Modified graphene PTFE-based coating and preparation method thereof
Copper-coated graphene powder is prepared by modifying copper-coated graphene powder with coupling agent and in-situ generation method, which solves the problem of insufficient wear resistance and corrosion resistance of PTFE-based coating in seawater environment, and achieves a better Good coating performance and extended equipment life.
Patent Information
- Application Number
- CN202410921082.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-10
AI Technical Summary
Existing PTFE-based coatings have insufficient wear resistance and corrosion resistance in seawater environments. Graphene is prone to agglomeration and has weak interface bonding with the PTFE matrix, causing the coating to be easily damaged by corrosion in seawater.
Coupling agent is used to modify copper-coated graphene powder, and copper-coated graphene powder is prepared through in-situ generation method to improve the coverage and dispersion of graphene on the PTFE surface, and coat copper nanoparticles on the graphene surface. , enhance the interfacial bonding force between PTFE matrix and filler.
The wear resistance and corrosion resistance of PTFE-based coatings are significantly improved, extending the service life of marine equipment and avoiding early wear and structural damage caused by seawater corrosion.
Smart Images

Figure CN118725701A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, in particular to a modified graphene PTFE-based coating and a preparation method thereof. Background Art
[0002] In the marine field, because seawater has high corrosiveness and complex mechanical stress, traditional materials are difficult to meet the long-term use requirements in the fields of marine engineering and shipbuilding. The PTFE-based three-layer self-lubricating composite material is composed of a metal matrix, an intermediate bonding layer and a PTFE-based coating. Among them, the metal matrix can provide mechanical strength, the intermediate bonding layer can ensure the firm bonding between the layers, and the PTFE-based coating can provide certain self-lubrication and wear-resistant properties. If this material is used in the seawater field, although it can reduce the friction and wear of mechanical parts to a certain extent, its wear resistance cannot meet the requirements of long-term application in the seawater field.
[0003] Since seawater is highly corrosive, and the internal structure of the PTFE-based coating in the prior art is relatively loose, after long-term use, the corrosive medium in the seawater is easy to penetrate into the metal matrix, resulting in the substrate coated with the PTFE-based coating being corroded. Graphene, as a nano-scale material, has excellent mechanical strength and corrosion resistance. When graphene is added to the PTFE matrix, the wear resistance and mechanical properties of the prepared coating can be significantly improved, while maintaining the original chemical corrosion resistance and low friction coefficient characteristics of the PTFE body. However, in the prior art, graphene will have the following problems in the process of enhancing the performance of the PTFE-based coating: First, graphene is easy to agglomerate, and it cannot be well dispersed when added to the PTFE matrix, which easily leads to the prepared coating being coated on the substrate. After the wear resistance and mechanical properties of the substrate are very different; second, the interface between graphene and the PTFE matrix is weak, resulting in poor adhesion between graphene and the PTFE matrix; third, the PTFE matrix itself has many micropores and cracks. The first and second problems mentioned above will seriously affect the wear resistance of the prepared PTFE-based coating. The third problem will cause the corrosive medium in seawater to penetrate into the metal substrate through the PTFE matrix, resulting in the substrate (i.e., the metal substrate) coated with the PTFE-based coating still being susceptible to corrosion by seawater in a seawater environment, resulting in its poor corrosion resistance. Summary of the invention
[0004] In order to solve the problem of poor wear resistance and corrosion resistance of PTFE-based coatings in the prior art, the present invention provides a modified graphene PTFE-based coating.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is: a modified graphene PTFE-based coating, the raw materials of which are calculated by weight: 40-80 parts of PTFE powder, 1-10 parts of coupling agent, 5-15 parts of aramid, 0.5-8 parts of graphene, 70-90 parts of copper nitrate trihydrate, and 15-25 parts of polyimide.
[0006] As a further improvement of the above scheme, the copper nitrate trihydrate is used to mix with the graphene to prepare copper-coated graphene powder, and the coupling agent is used to modify the copper-coated graphene powder to obtain modified graphene powder.
[0007] As a further improvement of the above scheme, the coupling agent is one or more of heptadecafluorooctyl triethoxysilane, γ-aminopropyl triethoxysilane, and tridecafluorooctyl triethoxysilane.
[0008] As a further improvement of the above solution, the coupling agent is used to respectively improve the interfacial bonding force between the aramid and the PTFE, the interfacial bonding force between the graphene and the PTFE, and the interfacial bonding force between the polyimide and the PTFE.
[0009] As a further improvement of the above solution, the particle size of the graphene is 2 μm-7 μm.
[0010] A method for preparing a modified graphene PTFE-based coating comprises the following steps:
[0011] preparing copper-coated graphene powder;
[0012] Add the coupling agent to anhydrous ethanol, stir to dissolve it, and obtain a mixed solution 1; then add the prepared copper-coated graphene powder to the mixed solution 1, and perform ultrasound and stirring on the mixed solution 1 to obtain the mixed solution 2; then adjust the pH of the mixed solution 2 with hydrochloric acid so that the pH of the mixed solution 2 is 4-5; then heat the mixed solution 2 in a water bath, cool it to room temperature, wash it with deionized water, filter it, and vacuum dry it to obtain the modified graphene powder;
[0013] Adding the modified graphene powder to the PTFE dispersion, stirring, filtering and drying in sequence to obtain a modified graphene PTFE composite powder;
[0014] Aramid and polyimide are added to the modified graphene PTFE composite powder respectively, and the mixture is evenly mixed to obtain a mixed mud material;
[0015] The mixed mud is evenly spread on the copper powder plate, and rolled using a rolling mill to obtain a plate with the mixed mud coated on the surface;
[0016] The plate with the surface coated with the mixed mud is then placed in a sintering device for plasticization at a plasticizing temperature of 370°C, a plasticizing time of 4 hours, and a heating rate of 10°C / min. After sintering, the plate is cooled to room temperature with the sintering device to obtain a plate with the modified graphene PTFE-based coating.
[0017] As a further improvement of the above solution, the copper-coated graphene powder is prepared by an in-situ generation method.
[0018] As a further improvement of the above scheme, the preparation of the copper-coated graphene powder comprises the following steps:
[0019] Graphene was dispersed in 600 mL of ethanol solution, and then ultrasonicated and magnetically stirred to obtain a mixed solution 3;
[0020] Adding copper nitrate trihydrate and glucose solution to the mixed solution three in sequence, and stirring for a period of time to obtain a mixed solution four;
[0021] A NaOH solution with a concentration of 5 mol / L and a volume of 500 mL was added dropwise to the mixed solution four three times, stirred for 3 hours after the addition was completed, and then the stirred solution was filtered to obtain a solid product; the solid product was washed with deionized water for multiple times and filtered and dried to obtain the copper-coated graphene powder.
[0022] As a further improvement of the above scheme, the PTFE dispersion is obtained by adding PTFE powder into distilled water and performing mechanical stirring and ultrasonic dispersion for 2 hours.
[0023] As a further improvement of the above scheme, the mixed solution 2 with adjusted pH value is reacted in a water bath at 50° C. for 30 minutes, then heated to 70° C. and reacted for 30 minutes, and finally cooled to room temperature.
[0024] As a further improvement of the above scheme, the mixed solution after cooling to room temperature is washed and filtered three times with deionized water, and vacuum dried at 60° C. to obtain the modified graphene powder.
[0025] As a further improvement of the above scheme, after the prepared modified graphene powder is added to the PTFE dispersion, it is mechanically stirred for 1 hour, then vacuum filtered, and finally dried at 100° C. for 9 hours to obtain a modified graphene PTFE composite powder.
[0026] A modified graphene PTFE-based composite plate comprises a modified graphene PTFE-based coating prepared by the above-mentioned preparation method.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] (1) In the present invention, a coupling agent is used to couple and modify the copper-coated graphene, thereby increasing the coverage of graphene on the PTFE surface, improving the micropores and crack defects of the PTFE matrix itself, and improving the corrosion resistance of the prepared PTFE-based coating.
[0029] (2) The present invention prepares copper-coated graphene powder by an in-situ generation method, so that copper nanoparticles can be evenly distributed on the surface and wrinkles of the graphene sheet, thereby improving the dispersibility of graphene and enhancing the wear resistance of the prepared PTFE-based coating.
[0030] (3) The present invention can effectively improve the interfacial bonding force between graphene and the PTFE matrix by coating copper nanoparticles on the surface of graphene, thereby enhancing the bonding force between the PTFE matrix and the filler in the prepared PTFE-based coating, thereby improving its wear resistance.
[0031] (4) The PTFE-based coating prepared by the present invention has good wear resistance and corrosion resistance, and can be applied to equipment in the marine field. By coating some devices in the marine field with the PTFE-based coating prepared by the present invention, the wear resistance and corrosion resistance of these devices can be improved, and the corrosion caused by long-term immersion in seawater can be avoided, thereby extending the service life of these devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a microscopic morphology of the graphene powder in the present invention.
[0033] Figure 2 This is a microscopic morphology of the copper-coated graphene powder prepared in the present invention.
[0034] Figure 3 The hardness curves of the composite plates corresponding to the PTFE-based coatings prepared in different embodiments of the present invention are shown in FIG.
[0035] Figure 4 The friction curves of the composite plates corresponding to the PTFE-based coatings prepared in different embodiments of the present invention are shown.
[0036] Figure 5 It is a histogram of the wear rate of the composite plate corresponding to the PTFE-based coating prepared in different embodiments of the present invention.
[0037] Figure 6 This is a wear scar morphology of a composite plate coated with the PTFE-based coating prepared in Example 8 of the present invention.
[0038] Figure 7 This is a wear scar morphology of a composite plate coated with the PTFE-based coating prepared in Example 9 of the present invention.
[0039] Figure 8 This is a wear scar morphology diagram of a composite plate coated with the PTFE-based coating prepared in Example 5 of the present invention.
[0040] Fig. 9 This is a wear scar morphology diagram of a composite plate coated with a PTFE-based coating prepared in Comparative Example 3 according to the present invention.
[0041] Fig.10 This is a surface morphology of the PTFE-based coating in the composite plate prepared in Example 5 of the present invention.
[0042] Fig.11 This is a surface morphology of the PTFE-based coating in the composite plate prepared in Comparative Example 3 of the present invention.
[0043] Fig.12 Polarization curves of the composite plates prepared in Example 5, Example 8, Example 9 and Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0044] The present invention is further described below in conjunction with specific implementation methods. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form a new embodiment.
[0045] In the description of the present invention, it should be noted that for directional words, such as the terms "center", "lateral", "longitudinal", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicating directions and positional relationships are based on the directions or positional relationships shown in the drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and cannot be understood as limiting the specific protection scope of the present invention. The terms "first", "second", etc. in the specification and claims of the present invention are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. The terms "including" and "having" in the specification and claims of the present invention and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device including a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0046] Example 1
[0047] A modified graphene PTFE-based coating, the raw materials of which are calculated by weight: 40-80 parts of PTFE powder, 1-10 parts of coupling agent, 5-15 parts of aramid, 0.5-8 parts of graphene, 70-90 parts of copper nitrate trihydrate, and 15-25 parts of polyimide.
[0048] The coupling agent is one or more of heptadecafluorotriethoxysilane, γ-aminopropyltriethoxysilane, and tridecafluorooctyltriethoxysilane. In this embodiment, the copper-plated graphene is modified by using a coupling agent, so that the number of micropores and crack defects in the PTFE matrix is greatly reduced, thereby improving the corrosion resistance of the PTFE-based coating.
[0049] Specifically, 17-fluoro-decyl triethoxysilane and 13-fluoro-octyl triethoxysilane are both fluorine-based coupling agents. Its CF group is very similar to the CF group in the PTFE matrix, so in the mixing process, according to the principle of like dissolves like, the compatibility between PTFE and filler (i.e., graphene, aramid and polyimide) is modified by a fluorine-containing coupling agent, so that the interface bonding between PTFE and filler is tighter, and its wear resistance is improved. At the same time, the coupling agent can also greatly reduce the micropores and crack defects of the PTFE matrix itself, thereby improving the corrosion resistance of the prepared PTFE-based coating. The improvement of corrosion resistance enables the prepared coating to be applied to devices in the marine field, thereby improving the corrosion resistance of these devices. The wear resistance and corrosion resistance of the equipment in the marine field coated with the coating are greatly improved.
[0050] γ-aminopropyltriethoxysilane is an amino coupling agent. The fluorine atoms on the surface of PTFE will repel the unshared electrons of the amino N, making it stay away from the fluorine atoms, while the H atoms in the amino group are attracted by the F atoms and accept the unshared electron pairs on the surface of the F atoms, thereby forming intermolecular hydrogen bonds, greatly reducing the repulsive force between the polytetrafluoroethylene surface and improving the organic-inorganic interface bonding strength. In this way, the micropores and cracks in the prepared PTFE-based coating can be reduced, and the corrosion resistance of the prepared PTFE-based coating can be improved.
[0051] In addition, the present embodiment uniformly adsorbs copper nanoparticles on the graphene surface or embeds them in the graphene sheet, so that the number of graphene layers is small and there is no agglomeration phenomenon. In addition, the copper nanoparticles can also effectively inhibit the agglomeration of graphene under van der Waals force, because the thinner graphene layer can provide adsorption sites for copper ions, which is conducive to the generation of copper nanoparticles, and these reactive adsorption sites will limit the aggregation of graphene, enhance the dispersibility of graphene in PTFE, and thus improve the wear resistance of the prepared PTFE-based coating.
[0052] The particle size of graphene is 2μm-7μm.
[0053] Example 2
[0054] A method for preparing a modified graphene PTFE-based coating comprises the following steps:
[0055] Preparation of copper-coated graphene powder:
[0056] The coupling agent is added into anhydrous ethanol, stirred to dissolve, and a mixed solution 1 is obtained; the prepared copper-coated graphene powder is then added into the mixed solution 1, and ultrasonicated and stirred to obtain a mixed solution 2; the pH of the mixed solution 2 is adjusted with hydrochloric acid so that the pH of the mixed solution 2 is 4-5; the mixed solution 2 is then heated in a water bath and then cooled to room temperature, and washed and filtered with deionized water, and vacuum dried to obtain the modified graphene powder.
[0057] The modified graphene powder is added into the PTFE dispersion, and the mixture is stirred, filtered and dried in sequence to obtain the modified graphene PTFE composite powder.
[0058] Aramid and polyimide are respectively added to the modified graphene PTFE composite powder and mixed evenly to obtain a mixed mud material.
[0059] The mixed mud material is evenly spread on the copper powder plate, and rolled using a rolling mill to obtain a plate with the mixed mud material coated on the surface.
[0060] The plate with the surface coated with the mixed mud is then placed in a sintering device for plasticization at a plasticizing temperature of 370°C, a plasticizing time of 4 hours, and a heating rate of 10°C / min. After sintering, the plate is cooled to room temperature with the sintering device to obtain a plate with a modified graphene PTFE-based coating.
[0061] Wherein, the sintering device can be a muffle furnace.
[0062] After rolling using a rolling mill, a plate with a total thickness of 2.1 mm and a surface thickness of 0.1 mm of mixed mud can be obtained.
[0063] When the plate with the surface coated with the mixed mud is placed in the sintering device for plasticization, a protective gas needs to be introduced into the sintering device, and the protective gas can be nitrogen with a purity of more than 99.9%.
[0064] Among them, the copper-coated graphene powder is prepared by an in-situ generation method, and the specific steps are as follows:
[0065] Graphene was dispersed in 600 mL of ethanol solution, and after ultrasonication and magnetic stirring, a mixed solution three was obtained.
[0066] Copper nitrate trihydrate and glucose solution were added to the mixed solution three in sequence, and the mixture was stirred for a period of time to obtain a mixed solution four.
[0067] A NaOH solution with a concentration of 5 mol / L and a volume of 500 mL was added dropwise to the mixed solution four three times, stirred for 3 hours after the addition was completed, and then the stirred solution was filtered to obtain a solid product; the solid product was washed with deionized water for multiple times and filtered and dried to obtain copper-coated graphene powder.
[0068] The PTFE dispersion is prepared by adding PTFE powder into distilled water and performing mechanical stirring and ultrasonic dispersion for 2 hours.
[0069] Example 3
[0070] A method for preparing a modified graphene PTFE-based coating comprises the following steps:
[0071] (1) First, 8 g of graphene was dispersed in 600 ml of ethanol solution, ultrasonicated for 10 min, and then magnetically stirred for 5 min.
[0072] (2) Then add 90gCu(NO 3 ) 2 ·3H 2 O, volume 300ml, concentration 1.25mol / L C 6 H 12 O 6 ·H 2 O solution and stir for about 2 hours.
[0073] (3) 500 ml of NaOH with a concentration of 5 mol / L was added dropwise to the solution of step (2) in three portions. After the addition was completed, the mixture was stirred in a magnetic stirrer for 3 hours. The obtained product was washed with deionized water and filtered, and dried at 80° C. for 9 hours. This process was repeated three times to obtain copper-coated graphene powder.
[0074] (4) Add 1 g of heptadecafluorodecyltriethoxysilane into anhydrous ethanol and stir to dissolve it.
[0075] (5) adding the copper-coated graphene powder prepared in step (3) to the solution of step (4), first ultrasonically treating for 10 min and then stirring for 1 h, and finally adjusting the pH of the solution with hydrochloric acid to a pH of 4 to 5.
[0076] (6) The pH-adjusted solution was placed in a 50°C water bath for 30 min, then the water bath was heated to 70°C, reacted for 30 min, and cooled to room temperature.
[0077] (7) The cooled solution in step (6) is washed and filtered three times with deionized water, and then vacuum dried at 60° C. to obtain modified graphene powder.
[0078] (8) Add 60 g of PTFE powder into 100 g of distilled water, stir mechanically and disperse ultrasonically for 2 h to obtain a PTFE dispersion.
[0079] (9) adding the modified graphene powder in step (7) to the PTFE dispersion in step (8), then mechanically stirring for 1 hour, and then vacuum filtering, and drying at 100° C. for 9 hours after filtration to obtain a modified graphene / PTFE composite powder.
[0080] (10) 10 g of aramid and 20 g of polyimide were added to the modified graphene / PTFE composite powder, respectively, and then stirred in a high-speed mixer for 30 min. After mixing evenly, a mixed mud was obtained.
[0081] (11) The mixed mud obtained in step (10) is evenly spread on the copper powder plate, and rolled using a rolling mill to obtain a plate with a total thickness of 2.1 mm and a surface layer coated with the mixed mud with a thickness of 0.1 mm.
[0082] (12) The plate coated with the mixed mud material on the surface is then placed in a muffle furnace with a protective atmosphere for plasticization, the plasticization temperature is 370° C., the plasticization time is 4 h, the heating rate is 10° C. / min, and the protective atmosphere is nitrogen with a purity of more than 99.9%. After sintering, the plate is cooled to room temperature with the furnace to obtain a plate with a modified graphene PTFE-based coating.
[0083] Example 4
[0084] A method for preparing a modified graphene PTFE-based coating comprises the following steps:
[0085] (1) First, 6 g of graphene was dispersed in 600 ml of ethanol solution, ultrasonicated for 10 min, and then magnetically stirred for 5 min.
[0086] (2) Then add 85gCu(NO 3 ) 2 ·3H 2 O, volume 300ml, concentration 1.25mol / L C 6 H 12 O 6 ·H 2 O solution and stir for about 2 hours.
[0087] (3) 500 ml of NaOH with a concentration of 5 mol / L was added dropwise to the solution of step (2) in three portions. After the addition was completed, the mixture was stirred in a magnetic stirrer for 3 hours. The obtained product was then washed with deionized water and filtered, and dried at 80° C. for 9 hours. This process was repeated three times to obtain copper-coated graphene powder.
[0088] (4) Add 2 g of heptadecafluorodecyltriethoxysilane into anhydrous ethanol and stir to dissolve it.
[0089] (5) adding the copper-coated graphene powder prepared in step (3) to the solution of step (4), first ultrasonically treating for 10 min and then stirring for 1 h, and finally adjusting the pH of the solution with hydrochloric acid to a pH of 4 to 5.
[0090] (6) The pH-adjusted solution was placed in a 50°C water bath for 30 min, then the water bath was heated to 70°C, reacted for 30 min, and cooled to room temperature.
[0091] (7) The cooled solution in step (6) is washed and filtered three times with deionized water, and then vacuum dried at 60° C. to obtain modified graphene powder.
[0092] (8) Add 60 g of PTFE powder into 100 g of distilled water, stir mechanically and disperse ultrasonically for 2 h to obtain a PTFE dispersion.
[0093] (9) adding the modified graphene powder in step (7) to the PTFE dispersion in step (8), then mechanically stirring for 1 hour, and then vacuum filtering, and drying at 100° C. for 9 hours after filtration to obtain a modified graphene / PTFE composite powder.
[0094] (10) 10 g of aramid and 20 g of polyimide were added to the modified graphene / PTFE composite powder, respectively, and then stirred in a high-speed mixer for 30 min. After mixing evenly, a mixed mud was obtained.
[0095] (11) The mixed mud obtained in step (10) is evenly spread on the copper powder plate, and rolled using a rolling mill to obtain a plate with a total thickness of 2.1 mm and a surface layer coated with the mixed mud with a thickness of 0.1 mm.
[0096] (12) The plate coated with the mixed mud material on the surface is then placed in a muffle furnace with a protective atmosphere for plasticization, the plasticization temperature is 370° C., the plasticization time is 4 h, the heating rate is 10° C. / min, and the protective atmosphere is nitrogen with a purity of more than 99.9%. After sintering, the plate is cooled to room temperature with the furnace to obtain a plate with a modified graphene PTFE-based coating.
[0097] Example 5
[0098] A method for preparing a modified graphene PTFE-based coating comprises the following steps:
[0099] (1) First, 4 g of graphene was dispersed in 600 ml of ethanol solution, ultrasonicated for 10 min, and then magnetically stirred for 5 min.
[0100] (2) Then add 80gCu(NO 3 ) 2 ·3H 2O, volume 300ml, concentration 1.25mol / L C 6 H 12 O 6 ·H 2 O solution and stir for about 2 hours.
[0101] (3) 500 ml of NaOH with a concentration of 5 mol / L was added dropwise to the solution of step (2) in three portions. After the addition was completed, the mixture was stirred in a magnetic stirrer for 3 hours. The obtained product was then washed with deionized water and filtered, and dried at 80° C. for 9 hours. This process was repeated three times to obtain copper-coated graphene powder.
[0102] (4) Add 5 g of heptadecafluorodecyltriethoxysilane into anhydrous ethanol and stir to dissolve it.
[0103] (5) adding the copper-coated graphene powder prepared in step (3) to the solution of step (4), first ultrasonically treating for 10 min and then stirring for 1 h, and finally adjusting the pH of the solution with hydrochloric acid to a pH of 4 to 5.
[0104] (6) The pH-adjusted solution was placed in a 50°C water bath for 30 min, then the water bath was heated to 70°C, reacted for 30 min, and cooled to room temperature.
[0105] (7) The cooled solution in step (6) is washed and filtered three times with deionized water, and then vacuum dried at 60° C. to obtain modified graphene powder.
[0106] (8) Add 60 g of PTFE powder into 100 g of distilled water, stir mechanically and disperse ultrasonically for 2 h to obtain a PTFE dispersion.
[0107] (9) adding the modified graphene powder in step (7) to the PTFE dispersion in step (8), then mechanically stirring for 1 hour, and then vacuum filtering, and drying at 100° C. for 9 hours after filtration to obtain a modified graphene / PTFE composite powder.
[0108] (10) 10 g of aramid and 20 g of polyimide were added to the modified graphene / PTFE composite powder, respectively, and then stirred in a high-speed mixer for 30 min. After mixing evenly, a mixed mud was obtained.
[0109] (11) The mixed mud obtained in step (10) is evenly spread on the copper powder plate, and rolled using a rolling mill to obtain a plate with a total thickness of 2.1 mm and a surface layer coated with the mixed mud with a thickness of 0.1 mm.
[0110] (12) The plate coated with the mixed mud material on the surface is then placed in a muffle furnace with a protective atmosphere for plasticization, the plasticization temperature is 370° C., the plasticization time is 4 h, the heating rate is 10° C. / min, and the protective atmosphere is nitrogen with a purity of more than 99.9%. After sintering, the plate is cooled to room temperature with the furnace to obtain a plate with a modified graphene PTFE-based coating.
[0111] Example 6
[0112] A method for preparing a modified graphene PTFE-based coating comprises the following steps:
[0113] (1) First, 2 g of graphene was dispersed in 600 ml of ethanol solution, ultrasonicated for 10 min, and then magnetically stirred for 5 min.
[0114] (2) Then add 75gCu(NO 3 ) 2 ·3H 2 O, volume 300ml, concentration 1.25mol / L C 6 H 12 O 6 ·H 2 O solution and stir for about 2 hours.
[0115] (3) 500 ml of NaOH with a concentration of 5 mol / L was added dropwise to the solution of step (2) in three portions. After the addition was completed, the mixture was stirred in a magnetic stirrer for 3 hours. The obtained product was then washed with deionized water and filtered, and dried at 80° C. for 9 hours. This process was repeated three times to obtain copper-coated graphene powder.
[0116] (4) Add 8 g of heptadecafluorodecyltriethoxysilane into anhydrous ethanol and stir to dissolve it.
[0117] (5) adding the copper-coated graphene powder prepared in step (3) to the solution of step (4), first ultrasonically treating for 10 min and then stirring for 1 h, and finally adjusting the pH of the solution with hydrochloric acid to a pH of 4 to 5.
[0118] (6) The pH-adjusted solution was placed in a 50°C water bath for 30 min, then the water bath was heated to 70°C, reacted for 30 min, and cooled to room temperature.
[0119] (7) The cooled solution in step (6) is washed and filtered three times with deionized water, and then vacuum dried at 60° C. to obtain modified graphene powder.
[0120] (8) Add 60 g of PTFE powder into 100 g of distilled water, stir mechanically and disperse ultrasonically for 2 h to obtain a PTFE dispersion.
[0121] (9) adding the modified graphene powder in step (7) to the PTFE dispersion in step (8), then mechanically stirring for 1 hour, and then vacuum filtering, and drying at 100° C. for 9 hours after filtration to obtain a modified graphene / PTFE composite powder.
[0122] (10) 10 g of aramid and 20 g of polyimide were added to the modified graphene / PTFE composite powder, respectively, and then stirred in a high-speed mixer for 30 min. After mixing evenly, a mixed mud was obtained.
[0123] (11) The mixed mud obtained in step (10) is evenly spread on the copper powder plate, and rolled using a rolling mill to obtain a plate with a total thickness of 2.1 mm and a surface layer coated with the mixed mud with a thickness of 0.1 mm.
[0124] (12) The plate coated with the mixed mud material on the surface is then placed in a muffle furnace with a protective atmosphere for plasticization, the plasticization temperature is 370° C., the plasticization time is 4 h, the heating rate is 10° C. / min, and the protective atmosphere is nitrogen with a purity of more than 99.9%. After sintering, the plate is cooled to room temperature with the furnace to obtain a plate with a modified graphene PTFE-based coating.
[0125] Example 7
[0126] A method for preparing a modified graphene PTFE-based coating comprises the following steps:
[0127] (1) First, 0.5 g of graphene was dispersed in 600 ml of ethanol solution, ultrasonicated for 10 min, and then magnetically stirred for 5 min.
[0128] (2) Then add 70gCu(NO 3 ) 2 ·3H 2 O, volume 300ml, concentration 1.25mol / L C 6 H 12 O 6 ·H 2 O solution and stir for about 2 hours.
[0129] (3) 500 ml of NaOH with a concentration of 5 mol / L was added dropwise to the solution of step (2) in three portions. After the addition was completed, the mixture was stirred in a magnetic stirrer for 3 hours. The obtained product was then washed with deionized water and filtered, and dried at 80° C. for 9 hours. This process was repeated three times to obtain copper-coated graphene powder.
[0130] (4) Add 10 g of heptadecafluorodecyltriethoxysilane into anhydrous ethanol and stir to dissolve it.
[0131] (5) adding the copper-coated graphene powder prepared in step (3) to the solution of step (4), first ultrasonically treating for 10 min and then stirring for 1 h, and finally adjusting the pH of the solution with hydrochloric acid to a pH of 4 to 5.
[0132] (6) The pH-adjusted solution was placed in a 50°C water bath for 30 min, then the water bath was heated to 70°C, reacted for 30 min, and cooled to room temperature.
[0133] (7) The cooled solution in step (6) is washed and filtered three times with deionized water, and then vacuum dried at 60° C. to obtain modified graphene powder.
[0134] (8) Add 60 g of PTFE powder into 100 g of distilled water, stir mechanically and disperse ultrasonically for 2 h to obtain a PTFE dispersion.
[0135] (9) adding the modified graphene powder in step (7) to the PTFE dispersion in step (8), then mechanically stirring for 1 hour, and then vacuum filtering, and drying at 100° C. for 9 hours after filtration to obtain a modified graphene / PTFE composite powder.
[0136] (10) 10 g of aramid and 20 g of polyimide were added to the modified graphene / PTFE composite powder, respectively, and then stirred in a high-speed mixer for 30 min. After mixing evenly, a mixed mud was obtained.
[0137] (11) The mixed mud obtained in step (10) is evenly spread on the copper powder plate, and rolled using a rolling mill to obtain a plate with a total thickness of 2.1 mm and a surface layer coated with the mixed mud with a thickness of 0.1 mm.
[0138] (12) The plate coated with the mixed mud material on the surface is then placed in a muffle furnace with a protective atmosphere for plasticization, the plasticization temperature is 370° C., the plasticization time is 4 h, the heating rate is 10° C. / min, and the protective atmosphere is nitrogen with a purity of more than 99.9%. After sintering, the plate is cooled to room temperature with the furnace to obtain a plate with a modified graphene PTFE-based coating.
[0139] Example 8
[0140] A method for preparing a modified graphene PTFE-based coating comprises the following steps:
[0141] (1) First, 4 g of graphene was dispersed in 600 ml of ethanol solution, ultrasonicated for 10 min, and then magnetically stirred for 5 min.
[0142] (2) Then add 80gCu(NO 3 ) 2 ·3H 2 O, volume 300ml, concentration 1.25mol / L C6 H 12 O 6 ·H 2 O solution and stir for about 2 hours.
[0143] (3) 500 ml of NaOH with a concentration of 5 mol / L was added dropwise to the solution of step (2) in three portions. After the addition was completed, the mixture was stirred in a magnetic stirrer for 3 hours. The obtained product was then washed with deionized water and filtered, and dried at 80° C. for 9 hours. This process was repeated three times to obtain copper-coated graphene powder.
[0144] (4) Add 5 g of γ-aminopropyltriethoxysilane into anhydrous ethanol and stir to dissolve it.
[0145] (5) adding the copper-coated graphene powder prepared in step (3) to the solution of step (4), first ultrasonically treating for 10 min and then stirring for 1 h, and finally adjusting the pH of the solution with hydrochloric acid to a pH of 4 to 5.
[0146] (6) The pH-adjusted solution was placed in a 50°C water bath for 30 min, then the water bath was heated to 70°C, reacted for 30 min, and cooled to room temperature.
[0147] (7) The cooled solution in step (6) is washed and filtered three times with deionized water, and then vacuum dried at 60° C. to obtain modified graphene powder.
[0148] (8) Add 60 g of PTFE powder into 100 g of distilled water, stir mechanically and disperse ultrasonically for 2 h to obtain a PTFE dispersion.
[0149] (9) adding the modified graphene powder in step (7) to the PTFE dispersion in step (8), then mechanically stirring for 1 hour, and then vacuum filtering, and drying at 100° C. for 9 hours after filtration to obtain a modified graphene / PTFE composite powder.
[0150] (10) 10 g of aramid and 20 g of polyimide were added to the modified graphene / PTFE composite powder, respectively, and then stirred in a high-speed mixer for 30 min. After mixing evenly, a mixed mud was obtained.
[0151] (11) The mixed mud obtained in step (10) is evenly spread on the copper powder plate, and rolled using a rolling mill to obtain a plate with a total thickness of 2.1 mm and a surface layer coated with the mixed mud with a thickness of 0.1 mm.
[0152] (12) The plate coated with the mixed mud material on the surface is then placed in a muffle furnace with a protective atmosphere for plasticization, the plasticization temperature is 370° C., the plasticization time is 4 h, the heating rate is 10° C. / min, and the protective atmosphere is nitrogen with a purity of more than 99.9%. After sintering, the plate is cooled to room temperature with the furnace to obtain a plate with a modified graphene PTFE-based coating.
[0153] Example 9
[0154] A method for preparing a modified graphene PTFE-based coating comprises the following steps:
[0155] (1) First, 4 g of graphene was dispersed in 600 ml of ethanol solution, ultrasonicated for 10 min, and then magnetically stirred for 5 min.
[0156] (2) Then add 80gCu(NO 3 ) 2 ·3H 2 O, volume 300ml, concentration 1.25mol / L C 6 H 12 O 6 ·H 2 O solution and stir for about 2 hours.
[0157] (3) 500 ml of NaOH with a concentration of 5 mol / L was added dropwise to the solution of step (2) in three portions. After the addition was completed, the mixture was stirred in a magnetic stirrer for 3 hours. The obtained product was then washed with deionized water and filtered, and dried at 80° C. for 9 hours. This process was repeated three times to obtain copper-coated graphene powder.
[0158] (4) Add 2 g of tridecafluorooctyltriethoxysilane into anhydrous ethanol and stir to dissolve it.
[0159] (5) adding the copper-coated graphene powder prepared in step (3) to the solution of step (4), first ultrasonically treating for 10 min and then stirring for 1 h, and finally adjusting the pH of the solution with hydrochloric acid to a pH of 4 to 5.
[0160] (6) The pH-adjusted solution was placed in a 50°C water bath for 30 min, then the water bath was heated to 70°C, reacted for 30 min, and cooled to room temperature.
[0161] (7) The cooled solution in step (6) is washed and filtered three times with deionized water, and then vacuum dried at 60° C. to obtain modified graphene powder.
[0162] (8) Add 60 g of PTFE powder into 100 g of distilled water, stir mechanically and disperse ultrasonically for 2 h to obtain a PTFE dispersion.
[0163] (9) adding the modified graphene powder in step (7) to the PTFE dispersion in step (8), then mechanically stirring for 1 hour, and then vacuum filtering, and drying at 100° C. for 9 hours after filtration to obtain a modified graphene / PTFE composite powder.
[0164] (10) 10 g of aramid and 20 g of polyimide were added to the modified graphene / PTFE composite powder, respectively, and then stirred in a high-speed mixer for 30 min. After mixing evenly, a mixed mud was obtained.
[0165] (11) The mixed mud obtained in step (10) is evenly spread on the copper powder plate, and rolled using a rolling mill to obtain a plate with a total thickness of 2.1 mm and a surface layer coated with the mixed mud with a thickness of 0.1 mm.
[0166] (12) The plate coated with the mixed mud material on the surface is then placed in a muffle furnace with a protective atmosphere for plasticization, the plasticization temperature is 370° C., the plasticization time is 4 h, the heating rate is 10° C. / min, and the protective atmosphere is nitrogen with a purity of more than 99.9%. After sintering, the plate is cooled to room temperature with the furnace to obtain a plate with a modified graphene PTFE-based coating.
[0167] Comparative Example 1
[0168] A method for preparing a PTFE-based coating comprises the following steps:
[0169] (1) Add 60 g of PTFE powder into 100 g of distilled water, stir mechanically and disperse ultrasonically for 2 h to obtain a PTFE dispersion.
[0170] (2) Add 10 g of aramid and 20 g of polyimide to the PTFE dispersion, stir in a high-speed mixer for 30 min, and mix well to obtain a mixed mud.
[0171] (3) The mixed mud obtained in step (2) is evenly spread on the copper powder plate, and rolled using a rolling mill to obtain a plate with a total thickness of 2.1 mm and a surface layer coated with the mixed mud with a thickness of 0.1 mm.
[0172] (4) The plate coated with the mixed mud material on the surface is then placed in a muffle furnace in a protective atmosphere for plasticization, the plasticization temperature is 370°C, the plasticization time is 4 hours, the heating rate is 10°C / min, and the protective atmosphere is nitrogen with a purity of more than 99.9%. After sintering, the plate is cooled to room temperature with the furnace to obtain a PTFE-based coated plate.
[0173] Comparative Example 2
[0174] A method for preparing a PTFE-based coating comprises the following steps:
[0175] (1) Add 60 g of PTFE powder into 100 g of distilled water, stir mechanically and disperse ultrasonically for 2 h to obtain a PTFE dispersion.
[0176] (2) 4 g of graphene powder was added to the PTFE dispersion, mechanically stirred for 1 h, vacuum filtered, and dried at 100 °C for 9 h to obtain a graphene / PTFE composite powder.
[0177] (3) 10 g of aramid and 20 g of polyimide were added to the graphene PTFE composite powder, respectively, and the mixture was stirred in a high-speed mixer for 30 min to obtain a mixed mud.
[0178] (4) The mixed mud obtained in step (3) is evenly spread on the copper powder plate, and rolled using a rolling mill to obtain a plate with a total thickness of 2.1 mm and a surface layer coated with the mixed mud with a thickness of 0.1 mm.
[0179] (5) The plate coated with the mixed mud material on the surface is then placed in a muffle furnace in a protective atmosphere for plasticization, the plasticization temperature is 370°C, the plasticization time is 4 hours, the heating rate is 10°C / min, and the protective atmosphere is nitrogen with a purity of more than 99.9%. After sintering is completed, the plate is cooled to room temperature with the furnace to obtain a plate with a graphene PTFE-based coating.
[0180] Comparative Example 3
[0181] A method for preparing a PTFE-based coating comprises the following steps:
[0182] First, 4 g of graphene was dispersed in 600 ml of ethanol solution, ultrasonicated for 10 min, and then magnetically stirred for 5 min.
[0183] (2) Then add 80gCu(NO 3 ) 2 ·3H 2 O, volume 300ml, concentration 1.25mol / L C 6 H 12 O 6 ·H 2 O solution and stir for about 2 hours.
[0184] (3) 500 ml of NaOH with a concentration of 5 mol / L was added dropwise to the solution of step (2) in three portions. After the addition was completed, the mixture was stirred in a magnetic stirrer for 3 hours. The obtained product was then washed with deionized water and filtered, and dried at 80° C. for 9 hours. This process was repeated three times to obtain copper-coated graphene powder.
[0185] (4) Add 60 g of PTFE powder into 100 g of distilled water, stir mechanically and disperse ultrasonically for 2 h to obtain a PTFE dispersion.
[0186] (5) adding the copper-coated graphene powder in step (3) to the PTFE dispersion in step (4), then mechanically stirring for 1 hour, and then vacuum filtering, and drying at 100° C. for 9 hours after filtration to obtain a graphene / PTFE composite powder.
[0187] (6) 10 g of aramid and 20 g of polyimide were added to the graphene / PTFE composite powder, respectively, and then stirred in a high-speed mixer for 30 min. After mixing evenly, a mixed mud was obtained.
[0188] (7) The mixed mud obtained in step (6) is evenly spread on the copper powder plate, and rolled using a rolling mill to obtain a plate with a total thickness of 2.1 mm and a surface layer coated with the mixed mud with a thickness of 0.1 mm.
[0189] (8) The plate coated with the mixed mud material on the surface is then placed in a muffle furnace in a protective atmosphere for plasticization, the plasticization temperature is 370° C., the plasticization time is 4 hours, the heating rate is 10° C. / min, and the protective atmosphere is nitrogen with a purity of more than 99.9%. After sintering is completed, the plate is cooled to room temperature with the furnace to obtain a plate with a graphene PTFE-based coating.
[0190] The PTFE-based coatings prepared in Examples 3-9 and Comparative Examples 1-3 were subjected to surface hardness, friction and wear tests, and corrosion resistance tests, respectively.
[0191] In the present invention, the hardness, friction and wear, and corrosion resistance of the substrate coated with the PTFE coating need to be tested to reflect these properties of the prepared PTFE-based coating.
[0192] The plates with PTFE-based coatings prepared in Examples 3-9 and the plates with PTFE-based coatings prepared in Comparative Examples 1-3 were subjected to hardness tests, friction and wear tests, and corrosion resistance tests.
[0193] The hardness test uses a Shore hardness tester (type D) to measure the hardness of 10mm (length), 10mm (width), and 2.1mm (thickness) samples. The test is performed at 5 locations on each sample, with a load of 15N and a holding time of 3s, and the average hardness value is calculated. The variation of the hardness value is within 10% of the average value.
[0194] The friction and wear experiment used an end face friction and wear tester (HDM-200) to test the tribological properties of each group of coating samples. The test device adopts the end face to end face contact form, and the mating material is 42CrMo. Five samples were prepared for each embodiment and comparative example, and each test lasted 60 minutes.
[0195] The corrosion resistance test was conducted using an electrochemical workstation (Princeton PMC-1000A) with a test frequency of 100 kHz to 10 mHz, an amplitude of 20 mV, and a scan rate of 1 mV / s.
[0196] In the present invention, the friction and wear test and corrosion resistance test of the composite sheet coated with the PTFE-based coating are carried out on the basis of seawater as the medium. Because the test is carried out on the basis of seawater as the medium, it can provide reference value for its later application in the marine field.
[0197] In the present invention, fillers refer to other raw materials other than the PTFE matrix in the preparation of the PTFE-based coating, which may specifically include graphene, aramid and polyimide.
[0198] During the preparation process, the properties of the intermediate products are also observed. Figure 1 The graphene powder in the raw materials used in Examples 3-9 and Comparative Example 2 (i.e., the graphene was not treated in any way) is shown in SEM images. Figure 1 Observation shows that the graphene powder has a translucent lamellar structure without much stacking.
[0199] Figure 2 is a SEM image of the modified graphene powder prepared in Example 3. Figure 2 1 is graphene and 2 is copper nanoparticles. Figure 2 It can be seen that Figure 2 A large number of milky white copper nanoparticles are uniformly adsorbed on the graphene surface or embedded in the graphene sheets. The graphene has fewer layers, no agglomeration, and is nearly transparent. By analyzing the figure, it can be seen that the thinner graphene layer can provide adsorption sites for copper ions, which is conducive to the generation of copper nanoparticles. Moreover, these adsorption sites also limit the aggregation of graphene after adsorbing copper ions, which proves that copper nanoparticles can effectively inhibit the aggregation of graphene under van der Waals forces, enhance the dispersibility of graphene in PTFE, and thus improve the wear resistance of the prepared PTFE-based coating.
[0200] Figure 3 The Shore hardness curve of the composite board obtained in Examples 3-7 and Comparative Examples 1-2 is shown in FIG. Figure 3It is known from the analysis that the maximum amount of graphene added in Example 3 is 8g, and the hardness of the composite sheet is also the largest, which is 94.6. No graphene is added in Comparative Example 1, so its hardness is 76.3 at the minimum, which proves that graphene can increase the hardness of the prepared PTFE-based coating. And in the PTFE-based coating prepared in Example 3 to Example 7, as the amount of graphene added is gradually reduced, the hardness of the composite sheet is also gradually reduced, so the hardness of the prepared PTFE-based coating can be controlled by controlling the amount of graphene in the actual preparation process. And when the amount of graphene added reaches 4g, the hardness of the composite sheet reaches 92.7 at this time. It can be seen from the line graph that as the amount of graphene increases again in Example 3 to Example 5, its hardness increase trend weakens.
[0201] In addition, through the analysis of Example 5 and Comparative Example 2, it can be seen that the addition amount of graphene in Example 3 and Comparative Example 2 is the same, and the difference is that the graphene is modified in Example 3, while the graphene is not modified in Comparative Example 2. The hardness of the composite board in Example 5 is 92.7, and the hardness of the composite board in Comparative Example 2 is 89.5. The difference in hardness between the two is not large, which indicates that the modification of graphene has little effect on its hardness.
[0202] Figure 4 It is the friction coefficient curve of the composite board prepared by Examples 3-9 of the present invention and Comparative Examples 1-2 under dry friction state. Figure 5 This is a bar graph of the wear rates of the composite plates prepared in Examples 3-9 of the present invention and Comparative Examples 1-2 under dry friction conditions.
[0203] Through Figure 4 and Figure 5 It can be seen from the analysis that the friction coefficient and wear rate of Comparative Example 1 are the largest, indicating that the friction reduction and wear resistance of the PTFE-based coating prepared in Comparative Example 1 is the worst. The main reason is that no graphene is added in Comparative Example 1, so adding graphene can effectively enhance the wear resistance of the prepared PTFE-based coating. In addition, the friction coefficient and wear rate of the composite sheet in Examples 3-9 are lower than those of the composite sheet in Comparative Examples 1-2, which shows that the modified graphene has a significant enhancement effect on the friction reduction and wear resistance of the PTFE-based coating.
[0204] By analyzing the friction coefficient and wear rate of the composite plate in Examples 5 to 8, it can be seen that when the amount of graphene added is in the range of 0.5g-4g, the friction coefficient and wear rate of the composite plate gradually decrease with the increase of the amount of graphene. When the amount of graphene added is 4g, the friction coefficient and wear rate of the composite plate are the lowest, specifically, the friction coefficient is 0.124 and the wear rate is 3.4×10 -5 mm 3 / Nm.
[0205] By analyzing Examples 3 to 5, it can be seen that when the amount of graphene added increases from 4g to 8g, as the amount of graphene added increases, the friction coefficient and wear rate of the composite plate increase. Therefore, in actual operation, the amount of graphene added can be selected to be 4g, which can ensure that the prepared PTFE-based coating has good wear resistance.
[0206] Figures 6 to 9 The surface morphology of the wear marks of the composite plate in different embodiments. Figure 6 The surface morphology of the wear scar position of the composite plate in Example 8; Figure 7 The surface morphology of the wear scar position of the composite plate in Example 9; Figure 8 The surface morphology of the wear scar position of the composite plate in Example 5; Fig. 9 This is the surface morphology of the wear scar position of the composite plate in Comparative Example 3.
[0207] Through Figures 6 to 9 It can be seen from the analysis that compared with Example 5, Example 8 and Example 9, Comparative Example 3 does not use a coupling agent, and combines Fig. 9 It can be seen that the surface density of the wear scar of the PTFE-based coating prepared in Comparative Example 3 is poor and there are many cracks. The main reason is that there is no coupling agent in Comparative Example 3, which will lead to loose interface bonding between the filler and the PTFE matrix, and under the action of friction, each filler and the PTFE matrix are prone to fall off.
[0208] Through Fig. 9 and Figure 6 By comparison, Figure 6 Wear scar surface morphology ratio of composite plate Fig. 9 The surface morphology of the wear scar of the composite plate is much smoother, and the crack propagation is also alleviated. This is because Figure 6 γ-aminopropyltriethoxysilane coupling agent is used in the process, and the fluorine atoms on the surface of the PTFE substrate will repel the unshared electrons of the amino group N in the γ-aminopropyltriethoxysilane coupling agent, making it away from the fluorine atoms, while the H atoms in the amino group are attracted by the fluorine atoms and accept the unshared electron pairs on the surface of the fluorine atoms, thereby forming intermolecular hydrogen bonds, greatly reducing the repulsive force between the filler and the PTFE substrate, and improving the organic-inorganic interface bonding strength, thereby achieving the improvement of its wear resistance. It can be seen that the wear resistance of the PTFE-based coating prepared by adding the coupling agent is much better than that of the PTFE-based coating without adding the coupling agent.
[0209] Through Figure 6 , Figure 7 and Figure 8 By comparison, Figure 7 and Figure 8 Compared with the wear scar surface morphology of the composite plate Figure 6In terms of the composite board, the wear marks on the surface are more minor, and there are fewer cracks and pores, resulting in a denser surface. The main reason is that the PTFE-based coatings in Example 9 and Example 5 both use fluorine-based coupling agents. The CF group in the fluorine-based coupling agent is very similar to the CF group in the PTFE matrix. Therefore, during the mixing process, according to the principle of similar compatibility, the PTFE matrix modified with the fluorine-based coupling agent has good compatibility with the filler (i.e., graphene, aramid and polyimide). For the PTFE-based coating modified with a fluorine-based coupling agent, during the sintering and plasticizing process, the compatibility of the CF bond in the fluorine group on the filler and the PTFE matrix is higher than the effect of the hydrogen bond in the amino group in the amino coupling agent. In combination with Figure 4 and Figure 5 It can be seen that the friction coefficient and wear rate of the composite plate coated with the PTFE-based coating in Example 9 and Example 5 are significantly lower than those in Example 8. It can be concluded that in the process of preparing the PTFE-based coating, the wear resistance of the PTFE-based coating prepared by adding a fluorine-based coupling agent is higher than that of the PTFE-based coating prepared by adding an amino coupling agent.
[0210] Fig.10 The surface morphology of the PTFE-based coating of the composite sheet in Example 5; Fig.11 The surface morphology of the PTFE-based coating of the composite sheet in Comparative Example 3. Fig.10 and Fig.11 By comparison, it can be seen that after the PTFE-based coating in Example 5 is modified with graphene by a coupling agent, the organizational morphology in the coating becomes denser. It can be seen that adding a coupling agent can reduce the micropores and cracks of the PTFE matrix itself, thereby improving its corrosion resistance.
[0211] Fig.12 Polarization curves of the composite plates prepared in Example 5, Example 8, Example 9 and Comparative Example 3 after being immersed in a 4% NaCl solution for 48 hours. Fig.12 It can be seen that by comparing Example 5, Example 8, Example 9 with Comparative Example 3, the corrosion potential of Example 5, Example 8 and Example 9 shifts to a more negative potential, and the corrosion current density is significantly reduced. The closer the corrosion potential is to the negative potential and the lower the corrosion current density is, the better the corrosion resistance is. It can be seen that the corrosion resistance can be improved by adding a coupling agent in the preparation of the PTFE-based coating. Among them, Example 5 has the best corrosion resistance, and Comparative Example 3 has the worst corrosion resistance. The above experiments confirm that the graphene modified by the coupling agent has an enhancing effect on the corrosion protection performance of the PTFE-based coating.
[0212] The above describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and the specification only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the present invention. The scope of protection claimed by the present invention is defined by the attached claims and their equivalents.
Claims
1. A modified graphene PTFE-based coating, characterized in that: The raw materials are calculated by weight as follows: 40-80 parts of PTFE powder, 1-10 parts of coupling agent, 5-15 parts of aramid, 0.5-8 parts of graphene, 70-90 parts of copper nitrate trihydrate, and 15-25 parts of polyimide; The copper nitrate trihydrate is used to mix with the graphene to prepare copper-coated graphene powder, and the coupling agent is used to modify the copper-coated graphene powder to obtain modified graphene powder; Wherein, the coupling agent is one or more of heptadecafluorooctyl triethoxysilane, γ-aminopropyl triethoxysilane, and tridecafluorooctyl triethoxysilane, and the coupling agent is used to respectively improve the interfacial bonding strength between the aramid and the PTFE, the interfacial bonding strength between the graphene and the PTFE, and the interfacial bonding strength between the polyimide and the PTFE.
2. A modified graphene PTFE-based coating, characterized in that: The particle size of the graphene is 2 μm-7 μm.
3. A method for preparing a modified graphene PTFE-based coating, characterized in that: It includes the following steps: preparing copper-coated graphene powder; The coupling agent in the modified graphene PTFE-based coating according to claim 1 is added to anhydrous ethanol, stirred to dissolve, and a mixed solution 1 is obtained, and the prepared copper-coated graphene powder is added to the mixed solution 1, and ultrasonicated and stirred to obtain the mixed solution 2; the pH of the mixed solution 2 is adjusted with hydrochloric acid so that the pH of the mixed solution 2 is 4 to 5; the mixed solution 2 is heated in a water bath and then cooled to room temperature, and washed and filtered with deionized water, and vacuum dried to obtain the modified graphene powder; Adding the modified graphene powder to the PTFE dispersion, stirring, filtering and drying in sequence to obtain a modified graphene PTFE composite powder; Aramid and polyimide are added to the modified graphene PTFE composite powder respectively, and the mixture is evenly mixed to obtain a mixed mud material; The mixed mud is evenly spread on the copper powder plate, and rolled using a rolling mill to obtain a plate with the mixed mud coated on the surface; The plate with the surface coated with the mixed mud is then placed in a sintering device for plasticization at a plasticizing temperature of 370°C, a plasticizing time of 4 hours, and a heating rate of 10°C / min. After sintering, the plate is cooled to room temperature with the sintering device to obtain a plate with the modified graphene PTFE-based coating.
4. The method for preparing a modified graphene PTFE-based coating according to claim 3, wherein The copper-coated graphene powder is prepared by an in-situ generation method.
5. The preparation method of modified graphene PTFE-based coating according to claim 3, characterized in that, The preparation of the copper-coated graphene powder comprises the following steps: Graphene was dispersed in 600 mL of ethanol solution, and then ultrasonicated and magnetically stirred to obtain a mixed solution 3; Adding copper nitrate trihydrate and glucose solution to the mixed solution three in sequence, and stirring for a period of time to obtain a mixed solution four; A NaOH solution with a concentration of 5 mol / L and a volume of 500 mL was added dropwise to the mixed solution four three times, stirred for 3 hours after the addition was completed, and then the stirred solution was filtered to obtain a solid product; the solid product was washed with deionized water for multiple times and filtered and dried to obtain the copper-coated graphene powder.
6. The method for preparing a modified graphene PTFE-based coating according to claim 3, wherein: The PTFE dispersion is obtained by adding PTFE powder into distilled water and performing mechanical stirring and ultrasonic dispersion for 2 hours.
7. The method for preparing a modified graphene PTFE-based coating according to claim 3, wherein: The mixed solution 2 with adjusted pH value was reacted in a water bath at 50° C. for 30 min, then heated to 70° C. and reacted for 30 min, and finally cooled to room temperature.
8. The method for preparing a modified graphene PTFE-based coating according to claim 7, wherein: The mixed solution after cooling to room temperature was washed and filtered three times with deionized water, and vacuum dried at 60° C. to obtain the modified graphene powder.
9. The method for preparing a modified graphene PTFE-based coating according to claim 7, wherein: After the prepared modified graphene powder is added to the PTFE dispersion, it is mechanically stirred for 1 hour, then vacuum filtered, and finally dried at 100° C. for 9 hours to obtain a modified graphene PTFE composite powder.
10. A modified graphene PTFE-based composite sheet, characterized in that: It includes a modified graphene PTFE-based coating prepared by the method for preparing a modified graphene PTFE-based coating as described in any one of claims 3-9.
Citation Information
Patent Citations
Preparation method for copper / graphene composite
CN108580893A
Long-lasting wear-resistant polytetrafluoroethylene coating
CN110144151A
Monodispersed nanometer graphene lubricant additive and production method
CN111979017A
Graphene and fluorpolymer composite
US20150093584A1
Copper-modified graphene oxide-based composite material, preparation method therefor and use thereof
WO2024027115A1
Cited By
Pre-dispersed polytetrafluoroethylene micro-powder, composite rubber material containing pre-dispersed polytetrafluoroethylene micro-powder and preparation method of composite rubber material
CN119859367A
Polytetrafluoroethylene composition, polytetrafluoroethylene composite material, preparation method of polytetrafluoroethylene composite material and sealing material
CN120682586A