Preparation method of oil painting stick
By adding a specific proportion of stabilizers and antioxidants to the oil pastel preparation method, combined with molding processing, the problem of insufficient light resistance, heat resistance and aging resistance of oil pastels is solved, and the color stability and adhesion of oil pastels are achieved. improvement.
Patent Information
- Application Number
- CN202410573169.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-10
- Publication Date
- 2024-10-01
AI Technical Summary
Oil pastels on the market have deficiencies in stability, light resistance, heat resistance and aging resistance, making it difficult to maintain color stability and adhesion for a long time.
The oil pastel preparation method is adopted, by mixing pigment powder, vegetable oil, composite wax, aluminum stearate, fillers, stabilizers and antioxidants in specific proportions, and after molding processing, nonylphenol polyoxyethylene ether and antioxidants are added To improve the weather resistance of oil pastels.
It significantly improves the stability and UV resistance of oil pastels, ensures the color stability and adhesion of oil pastels over a long period of time, and has better weather resistance and stability.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of painting tool materials, and in particular to a method for preparing an oil pastel. Background Art
[0002] Oil pastels are a kind of oily colored painting pigment, which has the characteristics of delicate and smooth feel, good spreadability, excellent layering and mixing performance, bright colors, etc. The coating has a certain thickness, and the coating has strong adhesion and covering power on the paper surface, has texture, can fully show the oil painting effect, and meet the difficulty requirements of various painting techniques.
[0003] However, the paintings made with oil pastels currently on the market still have the problems of poor stability, light resistance, heat resistance and aging resistance. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a method for preparing an oil pastel, which improves the light resistance, heat resistance and aging resistance of the oil pastel.
[0005] The technical solution adopted by the present invention is:
[0006] A method for preparing an oil pastel, wherein: the oil pastel comprises the following components by weight: 10-14 parts of pigment powder, 40-42 parts of vegetable oil, 12-15 parts of composite wax, 1-3 parts of aluminum stearate, 22-26 parts of filler, 2-4 parts of stabilizer, 3-5 parts of nonylphenol polyoxyethylene ether, and 2-4 parts by weight of antioxidant;
[0007] The oil pastel preparation method comprises the following steps:
[0008] Step S1. 10-14 parts of pigment powder, 22-26 parts of filler, and 40-42 parts of vegetable oil are mixed uniformly to obtain a first mixture;
[0009] Step S2. 12-15 parts of the composite wax and 1-3 parts of aluminum stearate are heated and melted, and mixed with the heated first mixture to obtain a second mixture;
[0010] Step S3. Add 2-4 parts of a stabilizer, 3-5 parts of nonylphenol polyoxyethylene ether and 2-4 parts of an antioxidant to the second mixture in sequence, and disperse them evenly to obtain a third mixture;
[0011] Step S4: inject the third mixture into a molding process to obtain an oil pastel.
[0012] Preferably, in the method for preparing oil pastels, the vegetable oil comprises 20-22 parts of olive oil, 10-15 parts of coconut oil, and 5-10 parts of linseed oil.
[0013] Preferably, in the method for preparing oil pastels, the filler is selected from one or more of calcium carbonate, kaolin, talcum powder, white carbon black, aluminum silicate, aluminum hydroxide, and barium sulfate.
[0014] Preferably, in the method for preparing oil pastels, the composite wax comprises 5-8 parts of microcrystalline wax, 2-4 parts of palm wax, and 3-5 parts of polyoxyethylene ether.
[0015] Preferably, in the method for preparing oil pastels, the stabilizer comprises 1-2 parts of pentaerythritol and 1-2 parts of barium stearate.
[0016] Preferably, in the method for preparing oil pastels, the antioxidant comprises 1-2 parts of 2,6-tert-butyl-4-methylphenol, 0.1-1 parts of titanium dioxide and 0.9-1 parts of 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole.
[0017] Preferably, in the method for preparing oil pastels, the melting temperature of step S2 is 90-100° C. and the melting time is 80-100 min.
[0018] Preferably, in the method for preparing oil pastels, the molding process in step S4 includes a cooling step, and the cooling temperature is 10-15°C.
[0019] Advantages of the present invention:
[0020] (1) The method for preparing oil pastels of the present invention significantly improves the stability and UV resistance of the obtained oil pastels by adding a stabilizer, nonylphenol polyoxyethylene ether and an antioxidant. The stabilizer includes pentaerythritol and barium stearate, and the antioxidant includes 2,6-tert-butyl-4-methylphenol, titanium dioxide and 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole. It shows that pentaerythritol, barium stearate, nonylphenol polyoxyethylene ether and 2,6-tert-butyl-4-methylphenol, titanium dioxide and 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole have obvious synergistic effects, so that the oil painting has long-term color stability and better weather resistance and stability.
[0021] (2) The method for preparing oil pastels of the present invention uses microcrystalline wax, palm wax and polyoxyethylene ether as composite wax, adds olive oil, coconut oil and linseed oil to enhance adhesion, and ensures smoothness of painting by adding polyoxyethylene ether. DETAILED DESCRIPTION
[0022] The present invention will be further described below in conjunction with specific embodiments.
[0023] Example 1
[0024] A method for preparing an oil pastel, wherein: the oil pastel comprises the following components by weight: 10 parts of pigment powder, 40 parts of vegetable oil, 12 parts of composite wax, 1 part of aluminum stearate, 22 parts of filler, 2 parts of stabilizer, 3 parts of nonylphenol polyoxyethylene ether, and 2 parts by weight of antioxidant;
[0025] The oil pastel preparation method comprises the following steps:
[0026] Step S1. 10 parts of pigment powder, 22 parts of filler, and 40 parts of vegetable oil are mixed evenly to obtain a first mixture;
[0027] Step S2. 12 parts of the composite wax and 1 part of aluminum stearate are heated and melted, and mixed with the heated first mixture to obtain a second mixture;
[0028] Step S3. Add 2 parts of stabilizer, 3 parts of nonylphenol polyoxyethylene ether and 1 part of antioxidant to the second mixture in sequence, and disperse them evenly to obtain a third mixture;
[0029] Step S4: inject the third mixture into a molding process to obtain an oil pastel.
[0030] The vegetable oil includes 20 parts of olive oil, 10 parts of coconut oil and 10 parts of linseed oil; the filler is calcium carbonate, the composite wax includes 5 parts of microcrystalline wax, 2 parts of palm wax and 5 parts of polyoxyethylene ether; the stabilizer includes 1 part of pentaerythritol and 1 part of barium stearate; the antioxidant includes 1 part of 2,6-tert-butyl-4-methylphenol, 0.1 part of titanium dioxide and 0.9 part of 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole.
[0031] The melting temperature of step S2 is 90°C and the melting time is 100 minutes; the molding process of step S4 includes a cooling step and the cooling temperature is 10°C.
[0032] Example 2
[0033] A method for preparing an oil pastel, wherein the oil pastel comprises the following components by weight: 12 parts of pigment powder, 41 parts of vegetable oil, 13 parts of composite wax, 2 parts of aluminum stearate, 25 parts of filler, 3 parts of stabilizer, 4 parts of nonylphenol polyoxyethylene ether, and 3 parts by weight of antioxidant;
[0034] The oil pastel preparation method comprises the following steps:
[0035] Step S1. 12 parts of pigment powder, 25 parts of filler, and 41 parts of vegetable oil are mixed evenly to obtain a first mixture;
[0036] Step S2. 13 parts of the composite wax and 2 parts of aluminum stearate are heated and melted, and mixed with the heated first mixture to obtain a second mixture;
[0037] Step S3. Add 3 parts of stabilizer, 4 parts of nonylphenol polyoxyethylene ether and 3 parts of antioxidant to the second mixture in sequence, and disperse them evenly to obtain a third mixture;
[0038] Step S4: inject the third mixture into a molding process to obtain an oil pastel.
[0039] The vegetable oil includes 21 parts of olive oil, 10 parts of coconut oil and 10 parts of linseed oil; the filler is calcium carbonate; the composite wax includes 6 parts of microcrystalline wax, 3 parts of palm wax and 4 parts of polyoxyethylene ether; the stabilizer includes 1 part of pentaerythritol and 2 parts of barium stearate; the antioxidant includes 1 part of 2,6-tert-butyl-4-methylphenol, 1 part of titanium dioxide and 1 part of 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole.
[0040] The melting temperature of step S2 is 90°C and the melting time is 100 minutes; the molding process of step S4 includes a cooling step and the cooling temperature is 10°C.
[0041] Example 3
[0042] A method for preparing an oil pastel, wherein the oil pastel comprises the following components by weight: 14 parts of pigment powder, 42 parts of vegetable oil, 15 parts of composite wax, 3 parts of aluminum stearate, 26 parts of filler, 4 parts of stabilizer, 5 parts of nonylphenol polyoxyethylene ether, and 4 parts by weight of antioxidant;
[0043] The oil pastel preparation method comprises the following steps:
[0044] Step S1. 14 parts of pigment powder, 26 parts of filler, and 42 parts of vegetable oil are mixed evenly to obtain a first mixture;
[0045] Step S2. 15 parts of the composite wax and 3 parts of aluminum stearate are heated and melted, and mixed with the heated first mixture to obtain a second mixture;
[0046] Step S3. Add 4 parts of stabilizer, 5 parts of nonylphenol polyoxyethylene ether and 4 parts of antioxidant to the second mixture in sequence and disperse them evenly to obtain a third mixture;
[0047] Step S4: inject the third mixture into a molding process to obtain an oil pastel.
[0048] The vegetable oil includes 22 parts of olive oil, 15 parts of coconut oil and 5 parts of linseed oil; the filler is calcium carbonate; the composite wax includes 8 parts of microcrystalline wax, 4 parts of palm wax and 3 parts of polyoxyethylene ether; the stabilizer includes 2 parts of pentaerythritol and 2 parts of barium stearate; the antioxidant includes 2 parts of 2,6-tributyl-4-methylphenol, 1 part of titanium dioxide and 1 part of 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole.
[0049] The melting temperature of step S2 is 90°C and the melting time is 100 minutes; the molding process of step S4 includes a cooling step and the cooling temperature is 10°C.
[0050] Comparative Example 1
[0051] A method for preparing an oil pastel, wherein: the oil pastel comprises the following components by weight: 10 parts of pigment powder, 40 parts of vegetable oil, 12 parts of composite wax, 1 part of aluminum stearate, 22 parts of filler, 3 parts of nonylphenol polyoxyethylene ether, and 2 parts by weight of antioxidant;
[0052] The oil pastel preparation method comprises the following steps:
[0053] Step S1. 10 parts of pigment powder, 22 parts of filler, and 40 parts of vegetable oil are mixed evenly to obtain a first mixture;
[0054] Step S2. 12 parts of the composite wax and 1 part of aluminum stearate are heated and melted, and mixed with the heated first mixture to obtain a second mixture;
[0055] Step S3. Add 3 parts of nonylphenol polyoxyethylene ether and 1 part of antioxidant to the second mixture in sequence and disperse them evenly to obtain a third mixture;
[0056] Step S4: inject the third mixture into a molding process to obtain an oil pastel.
[0057] The vegetable oil includes 20 parts of olive oil, 10 parts of coconut oil and 10 parts of linseed oil. The filler is calcium carbonate, the composite wax includes 5 parts of microcrystalline wax, 2 parts of palm wax and 5 parts of polyoxyethylene ether; the antioxidant includes 1 part of 2,6-tert-butyl-4-methylphenol, 0.1 part of titanium dioxide and 0.9 part of 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole.
[0058] The melting temperature of step S2 is 90°C and the melting time is 100 minutes; the molding process of step S4 includes a cooling step and the cooling temperature is 10°C.
[0059] Comparative Example 2
[0060] A method for preparing an oil pastel, wherein the oil pastel comprises the following components by weight: 12 parts of pigment powder, 41 parts of vegetable oil, 13 parts of composite wax, 2 parts of aluminum stearate, 25 parts of filler, 3 parts of stabilizer, and 3 parts by weight of antioxidant;
[0061] The oil pastel preparation method comprises the following steps:
[0062] Step S1. 12 parts of pigment powder, 25 parts of filler, and 41 parts of vegetable oil are mixed evenly to obtain a first mixture;
[0063] Step S2. 13 parts of the composite wax and 2 parts of aluminum stearate are heated and melted, and mixed with the heated first mixture to obtain a second mixture;
[0064] Step S3. Add 3 parts of stabilizer and 3 parts of antioxidant to the second mixture in sequence and disperse them evenly to obtain a third mixture;
[0065] Step S4: inject the third mixture into a molding process to obtain an oil pastel.
[0066] The vegetable oil includes 21 parts of olive oil, 10 parts of coconut oil and 10 parts of linseed oil; the filler is calcium carbonate; the composite wax includes 6 parts of microcrystalline wax, 3 parts of palm wax and 4 parts of polyoxyethylene ether; the stabilizer includes 1 part of pentaerythritol and 2 parts of barium stearate; the antioxidant includes 1 part of 2,6-tert-butyl-4-methylphenol, 1 part of titanium dioxide and 1 part of 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole.
[0067] The melting temperature of step S2 is 90°C and the melting time is 100 minutes; the molding process of step S4 includes a cooling step and the cooling temperature is 10°C.
[0068] Comparative Example 3
[0069] A method for preparing an oil pastel, wherein the oil pastel comprises the following components by weight: 14 parts of pigment powder, 42 parts of vegetable oil, 15 parts of composite wax, 3 parts of aluminum stearate, 26 parts of filler, 4 parts of stabilizer, 5 parts of nonylphenol polyoxyethylene ether, and 4 parts by weight of antioxidant;
[0070] The oil pastel preparation method comprises the following steps:
[0071] Step S1. 14 parts of pigment powder, 26 parts of filler, and 42 parts of vegetable oil are mixed evenly to obtain a first mixture;
[0072] Step S2. 15 parts of the composite wax and 3 parts of aluminum stearate are heated and melted, and mixed with the heated first mixture to obtain a second mixture;
[0073] Step S3. Add 4 parts of stabilizer, 5 parts of nonylphenol polyoxyethylene ether and 4 parts of antioxidant to the second mixture in sequence and disperse them evenly to obtain a third mixture;
[0074] Step S4: inject the third mixture into a molding process to obtain an oil pastel.
[0075] The vegetable oil includes 22 parts of olive oil, 15 parts of coconut oil, and 5 parts of linseed oil; the filler is calcium carbonate; the composite wax includes 8 parts of microcrystalline wax, 4 parts of palm wax, and 3 parts of polyoxyethylene ether; the stabilizer includes 2 parts of pentaerythritol and 2 parts of barium stearate; and the antioxidant is 4 parts of 2,6-tributyl-4-methylphenol.
[0076] The melting temperature of step S2 is 90°C and the melting time is 100 minutes; the molding process of step S4 includes a cooling step and the cooling temperature is 10°C.
[0077] The performance test results of Examples 1-3 and Comparative Examples 1-3 are listed below. The test results are shown in Table 1.
[0078] Table 1
[0079] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Flexural strength(N) 11 12 11 11 10 10 Oil painting color difference 0.03 0.02 0.04 0.86 0.81 0.72 UV test(h) >24 >24 >24 14 18 12
[0080] The oil pastels of Examples 1-3 and Comparative Examples 1-3 were applied on oil painting paper and placed at room temperature for half a year. The color difference of the oil paintings before and after the placement was measured. It can be seen from Table 1 that the color difference of the oil paintings of Example 1, Example 2, and Example 3 are 0.03, 0.02, and 0.04, respectively, and the color difference of the oil paintings of Comparative Examples 1-3 is 0.86, 0.81, and 0.72. The color difference of the oil paintings of Examples 1-3 changes very little, and the color stability of the oil paintings can be maintained after long-term placement; the embodiments of the present invention have a longer UV resistance time than the comparative examples, that is, better weather resistance and stability.
[0081] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing an oil pastel, characterized in that: The oil pastel comprises the following components by weight: 10-14 parts of pigment powder, 40-42 parts of vegetable oil, 12-15 parts of composite wax, 1-3 parts of aluminum stearate, 22-26 parts of filler, 2-4 parts of stabilizer, 3-5 parts of nonylphenol polyoxyethylene ether, and 2-4 parts by weight of antioxidant; The oil pastel preparation method comprises the following steps: Step S1. 10-14 parts of pigment powder, 22-26 parts of filler, and 40-42 parts of vegetable oil are mixed uniformly to obtain a first mixture; Step S2. 12-15 parts of the composite wax and 1-3 parts of aluminum stearate are heated and melted, and mixed with the heated first mixture to obtain a second mixture; Step S3. Add 2-4 parts of a stabilizer, 3-5 parts of nonylphenol polyoxyethylene ether and 2-4 parts of an antioxidant to the second mixture in sequence, and disperse them evenly to obtain a third mixture; Step S4: inject the third mixture into a molding process to obtain an oil pastel.
2. The method for preparing oil pastels according to claim 1, wherein: The vegetable oil comprises 20-22 parts of olive oil, 10-15 parts of coconut oil and 5-10 parts of linseed oil.
3. The method for preparing oil pastels according to claim 1, wherein: The filler is selected from one or more of calcium carbonate, kaolin, talc, white carbon black, aluminum silicate, aluminum hydroxide, and barium sulfate.
4. The method for preparing oil pastels according to claim 1, wherein: The composite wax comprises 5-8 parts of microcrystalline wax, 2-4 parts of palm wax and 3-5 parts of polyoxyethylene ether.
5. The method for preparing oil pastels according to claim 1, wherein: The stabilizer includes 1-2 parts of pentaerythritol and 1-2 parts of barium stearate.
6. The method for preparing oil pastels according to claim 1, wherein: The antioxidant comprises 1-2 parts of 2,6-tert-butyl-4-methylphenol, 0.1-1 parts of titanium dioxide and 0.9-1 parts of 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole.
7. The method for preparing oil pastels according to claim 1, wherein: The melting temperature of step S2 is 90-100° C., and the melting time is 80-100 min.
8. The method for preparing oil pastels according to claim 1, wherein: The molding process in step S4 includes a cooling step, and the cooling temperature is 10-15°C.
Citation Information
Patent Citations
Calligraphy and painting protecting mounting film
CN105237921A
Antioxidant and heat-resistant PVC modified material
CN108503992A
PVC preparation process for wire plastic particles
CN109354808A
Barium-zinc stabilizer and production method thereof
CN109535587A
Weather-resistant calcium-zinc stabilizer for PVC and preparation method thereof
CN110358215A