cooling, cooling the material in the mold to room temperature, and taking out the molded repair material.
[0082] Embodiment five:
[0083] An asphalt pavement repair material and a preparation method thereof, specifically comprising the following steps:
[0084] S1: Material preparation, weigh the following components by weight: 100 parts of asphalt, 18 parts of SBR modifier, 13 parts of EVA, 4.5 parts of calcium hydroxide, 2.5 parts of glass fiber, and 80 parts of talc;
[0085] S2: Material mixing: heat the asphalt to 150°C, add SBR modifier, EVA, calcium hydroxide, glass fiber and talcum powder in sequence, and stir evenly;
[0086] S3: heating, heating the mixed material to 180°C and maintaining for 30 minutes;
[0087] S4: Stirring: During the heating process, continue stirring for 30 minutes to ensure that the materials are evenly mixed;
[0088] S5: Forming: pour the evenly mixed material into the mold and compact it into shape;
[0089] S6: Cooling, cooling the material in the mold to room temperature, and taking out the molded repair material.
[0090] Comparative Example 1:
[0091] S1: Raw material preparation: weigh the following components by weight: 100 parts of asphalt, 10 parts of SBS modifier, 2 parts of lime, 50 parts of calcium carbonate powder;
[0092] S2: Material mixing: Heat the asphalt to 150°C, add SBS modifier, lime and calcium carbonate powder in sequence, and stir evenly;
[0093] S3: Heating: heating the mixed material to 160°C and maintaining for 20 minutes;
[0094] S4: Stirring: During the heating process, continue stirring for 30 minutes to ensure that the materials are evenly mixed;
[0095] S5: Molding: pour the evenly mixed material into the mold and compact it into shape;
[0096] S6: Cooling: Cool the material in the mold to room temperature and take out the molded repair material.
[0097] Comparative Example 2:
[0098] S1: Raw material preparation: weigh the following components by weight: 100 parts of asphalt, 12 parts of SBR modifier, 3 parts of calcium hydroxide, 60 parts of talc;
[0099] S2: Material mixing: Heat the asphalt to 155°C, add SBR modifier, calcium hydroxide and talcum powder in sequence, and stir evenly;
[0100] S3: Heating: Heat the mixed material to 165°C and keep it for 25 minutes;
[0101] S4: Stirring: During the heating process, continue stirring for 40 minutes to ensure that the materials are evenly mixed;
[0102] S5: Molding: pour the evenly mixed material into the mold and compact it into shape;
[0103] S6: Cooling: Cool the material in the mold to room temperature and take out the molded repair material.
[0104] The high temperature stability of seven groups of repair materials in Examples 1, 2, 3, 4, 5 and Comparative Examples 1 and 2 was comprehensively evaluated to obtain the critical temperature of high temperature resistance and take the average value. The higher the temperature value of the test result, the lower the temperature sensitivity of the group of repair materials. The temperature sensitivity test results of the repair materials are shown in Table 1. Therefore, the SBS modifier improves the elasticity and toughness of the asphalt and reduces the fluidity of the material at high temperature through the cross-linking effect of the molecular chain.
[0105] Table 1. Temperature sensitivity test results of Examples 1-5 and Comparative Examples 1-2
[0106] Test samples High temperature stability(℃) Example 1 78 Example 2 80 Example 3 79 Example 4 82 Example 5 79 Comparative Example 1 65 Comparative Example 2 67
[0107] The low-temperature crack resistance of seven groups of repair materials in Examples 1, 2, 3, 4, 5 and Comparative Examples 1 and 2 was comprehensively evaluated. The test temperature was minus 30°C, and the cracks in the repair materials were observed. The more severe the cracks, the worse the low-temperature crack resistance. Conversely, the lighter the cracks, the better the low-temperature crack resistance. The low-temperature crack resistance test results of the repair materials are shown in Table 2. Therefore, polyethylene wax improves the heat resistance and reduces the temperature sensitivity by changing the crystal structure of asphalt.
[0108] Table 2. Test results of low temperature crack resistance of Examples 1-5 and Comparative Examples 1-2
[0109] Test samples Low temperature crack resistance (-30℃) Example 1 No cracks Example 2 No cracks Example 3 No cracks Example 4 No cracks Example 5 No cracks Comparative Example 1 Minor cracks Comparative Example 2 Minor cracks
[0110] The support performance and anti-stripping performance of seven groups of repair materials in Examples 1, 2, 3, 4, 5 and Comparative Examples 1 and 2 were comprehensively evaluated. The support performance was tested using a TDW microcomputer-controlled fully automatic door-type gas spring tension and pressure testing machine. Pressure was applied under the same unit area, and the pressure value when the repair material was deformed was recorded. The larger the pressure value, the better the support performance of the group of repair materials. Conversely, the smaller the pressure value, the worse the support performance of the group of repair materials. The anti-stripping performance was tested using a HE-BLS series testing machine, and the anti-stripping rate was recorded. The higher the anti-stripping rate, the better the anti-stripping performance. Conversely, the lower the anti-stripping rate, the worse the anti-stripping performance. The low-temperature crack resistance test results of the repair material are shown in Table 3. Therefore, the fiber forms a three-dimensional network structure inside the material, which increases the strength and rigidity of the material, improves its bearing capacity, prevents road deformation, and the addition of the anti-stripping agent can improve the adhesion between asphalt and aggregate to prevent road peeling.
[0111] Table 3. Test results of support performance and anti-stripping performance of Examples 1-5 and Comparative Examples 1-2
[0112]
[0113]
[0114] The loss of raw materials during the production of seven groups of repair materials in Examples 1, 2, 3, 4, 5 and Comparative Examples 1 and 2 was recorded 5 times, and the average value was taken. The specific record results of the loss of raw materials during the production process are shown in Table 4. Therefore, vacuum forming can remove bubbles in the mixture, improve the density and molding quality of the material, and reduce the residue and loss of raw materials.
[0115] Table 4. Test results of raw material loss of Examples 1-5 and Comparative Examples 1-2
[0116] Test samples Raw material loss (%) Example 1 2.2 Example 2 2.3 Example 3 2.4 Example 4 2.2 Example 5 2.1 Comparative Example 1 5.5 Comparative Example 2 5.8
[0117] In summary, the present invention significantly reduces the temperature sensitivity of asphalt repair materials and improves their supporting performance by optimizing the formula and production process. Experimental results show that the repair material of the present invention has significantly improved high temperature stability, low temperature crack resistance and anti-stripping performance, and has significant economic and social benefits.
[0118] The above are only specific embodiments of the present invention, but the technical features of the present invention are not limited thereto. Any simple changes, equivalent replacements or modifications made based on the present invention to solve basically the same technical problems and achieve basically the same technical effects are all included in the protection scope of the present invention.
Claims
1. An asphalt pavement repair material, characterized in that: The composition comprises the following components by weight: 100 parts of asphalt, 10-20 parts of modifier, 5-15 parts of stabilizer, 2-5 parts of anti-stripping agent, 1-3 parts of reinforcing fiber, 50-100 parts of mineral powder.
2. The asphalt pavement repair material according to claim 1, characterized in that: The modifier is at least one of SBS (styrene-butadiene-styrene block copolymer) and SBR (styrene-butadiene rubber).
3. The asphalt pavement repair material according to claim 1, characterized in that: The stabilizer is at least one of polyethylene wax or EVA (ethylene-vinyl acetate copolymer).
4. The asphalt pavement repair material according to claim 1, characterized in that: The anti-stripping agent is at least one of lime or calcium hydroxide.
5. The asphalt pavement repair material according to claim 1, characterized in that: The reinforcing fiber is at least one of polypropylene fiber and glass fiber.
6. The asphalt pavement repair material according to claim 1, characterized in that: The mineral powder is at least one of calcium carbonate powder and talcum powder.
7. A method for preparing an asphalt pavement repair material, characterized in that: The following steps are involved: S1: Material preparation, weigh each component in proportion; S2: Material mixing: asphalt, modifier, stabilizer, anti-stripping agent, reinforcing fiber and mineral powder are added into the mixer in sequence; S3: heating, heating the mixed material to 160-180°C; S4: Stirring. During the heating process, continue stirring for 30-60 minutes until the materials are evenly mixed; S5: Forming: pour the evenly mixed material into the mold and compact it into shape; S6: Cooling, cooling the material in the mold to room temperature, and taking out the molded repair material.
8. The asphalt pavement repair material and preparation method thereof according to claim 7, characterized in that: The heating process adopts intermittent heating, with each heating lasting 10-20 minutes and an interval of 5-10 minutes.
9. The asphalt pavement repair material and preparation method thereof according to claim 7, characterized in that: The stirring process adopts high-speed stirring, and the stirring speed is 300-500 revolutions per minute.
10. The asphalt pavement repair material and preparation method thereof according to claim 7, characterized in that: The cooling process adopts natural cooling or air cooling.
Citation Information
Patent Citations
Traffic anti-track asphalt modifier and its modified asphalt and asphalt mixture
CN101165102A
Compound rubber asphalt
CN101205393A
Composite modified high-toughness asphalt mixture
CN105176106A
Directly-stirred SBS modifying agent and preparing method thereof
CN106147108A
Modified asphalt material for airport pavement, preparation method and applications thereof
CN106189290A