Bio-based polyurethane ink and preparation method thereof
By optimizing the raw material ratio and process conditions of bio-based polyurethane ink, a three-dimensional network structure is constructed, which solves the problem of poor adhesion of bio-based water-based polyurethane ink and achieves high adhesion, flexibility and degradability of the ink, which is suitable for many applications. printed materials.
Patent Information
- Application Number
- CN202410964168.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-01
AI Technical Summary
Bio-based water-based polyurethane ink has poor adhesion and is prone to cracking during use, which limits its wide application.
Using raw materials such as bio-based polyols, non-bio-based polyols, bio-based isocyanates and diisocyanates, a three-dimensional network structure is constructed by forming polyurethane chains, combined with hydrophilic chain extenders and amine catalysts, optimizing the raw material ratio and process conditions, and improving The compatibility, softness and adhesion of the ink form an ink coating that is not easy to crack.
The prepared bio-based polyurethane ink has the comprehensive properties of non-toxic, good adhesion, and not easy to crack. It is suitable for printing on textiles, leather, shoe materials, and paper packaging. It has good gloss, flexibility, and biodegradability, reducing the risk of environmental damage. Dependence on petrochemical raw materials.
Smart Images

Figure BDA0004951252000000061 
Figure BDA0004951252000000071 
Figure BDA0004951252000000081
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of inks, and more specifically, to a bio-based polyurethane ink and a preparation method thereof. Background Art
[0002] Polyurethane is a resin material made by the reaction of polyols and isocyanates. Due to its excellent adhesion and solvent resistance, it is widely used in plastics, inks, coatings, adhesives and other fields. However, the raw materials used in the synthesis of polyurethane are still derived from non-renewable petroleum resources, which consumes a large amount of petroleum resources in the production and manufacturing of polyurethane. In addition, the water-based polyurethane discarded after use is difficult to degrade, which has great harm to the environment. At present, as people attach great importance to the environment, the limited nature of petrochemical resources and the environmental problems caused by the development and utilization of petrochemical resources have prompted people to seek a green and sustainable need. Replacing some petroleum products with natural renewable resources is one of the main ways to alleviate the energy crisis and solve environmental pollution.
[0003] At present, the research on biomass materials from animal and plant resources is very active. Therefore, based on the advantages of bio-based materials being renewable, widely available and low-priced, the introduction of bio-based components into polyurethane materials can not only improve the mechanical properties, water resistance and degradability of polyurethane, but also have the advantages of natural materials such as being green and degradable. In addition, the ink prepared by introducing bio-based polyurethane has good durability when applied to fields such as textiles, so more and more developers are beginning to pay attention to the production of polyurethane using bio-based materials as raw materials.
[0004] The production and preparation of bio-based waterborne polyurethane is made by reacting bio-polyols as raw materials with isocyanates. Although bio-based waterborne polyurethane inks have certain water resistance and mechanical properties after curing, they have poor adhesion and are prone to cracking during use, which limits the wide application of bio-based waterborne polyurethanes. Summary of the invention
[0005] In order to solve the problem that bio-based water-based polyurethane ink has poor adhesion and is easy to crack during use, the present application provides a bio-based polyurethane ink and a preparation method thereof.
[0006] In a first aspect, the present application provides a bio-based polyurethane ink, which adopts the following technical solution: A bio-based polyurethane ink is prepared from the following raw materials in weight percentage: 50-90% bio-based polyurethane, 1-30% toner, 0.5-2% thickener, 3-5% curing agent, and 3.7-24.5% other additives; The bio-based polyurethane is prepared from the following raw materials in parts by weight: 50-70% of bio-based polyol, 0-10% of non-bio-based polyol, 5-15% of bio-based isocyanate, 10-20% of diisocyanate, 0.1-0.5% of catalyst, 3-10% of hydrophilic chain extender, 3-15% of amine catalyst, 3-10% of neutralizer and 3-20% of water.
[0007] The bio-based polyurethane of the present application is preferably a water-based bio-based polyurethane prepared by polymerization of bio-based polyols, bio-based isocyanates and diisocyanates, and is biodegradable, solvent-resistant, weather-resistant and chemical-resistant. By optimizing the raw materials and dosage ratio, the ink further prepared from the prepared bio-based polyurethane has comprehensive properties such as non-toxicity, good adhesion and not easy to crack, and the printing effect is stable.
[0008] The ink prepared is a water-based ink composition, which can be widely used on textile, leather, shoe material substrates and various paper packaging printing substrates. The ink coating has good adhesion to the substrate and has the advantages of good gloss, good flexibility and biodegradability. Most of the raw materials come from plant resources and are renewable, reducing dependence on petrochemical raw materials.
[0009] Among them, bio-based polyurethane, as the main film-forming substance, has good flexibility, wear resistance, adhesion, and is not easy to crack; toner provides the color of the ink, and is combined with other raw materials such as bio-based polyurethane to make the prepared ink layer have better gloss; the thickener adjusts the viscosity of the ink to adapt it to different printing needs; the curing agent can accelerate the drying speed of the ink and improve printing efficiency. Specifically, the curing agent is added and mixed before using the ink; other additives are used to improve the processing performance and storage stability of the ink.
[0010] The toner component in the ink of the present application is preferably a toner of a color such as watermelon red, sunflower yellow, rose red, cuttlefish black, etc., and the color can be specifically formulated according to the color requirements of the ink; and preferably ground before adding to the ink to improve the dispersibility of the toner in the ink system, so that the color distribution of the ink layer is uniform. More preferably, the ground toner can be mixed with water to prepare a pigment slurry, which is then added to the ink components. The fluidity of the pigment slurry promotes the mixing of the materials of the ink components, thereby making the toner dispersed evenly.
[0011] Preferably, in the bio-based polyurethane, the relative molecular mass of the bio-based polyol is 1000-5000, and commercially available Korean SK H2000, Korean SK H1000, Covestro 33085AU, etc. can be preferably selected.
[0012] Preferably, in the bio-based polyurethane, the non-bio-based polyol is a polyester polyol or a polyether polyol with a relative molecular mass of 1000-3000, more preferably, a relative molecular mass of 1000-2000, which can improve the softness and crystallinity of the bio-based polyurethane.
[0013] Preferably, in the bio-based polyurethane, the diisocyanate is at least one of toluene diisocyanate, isophorone diisocyanate and hexamethylene diisocyanate.
[0014] Preferably, in the bio-based polyurethane, the bio-based isocyanate is BASF MM103C.
[0015] The applicant has found that when there are more components such as color powder and filler in the ink composition, the uneven compatibility of the polyurethane component with the color powder and filler may lead to more powder in the local area of the ink coating, which may cause the local area to crack, become unstable in adhesion and fall off after curing.
[0016] Therefore, the present application adopts the above-mentioned technical scheme to make the hydroxyl groups (-OH) in bio-based polyols and non-bio-based polyols react with the isocyanate groups (-NCO) in bio-based isocyanates and diisocyanates to form polyurethane chains and construct a three-dimensional network structure, thereby improving the compatibility, softness, adhesion and weather resistance of bio-based polyurethane. When added to the ink components, it is evenly dispersed with other ink materials, and the ink coating formed by curing is not prone to cracking.
[0017] Preferably, in the bio-based polyurethane, the hydrophilic chain extender includes at least one of dimethylol propionic acid, dimethylol butyric acid, and dihydroxy sulfonate; and the amine chain extender includes at least one of ethylenediamine, hexamethylenediamine, isophoronediamine, and methylpentamethylenediamine.
[0018] By adopting the above technical scheme, the main role of chain extension and cross-linking is played in the synthesis of bio-based polyurethane. The hydrophilic chain extender can improve the wettability of the bio-based polyurethane obtained, reduce its surface tension, and improve its compatibility with other additives such as color powder, thereby reducing the situation where the ink layer is prone to cracking due to more local powder distribution in the ink layer due to uneven compatibility of powder particles; and the amine curing agent can accelerate the synthesis speed of polyurethane and improve the preparation efficiency.
[0019] Preferably, in the bio-based polyurethane, the neutralizer includes at least one of dimethylethanolamine, monoethanolamine, triethanolamine, and triethylamine; the catalyst is an organic bismuth catalyst or an organic zinc-bismuth alloy catalyst, and further preferably, the catalyst includes at least one of bismuth methanesulfonate, bismuth octoate, bismuth citrate, bismuth carboxylate, and zinc bismuth oxide.
[0020] By adopting the above technical scheme, the neutralizer can neutralize the acidic groups in the hydrophilic chain extender to form salts to adjust the pH value of the bio-based polyurethane, improve the stability of the bio-based polyurethane and the ink obtained, and reduce the phenomena of separation and precipitation during the storage process; and the catalyst can accelerate the polymerization reaction, so that the reaction can be carried out under mild conditions and reduce energy consumption costs. In this application, Jinshi K348 can be used as the catalyst.
[0021] Preferably, the preparation of the bio-based polyurethane comprises the following steps: Add bio-based polyol, non-bio-based polyol and catalyst to a reaction device equipped with a reflux condenser, then add diisocyanate and bio-based isocyanate, mix and react at 60-80°C for 1-3h, then add acetone to reduce viscosity, then add a hydrophilic chain extender, react for another 3-5h, cool to 25-40°C, then add acetone until the mixture is easy to stir, add a neutralizer to neutralize it while stirring, then add water according to the required solid content and emulsify and stir for 50-70s, add an amine chain extender to continue mixing and reacting, and finally distill off the acetone under reduced pressure to obtain a bio-based polyurethane.
[0022] By adopting the above technical scheme, a bio-based polyurethane with good compatibility, softness, adhesion and weather resistance can be prepared. It is stable in storage and can be evenly compatible with other ink materials when used in inks. The ink coating formed by curing is not prone to local uneven dispersion, resulting in local cracking and falling off.
[0023] Among them, polyol reacts with isocyanate to form a polyurethane prepolymer, and after being treated with a hydrophilic chain extender and an amine chain extender, the molecular chain of the polyurethane prepolymer is extended to form a stable bio-based polyurethane, and then emulsified with water to form a water-based bio-based polyurethane, which is compatible with other components of the ink and dispersed evenly. On the other hand, the entire preparation step is controlled under relatively mild conditions, and the added acetone can promote the dispersion of materials, promote the action of neutralizers and chain extenders, and finally it is easy to distill and remove without residue in the bio-based polyurethane component, thereby ensuring the stable storage of the bio-based polyurethane.
[0024] Preferably, in the ink, the thickener is at least one of a nonionic polyurethane associative thickener, an aqueous acrylic alkali swelling thickener, methyl cellulose, and a polyacrylic thickener, and the curing agent is at least one of a hydrophilic isocyanate, carbodiimide, and aziridine.
[0025] The thickener used in this application mainly plays an intermolecular association role to increase the viscosity of the ink, and commercially available Rohm and Haas ASE-60, Lamberti PS166, Digo 3030, etc. are preferably used. The curing agent used mainly cross-links with bio-based polyurethane to form a film, and commercially available Covestro 2655, Covestro 305, etc. are preferably used.
[0026] Preferably, in the ink, other additives include at least one of a filler, a dispersant, a leveling agent, a surfactant, a film-forming aid, and a defoaming agent.
[0027] The filler is in powder form, with a particle size of less than 3 μm, and can be evenly dispersed with other components of the ink; preferably, the filler is made of materials such as corn starch, cassava flour, wood flour, straw powder, recycled materials from waste clothes, recycled materials from waste rubber, etc., so that the filler component of the ink is environmentally friendly and improves resource utilization. In this application, based on the total weight of the ink, the amount of filler used is 0-15wt% of the total amount of the ink system.
[0028] The dispersant can improve the dispersibility of materials such as toner, filler, bio-based polyurethane in the ink system, making the ink materials uniform. Preferably, commercially available NNO dispersant, BYK-425, RJNM-0201, RJDA-0308, RJNM-0211, etc. can be selected. In this application, based on the total weight of the ink, the amount of the dispersant is 0.5-2wt% of the total amount of the ink system.
[0029] The leveling agent can improve the fluidity, ductility and adhesion of the ink system, making the ink easy to apply and use, having good adhesion to the substrate, and can reduce the shrinkage cavities and fisheye defects of the ink layer, so that the ink can form a continuous and smooth coating during the drying process. Preferably, the leveling agent can be a polyether-modified silicone leveling agent, a polyester-modified silicone leveling agent, a reactive silicone, a polysiloxane-polyether copolymer, etc., preferably commercially available TGEO Glide 410, TGEO Glide 450, BYK-333, etc. In the present application, based on the total weight of the ink, the amount of the leveling agent is 0.05-1wt% of the total amount of the ink system.
[0030] Surfactants can reduce the surface tension of ink, increase the fluidity of ink, improve the wettability of ink to the printing substrate, so that the ink can be more evenly distributed on the surface of the printing substrate, forming a continuous and smooth ink coating, and improving the adhesion and durability of the ink coating. Preferably, the surfactant can be dialkyl sulfosuccinate, polyoxyethylene glycol alkyl ester, polyphosphate, silicon-based surfactant, sodium polyacrylate, sulfonated styrene-sodium maleic acid salt, etc., preferably commercially available TEGO WET 260, Cytec OT75, TEGO WET 500, etc. can be selected. In this application, based on the total weight of the ink, the amount of surfactant used is 0.05-0.5wt% of the total amount of the ink system.
[0031] The defoamer can eliminate foam and inhibit foam regeneration during the preparation of the ink mixture, improve the coating performance of the ink, and help improve the adhesion between the ink and the substrate surface. Preferably, the defoamer can be emulsified silicone oil, silicone defoamer, high carbon alcohol fatty acid ester defoamer, acetylene glycol defoamer, etc., preferably commercially available TEGO 810, TEGO 902W, BYK-028. In this application, based on the total weight of the ink, the amount of the surfactant is 0.1-1wt% of the total amount of the ink system.
[0032] The film-forming aid can make the ink form a uniform film on the surface of the substrate with good adhesion. The formed ink layer has good wear resistance and weather resistance and is not prone to cracking. Preferably, the film-forming aid can be propylene glycol, ethylene glycol, polyethylene glycol, etc., preferably Dow PPH, TPM, DPM, etc. In this application, based on the total weight of the ink, the amount of the film-forming aid is 3-5wt% of the total amount of the ink system.
[0033] The present application can add water to adjust the viscosity of the ink according to the viscosity of the ink.
[0034] In a second aspect, the present application provides a method for preparing a bio-based polyurethane ink, which adopts the following technical scheme: adding bio-based polyurethane, color powder, and other additives into a stirring device, stirring at a speed of 3000-5000rpm for 25-35min, then adding a thickener to adjust the viscosity to 3000-5000CPS, stirring at a speed of 3000-5000rpm for 10-20min, and then adding a thickener to adjust the viscosity to 15000-18000CPS, and filtering to obtain a bio-based polyurethane ink semi-finished product; before application and use, mixing the bio-based polyurethane ink semi-finished product with a curing agent for 5-10min to obtain a bio-based polyurethane ink.
[0035] By adopting the above technical solution, the components of the ink are compatible and dispersed evenly, and the thickener is added in batches for multiple viscosity adjustment treatments, which can ensure that the material is evenly dispersed while the viscosity of the ink increases, and reduce the phenomenon of uneven local dispersion of the material when the viscosity increases. After the ink is finally cured, the coating formed is not easy to split or fall off.
[0036] In summary, this application has the following beneficial effects: 1. The ink prepared in the present application is a water-based ink composition, which can be widely used on textile, leather, shoe material substrates and various paper packaging printing substrates. The coating formed after curing has good gloss, good flexibility, good adhesion between the coating and the substrate, and the coating is not prone to cracking, falling off, etc. Most of the raw materials come from plants or renewable resources, are renewable and biodegradable, and reduce dependence on petrochemical raw materials.
[0037] 2. The bio-based polyurethane used in the ink of the present application is preferably a water-based bio-polyurethane polymerized by bio-based polyols, bio-based isocyanates, and diisocyanates, and has good compatibility, softness, adhesion, biodegradability, solvent resistance, weather resistance, and chemical resistance, making the ink non-toxic and having excellent overall performance. DETAILED DESCRIPTION
[0038] The present application is further described in detail below with reference to embodiments and comparative examples.
[0039] Preparation Example Preparation Example 1 A bio-based polyurethane, the preparation of which comprises the following steps: 50% bio-based polyol, 3% non-bio-based polyol (polyether polyol) and 0.3% catalyst (bismuth citrate) were added to a reaction device equipped with a reflux condenser, and then 15% toluene diisocyanate and 6% bio-based isocyanate (BASF MM103C) were added, and the mixture was mixed and reacted at 80°C for 1 hour, and then acetone was added to reduce the viscosity, and then 5% hydrophilic chain extender (sodium dihydroxysulfonate) was added, and the mixture was reacted for another 3 hours, cooled to 40°C, and then acetone was added until the mixture was easy to stir, and 6% neutralizer (triethanolamine) was added under stirring for neutralization, and then 5% water was added for emulsification and stirring for 50 seconds to adjust the solid content, and 9.7% amine chain extender (isophorone diamine) was added to continue the mixing reaction, and finally the acetone was distilled off under reduced pressure to obtain bio-based polyurethane.
[0040] Preparation Example 2-3 The difference between Preparation Example 2-3 and Preparation Example 1 is that the types, amounts and process conditions of raw materials are different, see Table 1 below for details: Table 1 Raw materials, dosage, and process parameters for preparing bio-based polyurethanes in Preparation Examples 1-3 Preparation Example 4 The difference between this preparation example and preparation example 2 is that acetone is not added to reduce viscosity in the preparation step, and the specific steps are as follows: 56% bio-based polyol, 5% non-bio-based polyol (polyether polyol) and 0.3% catalyst (Jinshi K348) were added to a reaction device equipped with a reflux condenser, and then 10% isophorone diisocyanate and 8% bio-based isocyanate (BASF MM103C) were added, mixed and reacted at 70°C for 2h, and then 6% hydrophilic chain extender (dimethylolpropionic acid) was added, and the reaction was continued for 4h, and the temperature was lowered to 40°C, and then 3% neutralizer (triethylamine) was added under stirring for neutralization, and then 6% water was added for emulsification and stirring for 60s to adjust the solid content, and 5.7% amine chain extender (methylpentanediamine) was added to continue mixing and reacting to obtain bio-based polyurethane.
[0041] Preparation Example 5 The difference between this preparation example and preparation example 2 is that the hydrophilic chain extender and the amine chain extender are added together in the preparation step. The specific steps are as follows: 56% bio-based polyol, 5% non-bio-based polyol (polyether polyol) and 0.3% catalyst (Jinshi K348) were added to a reaction device equipped with a reflux condenser, and then 10% isophorone diisocyanate and 8% bio-based isocyanate (BASF MM103C) were added, and the mixture was mixed and reacted at 70°C for 2 hours, and then acetone was added to reduce the viscosity, and then 6% hydrophilic chain extender (dimethylolpropionic acid) and 5.7% amine chain extender (methylpentanediamine) were added, and the mixture was reacted for another 4 hours, cooled to 40°C, and then acetone was added until the mixture was easy to stir, and 3% neutralizer (triethylamine) was added under stirring for neutralization, and then 6% water was added for emulsification and stirring for 60 seconds to adjust the solid content, and finally the acetone was distilled off under reduced pressure to obtain bio-based polyurethane.
[0042] Preparation Comparative Example 1 The difference between this preparation comparative example and Preparation Example 2 is that an equal amount of bio-based polyol is replaced by polyether polyol (Bluestar Dongda PPG polypropylene glycol DL-2000D), that is, non-bio-based polyol, diisocyanate and bio-based isocyanate are used as the synthetic main body in the preparation of bio-based polyurethane. The parameter conditions are detailed in Table 2 below.
[0043] Preparation Comparative Example 2 The difference between this preparation comparative example and Preparation Example 2 is that an equal amount of diisocyanate is replaced by bio-based isocyanate (SK H2000 from South Korea), that is, bio-based polyols, non-bio-based polyols, and bio-based isocyanates are used as the synthetic main bodies in the preparation of bio-based polyurethane. The parameter conditions are detailed in Table 2 below.
[0044] Preparation Comparative Example 3 The difference between this preparation comparative example and Preparation Example 2 is that an equal amount of bio-based isocyanate is replaced by diisocyanate (isophorone diisocyanate), that is, bio-based polyols, non-bio-based polyols, and diisocyanates are used as the synthetic main bodies in the preparation of bio-based polyurethane. The parameter conditions are detailed in Table 2 below.
[0045] Preparation Comparative Example 4 The difference between this preparation comparative example and Preparation Example 2 is that an equal amount of non-bio-based polyol is replaced by a bio-based polyol (SK H2000 from South Korea), and an equal amount of bio-based isocyanate is replaced by a diisocyanate (isophorone diisocyanate), that is, bio-based polyol and diisocyanate are used as the synthetic main body in the preparation of bio-based polyurethane. The parameter conditions are detailed in Table 2 below.
[0046] Preparation Comparative Example 5 The difference between this preparation comparative example and Preparation Example 2 is that an equal amount of the hydrophilic chain extender is replaced by an amine chain extender (methylpentamethylenediamine), that is, no hydrophilic chain extender is added in the preparation of the bio-based polyurethane. The parameter conditions are detailed in Table 2 below.
[0047] Table 2 Raw materials, dosage, and process parameters for preparing bio-based polyurethanes for comparative examples 1-5 Example
[0048] Example 1 A bio-based polyurethane ink, the preparation of which comprises the following steps: 70% of the bio-based polyurethane prepared in Preparation Example 1, 6% of color powder, 5% of filler (cassava flour with a particle size of less than 3 μm), 4.2% of film-forming aid (Dow PPH), 1.3% of dispersant (NNO dispersant), 8% of water, and 0.3% of defoamer (TEGO 810) were added to a stirring device, and dispersed and ground at room temperature and 5000 rpm for 25 minutes, and then 0.5% of thickener (Rohm and Haas ASE-60) was added to adjust the viscosity. At this time, the viscosity was measured to be 5331 CPS, and then stirred at 5000 rpm for 10 minutes, and then 0.3% of leveling agent (TGEO Glide 410), 0.2% of surfactant (TEGO WET 260), and 1.2% of thickener (Rohm and Haas ASE-60) were added, stirred evenly, and the viscosity was adjusted. At this time, the viscosity was measured to be 18276 CPS, and after filtering, a semi-finished bio-based polyurethane ink was obtained; Before application, the bio-based polyurethane ink semi-finished product was mixed with 3% curing agent (Covestro 2655) for 5-10 minutes to obtain the bio-based polyurethane ink.
[0049] The viscosity in this embodiment is measured using a rotational viscometer, specifically a Shanghai Instrument NDJ-8S type rotational viscometer.
[0050] Example 2-3 The difference between Example 2-3 and Example 1 is that the types, amounts and process conditions of raw materials are different, see Table 3 below for details.
[0051] Embodiment 4-5 The difference between Example 4-5 and Example 2 is that the sources of bio-based polyurethane are different. Specifically, Example 4 uses the bio-based polyurethane prepared in Preparation Example 4, and Example 5 uses the bio-based polyurethane prepared in Preparation Example 5, see Table 3 below: Table 3 Raw materials, dosage, and process parameters for preparing bio-based polyurethane inks of Examples 1-5 Example 6 The difference between Example 6 and Example 2 is that the thickener in the preparation method is added once and the viscosity is adjusted once. Specifically, 1.3% thickener is added after the leveling agent and the surfactant are added. The specific steps are as follows: 73% of the bio-based polyurethane prepared in Preparation Example 2, 10% of color powder, 5% of filler (corn starch with a particle size of less than 3 μm), 3% of film-forming aid (TPM), 1.1% of dispersant (BYK-425), and 0.8% of defoamer (TEGO 902W) were added to a stirring device, and dispersed and ground at room temperature and 4000 rpm for 35 minutes, and then 0.3% of leveling agent (TGEOGlide450), 0.5% of surfactant (TEGO WET 500), and 1.3% of thickener (Ningbodi PS166) were added, stirred evenly, and the viscosity was adjusted. At this time, the viscosity was measured to be 18936 CPS. After filtering, a semi-finished bio-based polyurethane ink was obtained; Before application, the bio-based polyurethane ink semi-finished product was mixed with 5% curing agent (Covestro 2655) for 5-10 minutes to obtain the bio-based polyurethane ink.
[0052] Example 7 The difference between Example 7 and Example 2 is that in the preparation method, all raw materials are added and mixed at one time, and the specific steps are as follows: 73% of the bio-based polyurethane prepared in Preparation Example 2, 10% toner, 5% filler (corn starch with a particle size of less than 3 μm), 3% film-forming aid (TPM), 1.1% dispersant (BYK-425), 0.8% defoamer (TEGO 902W), 0.3% leveling agent (TGEO Glide 450), 0.5% surfactant (TEGO WET 500), and 1.3% thickener (Ningbodi PS166) were added to a stirring device, and dispersed and ground at room temperature and 4000 rpm for 50 minutes. At this time, the viscosity was measured to be 20381 CPS. After filtering, a semi-finished bio-based polyurethane ink was obtained; Before application, the bio-based polyurethane ink semi-finished product was mixed with 5% curing agent (Covestro 2655) for 5-10 minutes to obtain the bio-based polyurethane ink.
[0053] Comparative Examples 1-6 The difference between Comparative Examples 1-6 and Example 2 is that the sources of bio-based polyurethane are different. Specifically, Comparative Example 1 uses the bio-based polyurethane prepared in Comparative Example 1, Comparative Example 2 uses the bio-based polyurethane prepared in Comparative Example 2, Comparative Example 3 uses the bio-based polyurethane prepared in Comparative Example 3, Comparative Example 4 uses the bio-based polyurethane prepared in Comparative Example 4, Comparative Example 5 uses the bio-based polyurethane prepared in Comparative Example 5, and Comparative Example 6 uses commercially available bio-based polyurethane. The parameter conditions are detailed in Table 4 below.
[0054] Table 4 Raw materials, dosage, and process parameters for preparing bio-based polyurethane inks of Comparative Examples 1-6 Performance Testing The adhesion, glossiness, softness, weather resistance and alkali resistance of the bio-based polyurethane inks prepared in the above Examples 1-7 and Comparative Examples 1-6 were coated on a substrate. The test method is as follows: (1) Preparation of substrate: Using BASF's Elastollan S85A TPU material, prepare a sheet with a length of 10 cm, a width of 5 cm, and a thickness of 2 cm for later use; (2) Ink coating: The bio-based polyurethane ink prepared in Examples 1-7 and Comparative Examples 1-6 was coated on one surface of the sheet, and the coating amount was controlled to be 10 g / m 2 The dry amount of each solution is equipped with at least four sheets coated with bio-based polyurethane ink; (3) Adhesion test: A tensile testing machine AI-7000-MU1 from High Speed Rail Testing Instruments (Dongguan) Co., Ltd. was used with a test speed of 80 mm / min to test the tensile force when the ink layer and the sheet are peeled off. Each set of solutions was tested 5 times, and the average value was taken as the average adhesion. (4) Alkali resistance test: The sheet sample with the ink layer was immersed in a 10% NaOH alkaline solution at 4°C for 24 hours. The sample was then taken out, rinsed with clean water, and dried to observe whether the ink layer was peeled off or missing. (5) Softness test: The sheet sample with the ink layer was bent using a bending machine GT-7071 produced by High Speed Rail Testing Instruments (Dongguan) Co., Ltd., and the number of bends when cracks or splits appeared on the ink layer was recorded; (6) Weather resistance test: For each group of solutions, a sheet sample with an ink layer (without adhesion test, alkali resistance test and bending treatment) was taken and bent using the cold resistance test machine GT-7006-v30 produced by High Speed Rail Testing Instrument (Dongguan) Co., Ltd. The test environment temperature was controlled at -20°C, and the number of bending times when cracks or cracks appeared on the ink layer was recorded; (7) Gloss test: A KESGA gloss meter WGG60-E4 was used to test the gloss of the cured ink layer at an angle of 60°.
[0055] The data of the above performance test are as follows: Table 5 Performance data of bio-based polyurethane inks of Examples 1-7 and Comparative Examples 1-6 It can be seen from the above performance data that the bio-based polyurethane ink prepared in the present application has good compatibility. Compared with the ink prepared by commercially available bio-based polyurethane, the ink coating formed after coating and curing in the present application has excellent weather resistance, solvent resistance, gloss and flexibility, and has good adhesion to the substrate. After multiple bending tests, it is not easy to crack or ink fall off.
[0056] The bio-based polyurethane used in Comparative Example 1 is specifically prepared using non-bio-based polyols, diisocyanates, and bio-based isocyanates as the main synthetic entities; the bio-based polyurethane used in Comparative Example 2 is specifically prepared using bio-based polyols, non-bio-based polyols, and bio-based isocyanates as the main synthetic entities; the bio-based polyurethane used in Comparative Example 3 is specifically prepared using bio-based polyols, non-bio-based polyols, and diisocyanates as the main synthetic entities; the bio-based polyurethane used in Comparative Example 4 is specifically prepared using bio-based polyols and diisocyanates as the main synthetic entities. The ink coating formed by curing the ink prepared in the above comparative examples 1-4 has significantly reduced adhesion to the substrate, and its softness and weather resistance are also reduced. After 80,000 bending tests at room temperature, the ink coating cracked and fell off. After 30,000 bending tests at -20°C, the ink coating cracked and fell off. This shows that the present application uses bio-based polyols, non-bio-based polyols, bio-based isocyanates, and diisocyanates as the main synthetic entities of bio-based polyurethanes. The prepared bio-based polyurethanes are applied to the preparation of inks and can be dispersed and compatible with other raw materials of the inks. The applied ink coating has excellent adhesion, gloss, softness and weather resistance, and is not prone to uneven adhesion of local ink to the substrate and uneven surface of the ink coating due to uneven dispersion or uneven compatibility, which affects the adhesion, softness and gloss of the ink coating.
[0057] The bio-based polyurethane used in Comparative Example 5 only uses amine chain extenders in the synthesis process. When the obtained bio-based polyurethane is applied to the ink, the adhesion between the ink coating and the substrate decreases, and the softness and weather resistance also decrease. The reason may be that the bio-based polyurethane obtained without using a hydrophilic chain extender has a low hydrophilicity, and its compatibility with other raw materials of the ink is reduced, resulting in uneven material dispersion and uneven application of the ink coating, resulting in cracks when bent 70,000 times at room temperature and 30,000 times in a -20°C environment, and the adhesion tension and gloss also decrease. This shows that the present application uses a hydrophilic chain extender in combination with an amine chain extender to make the obtained bio-based polyurethane compatible and uniform with other raw materials of the ink, and the cured ink coating has excellent substrate adhesion, gloss and softness.
[0058] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A bio-based polyurethane ink, characterized in that: It is made of the following raw materials in weight percentage: 50-90% bio-based polyurethane, 1-30% color powder, 0.5-2% thickener, 3-5% curing agent, and 3.7-24.5% other additives; The bio-based polyurethane is prepared from the following raw materials in weight percentage: 50-70% of bio-based polyol, 0-10% of non-bio-based polyol, 5-15% of bio-based isocyanate, 10-20% of diisocyanate, 0.1-0.5% of catalyst, 3-10% of hydrophilic chain extender, 3-15% of amine chain extender, 3-10% of neutralizer and 3-20% of water.
2. A bio-based polyurethane ink according to claim 1, characterized in that: In the bio-based polyurethane, the relative molecular mass of the bio-based polyol is 1000-5000, and the non-bio-based polyol is polyester polyol or polyether polyol, and the relative molecular mass is 1000-3000.
3. The bio-based polyurethane ink according to claim 1, characterized in that: In the bio-based polyurethane, the diisocyanate is at least one of toluene diisocyanate, isophorone diisocyanate and hexamethylene diisocyanate.
4. The bio-based polyurethane ink according to claim 1, characterized in that: In the bio-based polyurethane, the hydrophilic chain extender includes at least one of dimethylol propionic acid, dimethylol butyric acid, and dihydroxy sulfonate, and the amine chain extender includes at least one of ethylenediamine, hexamethylenediamine, isophoronediamine, and methylpentamethylenediamine.
5. The bio-based polyurethane ink according to claim 1, characterized in that: In the bio-based polyurethane, the neutralizer includes at least one of dimethylethanolamine, monoethanolamine, triethanolamine, and triethylamine, and the catalyst is an organic bismuth catalyst or an organic zinc-bismuth alloy catalyst.
6. A bio-based polyurethane ink according to claim 5, characterized in that: In the bio-based polyurethane, the catalyst includes at least one of bismuth methanesulfonate, bismuth octoate, bismuth citrate, bismuth carboxylate, and bismuth zinc oxide.
7. The bio-based polyurethane ink according to claim 1, characterized in that: The preparation of the bio-based polyurethane comprises the following steps: Add bio-based polyol, non-bio-based polyol and catalyst to a reaction device equipped with a reflux condenser, then add diisocyanate and bio-based isocyanate, mix and react at 60-80°C for 1-3h, then add acetone to reduce viscosity, then add a hydrophilic chain extender, react for another 3-5h, cool to 25-40°C, then add acetone until the mixture is easy to stir, add a neutralizer to neutralize it while stirring, then add water according to the required solid content and emulsify and stir for 50-70s, add an amine chain extender to continue mixing and reacting, and finally distill off the acetone under reduced pressure to obtain a bio-based polyurethane.
8. The bio-based polyurethane ink according to claim 1, characterized in that: In the ink, the thickener includes at least one of a nonionic polyurethane associative thickener, an aqueous acrylic acid alkali swelling thickener, methyl cellulose, and a polyacrylic thickener, and the curing agent is at least one of a hydrophilic isocyanate, a carbodiimide, and an aziridine.
9. The bio-based polyurethane ink according to claim 1, characterized in that: In the ink, other additives include at least one of fillers, dispersants, leveling agents, surfactants, defoamers, film-forming aids, and water.
10. A method for preparing a bio-based polyurethane ink according to any one of claims 1 to 9, characterized in that: The following steps are involved: Add bio-based polyurethane, color powder and other additives into a stirring device, stir at 3000-5000 rpm for 25-35 min, then add a thickener to adjust the viscosity to 3000-5000 CPS, stir at 3000-5000 rpm for 10-20 min, then add a thickener to adjust the viscosity to 15000-18000 CPS, filter, and obtain a semi-finished bio-based polyurethane ink; Before application, the bio-based polyurethane ink semi-finished product is mixed with a curing agent for 5-10 minutes to obtain the bio-based polyurethane ink.
Citation Information
Cited By
Preparation method of bio-based degradable water-based ink
CN121045877A