Coating composition, coating, preparation method and application

By using the hydrolysis reaction of fluorine-containing silanes and metal compounds in the coating composition, a coating with high hardness and self-cleaning properties is formed, which solves the problems of short service life and high cost of coatings in high temperature and humid environments in the existing technology. problem, achieving long-term performance retention on different substrates.

CN118725731APending Publication Date: 2024-10-01NINGBO TIANXUAN NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310327470.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing technology, the hydrophobic and oleophobic film coating has a short long-term service life in high temperature and humid environments, and the cost is high, and it is difficult to maintain performance on different substrate surfaces, especially in windy sand and high temperature environments, which are susceptible to contamination.

Method used

Using a coating composition, including a first precursor composition and a second precursor composition, utilizing the hydrolysis of a fluorine-containing silane and a metal or metalloid compound by mixing in a solvent and forming a dense thin layer on a substrate The reaction forms a polymer that, combined with the appropriate catalysts and solvents, produces a coating with high hardness and self-cleaning properties.

Benefits of technology

Achieve high hardness, excellent self-cleaning properties and long-term durability coatings that form films on both smooth and rough substrates, reducing costs and maintaining performance under abrasion and environmental conditions without the need for additional primer applications layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725731A_ABST
    Figure CN118725731A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of functional coatings, and particularly relates to a coating composition, a coating, a preparation method and application. The coating composition provided by the invention comprises a first precursor composition, a second precursor composition and a solvent, the prepared coating has excellent optical performance, self-cleaning performance, high hardness and long-term durability, the performance can be kept under abrasion and environmental conditions, films can be formed on smooth and rough base material surfaces and different types of base materials, and film forming does not need to be achieved through an additional primer coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of functional coatings, and in particular relates to a coating composition, a coating, a preparation method and an application thereof. Background Art

[0002] In many current application fields, such as electronics and consumer products, such as solar panels, touch display panels, glass windows, and mobile phone and notebook cases, the surface needs to be kept free of pollution to ensure normal operation or visual appearance. However, in real environments, photovoltaic panels must consider the windy and sandy environment. The adhesion of particles will seriously affect the collection of optical signals. The sweat and grease on the fingers can easily contaminate the touch display panel and affect normal viewing.

[0003] In the prior art, a hydrophobic and oleophobic thin film coating is usually used as a protective layer. The thin film coating must be thin enough and have good optical properties so as not to affect the normal operation and appearance of the equipment. The coating must also have certain durability and wear resistance to ensure that the equipment or application can maintain a better performance during operation. At present, dense structures or fluorinated materials are usually selected to obtain certain hydrophobic and oleophobic properties, but material design and selection need to consider the film formation, film surface conditions, film surface adhesion, etc. of the material, among which the film surface flatness, film thickness, film surface optical transmittance, film surface water drop angle size, etc. affect the performance, and the adhesion of the film surface to the substrate affects the stability. At the same time, the cost of the material needs to be considered. For example, the use of a large amount of fluorinated solvents will increase the cost. There are also methods such as plasma enhanced chemical vapor deposition (PECVD) to prepare a single-layer coating structure, but this processing method has high requirements on the size of the equipment and substrate, and the prepared structure has poor long-term thermal stability, especially when exposed to high temperature or humid environment. The single-layer coating cannot pass harsh wear conditions and maintain a long service life.

[0004] Therefore, in order to adapt to the use requirements of different environments, the thin film coating is required to have higher hardness, excellent self-cleaning properties and high durability, and can maintain these properties under wear and environmental conditions, and can form a film on smooth and rough substrate surfaces, as well as on different types of substrates, and the film formation does not require an additional primer coating to achieve. Summary of the invention

[0005] Therefore, the technical problem to be solved by the present invention is to overcome the above-mentioned defects in the prior art, thereby providing a coating composition, a coating, a preparation method and an application.

[0006] To this end, the present invention provides the following technical solutions:

[0007] The present invention provides a coating composition, comprising: a first precursor composition, a second precursor composition and a solvent;

[0008] (a) The first precursor composition has a structural composition of M1(OR1) m R 2n (I), or, the first precursor composition is a polymer formed by at least partial hydrolysis of the compound represented by formula (I),

[0009] Among them, M1 is a metal or metalloid with a valence of x;

[0010] R1 is selected from C1-C 10 Organic or hybrid organic;

[0011] R2 is selected from C1-C 20 Organic or hybrid organic;

[0012] The value of M is 1 to x, the value of n is x-1 to 0, and m+n=x;

[0013] (b) The second precursor composition is selected from fluorine-containing silane or fluorine-containing polysiloxane containing a hydrolyzable group.

[0014] Optionally, the mass ratio of the first precursor composition to the second precursor composition is 100-0.1:1, preferably 60-0.2:1, and more preferably 35-0.5:1.

[0015] Optionally, the mass ratio of the total mass of the first precursor composition and the second precursor composition to the solvent is 10-0.02:100, preferably 5-0.05:100.

[0016] Optionally, in the first precursor, the valence of M1 is greater than 4; Optionally, M1 is at least one of Si, Ge, Sb, Ti or Zr; preferably Si;

[0017] and / or, R1 and R2 are independently selected from substituted or unsubstituted C1 to C 24 Alkyl, substituted or unsubstituted C3 to C 30 Cycloalkyl, substituted or unsubstituted C6 to C 30 Aryl or a combination thereof;

[0018] Preferably, R2 is C1-C 10 A fluorine-containing organic group or a fluorine-containing hybrid organic group, wherein, more preferably, the fluorine-containing organic group or the fluorine-containing hybrid organic group contains 1-20 fluorine atoms, and further preferably 3-17 fluorine atoms;

[0019] And / or, in the structure represented by formula (I), the value of n is 0-3, preferably 0-2.

[0020] Optionally, the method of forming a polymer from the compound represented by formula (I) comprises: reacting the compound represented by formula (I) to form a polymer under the action of a solvent and a catalyst;

[0021] Optionally, the catalyst is an organic acid or an organic base;

[0022] Optionally, the reaction temperature is 50-150° C., and the reaction time is 0.5-10 h.

[0023] Optionally, the fluorine-containing silane containing a hydrolyzable group in the second precursor composition has a structure shown in formula (II):

[0024] R F -Q-Si(OR3) a R 4b (II)

[0025] in:

[0026] R F is a fluorine-containing group, optionally, the fluorine-containing group R F It is a fluorine-containing long chain or a fluoropolyether group, usually having a molecular weight of 250-10000 g / mol, preferably 400-5000 g / mol;

[0027] Q is a divalent linking group; preferably an amide-containing group or an alkylene group;

[0028] R3 are each independently selected from C1-C 10 An organic group or a hybrid organic group, preferably an alkoxy group, an acyloxy group or an aryloxy group;

[0029] R4 are each independently selected from C1-C 20 Organic or hybrid organic groups:

[0030] a is 1, 2 or 3, preferably 2 or 3; b is 0, 1 or 2, preferably 0 or 1; a+b=3.

[0031] Optionally, the solvent includes at least one of a fluorine-containing solvent, an alcohol solvent, an alcohol ether solvent, and an ester solvent;

[0032] Optionally, the fluorine-containing solvent comprises at least one of a perfluorinated alkane, a partially fluorinated alkane;

[0033] The alcohol solvent includes at least one of aliphatic hydrocarbon monoalcohol and aliphatic hydrocarbon diol;

[0034] The alcohol ether solvent includes at least one of aliphatic hydrocarbon alcohol ethers;

[0035] The ester solvent includes at least one of aliphatic alkane esters;

[0036] Optionally, the solvent is a mixed solvent of a fluorine-containing solvent, an ether solvent and an alcohol solvent, and the mass composition ratio of the three is 10-0.1:10-0.1:5-0, and a more preferred ratio is 5-0.1:5-0.1:1-0.

[0037] The present invention also provides a method for preparing the above-mentioned coating composition, comprising the following steps: dissolving the first precursor composition and the second precursor composition in solvents respectively, and mixing them to obtain the coating composition.

[0038] The present invention also provides a coating, which is prepared from the above coating composition or the coating composition prepared by the above preparation method;

[0039] Optionally, the coating has a thickness of 10-500 nm;

[0040] Optionally, the method for preparing the coating comprises applying the coating composition onto a substrate and curing to obtain the coating;

[0041] Optionally, the substrate is selected from ceramic, glass, metal, natural or artificial stone, polymer material, paint, powder coating, wood or fiber substrate.

[0042] The present invention also provides an application of the coating in a solar panel, a display panel, an electronic product housing or a decoration field (such as a glass curtain wall in a building decoration field). DETAILED DESCRIPTION OF THE INVENTION

[0044] In this specification, when no other definition is provided, "organic group" refers to a substituent containing carbon atoms, including substituted or unsubstituted C1 to C 24 Alkyl, substituted or unsubstituted C3 to C 30 Cycloalkyl, substituted or unsubstituted C6 to C 30 Aryl or a combination thereof.

[0045] In the present specification, when no definition is otherwise provided, "hetero" means that at least one carbon atom is selected from a heteroatom including N, O, S, B and P, or at least one hydrogen atom is substituted with halogen.

[0046] In the present specification, when no definition is otherwise provided, "fluoro" refers to an organic group or a hybrid organic group as defined above, wherein at least one hydrogen atom is substituted with fluorine.

[0047] A coating composition, comprising: a first precursor composition, a second precursor composition and a solvent; wherein each component comprises:

[0048] a) The first precursor composition is a metal or metalloid compound having the structure M1(OR1) m R2n (I), or, the first precursor composition is a polymer formed by at least partial hydrolysis of the compound represented by formula (I);

[0049] Wherein, M1 is a metal or metalloid with a valence of x;

[0050] R1 is selected from C1-C 10 Organic or hybrid organic;

[0051] R2 is selected from C1-C 20 Organic group, hybrid organic group, fluorine-containing organic group or fluorine-containing hybrid organic group;

[0052] m is 1 to x, n is x-1 to 0, and m+n is x;

[0053] b) the second precursor composition is a fluorine-containing silane or fluorine-containing polysiloxane containing a hydrolyzable group,

[0054] c) the solvent combination at least includes a combination of fluorinated solvents, alcohols, alcohol ethers, and ester solvents,

[0055] Among them, the coating preparation method is to form a solution through a first precursor compound composition, a second precursor, and a solvent combination, and can form a film on a substrate through processes such as dip coating, slit coating, combined slit + spin coating, spin coating, spray coating, inkjet printing, curtain coating, roller coating, roll-to-roll coating, screen printing, etc., and then be formed through heat treatment.

[0056] The polymer formed by the compound represented by formula (I) is obtained by reacting the compound represented by formula (I) with a solvent and a catalyst to form a polymer.

[0057] In the first precursor composition, M1 is Si, Ge, Sb, Ti or Zr, preferably Si.

[0058] In an embodiment, the first precursor composition is one or more of a metal or a metalloid, wherein R1 and R2 are fluorine-free, and no fluorine-containing solvent is required in preparing the first precursor composition, or R1 or R2 contains at least one fluorine atom, and a combination solvent including a fluorine-containing solvent is required in preparing the first precursor composition. R1 and R2 are substituted or unsubstituted C1 to C 24 Alkyl, C3 to C 30 Cycloalkyl, C6 to C 30 The aryl group or a combination thereof, or contains heteroatoms, such as at least one halogen or 1-2 heteroatoms selected from N, O, S, B and P.

[0059] Preferably R1 is C1-C 15 Organic or C1-C 15 Hybrid organic group, more preferably C1-C 10The hydrocarbon group is more preferably a C1-C8 straight, branched or cyclic alkyl group or a hybrid organic group.

[0060] R2 is preferably C1-C 15 Organic or C1-C 15 Hybrid organic group, more preferably C1-C 10 A hydrocarbon group, more preferably a C1-C8 straight, branched or cyclic alkyl or a hybrid organic group. Another preferred R2 is C1-C 10 The fluorinated organic group or hybrid organic group preferably contains 1 to 20 fluorine atoms, more preferably 3 to 17 fluorine atoms.

[0061] In the case where the valence of the metal or metalloid M1 is 4 or more, m is preferably 1-X, more preferably 1-4, and n is preferably 0-3, more preferably 0-2.

[0062] In each compound represented by formula (I), R1 and R2 may be the same or different.

[0063] Suitable compounds of formula (I) are, for example, triethoxysilane, tetraethoxysilane, dimethyldiethoxysilane, diethyldimethoxysilane, dimethyldiethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, butyltriethoxysilane, methyldiethoxyvinylsilane, phenyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methylacrylpropyltrimethoxysilane, mercaptopropyltriethoxysilane, perfluorooctylethyl Triethoxysilane, perfluorodecylethyltriethoxysilane, pentafluorophenethyltrimethoxysilane, 1,2-bistrimethoxymethylsilylethane, 1,2-bistriethoxymethylsilylethane, 1,2-bistrimethoxymethylsilylmethane, 1,2-bistriethoxymethylsilylmethane, 1,2-bistriethoxymethylsilylmethane, 1,2-bis(diethoxymethylsilyl)methane, 1,2-bis(diethoxymethylsilyl)ethane, 1,2-bis(diethoxymethylsilyl)benzene and combinations thereof.

[0064] As mentioned above, at least partial hydrolysis is preferably carried out under acidic or basic conditions, usually using a catalyst such as sulfuric acid, hydrochloric acid, nitric acid, acetic acid, trifluoromethanesulfonic acid, perfluorobutyric acid or other inorganic or organic acids, acidic ion resins, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, ammonia, triethylamine or other inorganic or organic bases, basic ion resins, such as C1-C6 trialkylamines.

[0065] When an acid or base is used, the concentration is preferably 0.01-10 mol / l, more preferably 0.05-0.5 mol / l. The acid or base is usually dissolved in water or in a mixture of water and an organic solvent, and the organic solvent is preferably an alcohol or a ketone, such as propylene glycol methyl ether, isopropanol, acetone, methyl isobutyl ketone, and cyclohexanone.

[0066] The at least partial hydrolysis is preferably carried out at a temperature of 50-150°C, more preferably 80-120°C.

[0067] The at least partial hydrolysis is preferably carried out for 0.5 to 10 hours, preferably 1.0 to 3.5 hours.

[0068] When the first precursor composition is a polymer formed by at least partial hydrolysis of the compound represented by formula (I), one or more solvents may be used in its preparation process. The solvent is selected from alcohols, preferably alcohols containing 1 to 6 carbon atoms, such as methanol, ethanol, propanol, butanol; ether alcohols, such as propylene glycol monomethyl ether, dipropylene glycol methyl ether, diethylene glycol methyl ether, ketones, such as acetone, methyl isobutyl ketone; esters, such as propylene glycol monomethyl ether acetate, ethyl acetate, butyl acetate; and ethers, such as diethyl ether, THF; preferably alcohols, ether alcohols or ketones.

[0069] The first precursor composition can be a compound or a polymer of a compound, such as methyl silicone resin, MQ silicone resin, phenyl silicone resin, fluorine-containing silicone resin and a combination thereof.

[0070] The second precursor composition is a fluorine-containing silane or a fluorine-containing polysiloxane containing a hydrolyzable group,

[0071] The fluorine-containing silicon compound comprising a hydrolyzable group is preferably selected from the compounds of the following formula (II):

[0072] R F -Q-Si(OR3) a R 4b (II)

[0073] in:

[0074] R F is a fluorine-containing group;

[0075] Q is a divalent linking group; preferably an amide-containing group and an alkylene group;

[0076] R3 are each independently selected from C1-C 10 Organic or hybrid organic groups: preferably alkoxy, acyloxy and aryloxy;

[0077] R4 are each independently selected from C1-C 20 Organic or hybrid organic;

[0078] a is 1, 2 or 3, preferably 2 or 3; b is 0, 1 or 2, preferably 0 or 1; a+b=3;

[0079] Fluorinated group R F It is a fluorine-containing long chain group or a fluoropolyether group, and generally has a molecular weight of 250-10000 g / mol, preferably 400-5000 g / mol.

[0080] Fluorinated group R F It may be a straight chain or branched group, preferably a straight chain group.

[0081] In the fluoropolyether group R F In the case where hydrogen atoms are present, the molecular ratio of fluorine to hydrogen is preferably at least 10. More preferably, the fluorine-containing group R F It is a perfluoropolyether group.

[0082] Fluorinated long chain group R F C1-C 20 Fluorinated long chain, preferably C1-C 12 Contains long fluorinated chains.

[0083] Fluoropolyether group R F The repeating unit is preferably a C1-C6 fluorinated diol, more preferably a C1-C4 fluorinated diol, and most preferably a C1-C3 fluorinated diol.

[0084] The perfluoropolyether group may be divalent or monovalent, wherein the preferred structure of the divalent perfluoropolyether group includes:

[0085] -CF2O(CF2O) x (C2F4O) y CF2-, where the average of x and y is 0-45, provided that x and y are not simultaneously zero,

[0086] -CF(CF3)O(CF(CF)CF2O) z CF(CF3)-,

[0087] -CF2O(C2F4O) z CF2- and

[0088] -(CF2)3O(C2F4O) z (CF2)3-

[0089] The average value of z is 3-45.

[0090] Preferred structures of monovalent perfluoropolyether groups include:

[0091] CF3CF2O(CF2O) x (C2F4O) y CF2-,

[0092] CF3CF2O(C2F4O) y CF2-,

[0093] CF3CF2CF2O(CF(CF3)CF2O) y CF(CF3)-,

[0094] or a combination thereof, wherein the average values ​​of x and y are 0-45, and x and y are not 0 at the same time.

[0095] The weight ratio of the first precursor composition to the second precursor is 100-0.1:1, preferably 60-0.2:1, and more preferably 35-0.5:1.

[0096] The weight ratio of the first precursor composition to the second precursor to the solvent is 10-0.02:100, preferably 5-0.05:100.

[0097] Among them, the solvent is a combination of fluorinated solvents, ethers, alcohols, and ester solvents. The fluorinated solvent is preferably a perfluorinated alkane, a partially fluorinated alkane, the alcohol is preferably an aliphatic monoalcohol, an aliphatic diol, the alcohol ether is an aliphatic alcohol ether, and the ester is preferably an aliphatic alkane ester.

[0098] The solvent that can be added is selected from alcohols, preferably alcohols containing 1-6 carbon atoms, such as methanol, ethanol, isopropanol, butanol; ether alcohols, such as propylene glycol monomethyl ether, dipropylene glycol methyl ether, propylene glycol methyl ether acetate; esters such as ethyl acetate, butyl acetate; ethers such as partially or completely fluorinated ethers; particularly preferably alcohols, preferably alcohols containing 1-6 carbon atoms, such as methanol, ethanol, ethylene glycol, isopropanol, propylene glycol, butanol, dipropylene glycol; ether alcohols, such as propylene glycol monomethyl ether, dipropylene glycol methyl ether, partially or completely fluorinated ethers, ethylene glycol or mixtures thereof; for example methoxynonafluorobutane, methylnonafluorobutyl ether, methylnonafluoroisobutyl ether, ethoxynonafluorobutane, perfluorobutyl ethyl ether, ethyl acetate, butyl acetate, n-hexane, n-heptane, n-pentane, isopropanol, ethanol, butanol, propylene glycol monomethyl ether, propylene glycol, dipropylene glycol.

[0099] The solvent is a mixed solvent of a fluorine-containing solvent, an ether solvent and an alcohol solvent, and the mass composition ratio of the three is 10-0.1:10-0.1:5-0, and a more preferred ratio is 5-0.1:5-0.1:1-0.

[0100] The coating composition provided by the present invention can generally be added with common additives for coating compositions for thin films. Such commonly used additives include, for example, surfactants, leveling agents, processing aids, antistatic agents, antioxidants, water and oxygen scavengers, catalysts, photoinitiators or mixtures thereof. In some cases, scattering particles may also be preferably introduced into the film coating solution. Such particles generally provide additional optical effects, for example to meet specific requirements, for example for lighting applications. These particles may, for example, be silicon oxide, titanium oxide, zirconium oxide or similar inorganic particles.

[0101] The temperature for preparing the coating composition is preferably 0-75° C., more preferably 10-50° C. The reaction time is usually less than 24 hours, preferably 3-12 hours.

[0102] The coating is prepared by forming a thin layer on a substrate, suitable substrates include ceramics, glass, metals, natural and artificial stones, polymer materials (e.g. poly(meth)acrylates, polycarbonates, polystyrenes, styrene copolymers such as styrene acrylonitrile copolymers, polyesters, polyethylene terephthalate), paints (e.g. those based on acrylic resins), powder coatings (e.g. polyurethane or hybrid powder coatings), wood and fiber substrates (e.g. textiles, leather, carpets, paper). Preferably, the substrate is selected from ceramics, glass, metals, polymer materials (e.g. poly(meth)acrylates, polycarbonates, polystyrenes, styrene copolymers such as styrene acrylate copolymers, polyesters, polyethylene terephthalate), natural and artificial stones; more preferably selected from metals, ceramics, glass and polymer materials (e.g. poly(meth)acrylates, polycarbonates, polystyrenes, styrene copolymers such as styrene acrylate copolymers, polyesters, polyethylene terephthalate).

[0103] The obtained composition can be deposited on a substrate by techniques such as spraying, spin coating, roller coating, rod coating, and slit coating. For each deposition technique, the formulation, material composition, solvent system, and additives must be selected in a manner suitable for the specific deposition technique. It is particularly advantageous for the novel material described in the present invention that other solvents except fluorinated solvents can be used in combination with material deposition. In order to obtain satisfactory optical, mechanical and chemical properties, the film thickness, coating uniformity, and coating quality of the coating must be optimized. By adjusting the material composition ratio, solvent formulation, and deposition parameters, the film thickness, coating uniformity, and coating quality can be optimized. The material of the present invention allows particularly high adjustability in composition and formulation to suit the wide range of liquid deposition techniques used. In addition, when optimizing the low temperature curing performance of the material, for example, when working at a curing temperature of 80°C, the solvent mixture must be optimized so that all solvents can evaporate during thermal curing to promote the desired film properties.

[0104] The thickness of the prepared films is 10-500nm.

[0105] The technical solution of the present invention has the following advantages:

[0106] The coating composition provided by the present invention comprises: a first precursor composition, a second precursor composition and a solvent; the prepared coating can form a thin but dense layer on a substrate, the coating has excellent optical properties, self-cleaning properties, high hardness and long-term durability, and can maintain these properties under wear and environmental conditions, can form a film on smooth and rough substrate surfaces, and on different types of substrates, and the film formation does not require an additional primer coating to achieve. BRIEF DESCRIPTION OF THE DRAWINGS

[0107] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0108] Figure 1 This is a water drop angle test diagram of Example 1 of the present invention. DETAILED DESCRIPTION

[0109] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0110] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0111] Example 1

[0112] This embodiment provides a coating composition, and its specific composition and preparation method are as follows:

[0113] Preparation of the first precursor polymer solution

[0114] 35.92 g of tetraethoxysilane and 150 g of acetone were added to a round-bottom flask, and 25.3 g of 0.1 M hydrochloric acid was added dropwise. After the addition was completed, the temperature was raised to 90° C. and reacted for 2 h. After cooling, the solvent acetone was distilled off, and 115 g of propylene glycol methyl ether was added to obtain a first precursor solution 1.

[0115] Preparation of the second precursor solution

[0116] The second precursor solution 2 was prepared by diluting the anti-fingerprint fluorinated liquid Optool UD509 with perfluorobutyl ether Novel 7200 from 20% to 0.4%.

[0117] Composition preparation

[0118] 35.1 g of the first precursor solution 1, 56.5 g of the second precursor solution 2, 158.2 g of Novel7200, 172.3 g of propylene glycol monomethyl ether and 13.5 g of ethylene glycol were added to a round-bottom flask and stirred at room temperature overnight to obtain a coating composition.

[0119] Example 2

[0120] This embodiment provides a coating composition, and its specific composition and preparation method are as follows:

[0121] Preparation of the first precursor polymer solution

[0122] 28.3 g of tetraethoxysilane, 7.6 g of methyltriethoxysilane and 150 g of acetone were added to a round-bottom flask, and 25.8 g of 0.1 M hydrochloric acid was added dropwise. After the addition was completed, the temperature was raised to 95° C. and refluxed for 2 h. After cooling, the solvent acetone was distilled off, and 120 g of propylene glycol methyl ether was added to obtain a first precursor solution 2.

[0123] The second precursor solution was prepared in the same manner as in Example 1.

[0124] Composition preparation

[0125] 38.1 g of the first precursor solution 2, 57.8 g of the second precursor solution 2, 160.5 g of Novel7200, 168.8 g of propylene glycol monomethyl ether and 12.5 g of ethylene glycol were added to a round-bottom flask and stirred at room temperature overnight to obtain a coating composition.

[0126] Example 3

[0127] This embodiment provides a coating composition, and its specific composition and preparation method are as follows:

[0128] Preparation of the first precursor polymer solution

[0129] 25.1 g of tetraethoxysilane, 5.8 g of 1,2-bistriethoxymethylsilylethane and 100 g of isopropanol were added to a round-bottom flask, and 22.0 g of 0.1 M nitric acid was added dropwise. After the addition was completed, the temperature was raised to 90° C. and reacted for 2 h. After cooling, 20 g of isopropanol was added to obtain a first precursor solution 3.

[0130] Preparation of the second precursor solution

[0131] The second precursor solution 1 was prepared by diluting Optool UD509 with perfluorobutyl methyl ether Novel 7100 from 20% to 0.4%.

[0132] Composition preparation

[0133] 36.6 g of the first precursor solution 3, 52.0 g of the second precursor solution 1, 158.7 g of Novel7100, 173.5 g of propylene glycol monomethyl ether and 9.5 g of ethylene glycol were added to a round-bottom flask and stirred at room temperature overnight to obtain a coating composition.

[0134] Example 4

[0135] This embodiment provides a coating composition, and its specific composition and preparation method are as follows:

[0136] Composition preparation

[0137] Take 35.5g of the first precursor solution methyl silicone resin (Shin-Etsu Chemical KL-220L, diluted to 10% with propylene glycol monomethyl ether), 56.8g of the second precursor solution 2 (prepared by the same method as in Example 1), 162.5g of Novel7200, 168.8g of propylene glycol monomethyl ether and 11.2g of ethylene glycol, add them into a round-bottom flask, stir at room temperature overnight, and obtain a coating composition.

[0138] Example 5

[0139] This embodiment provides a coating composition, and its specific composition and preparation method are as follows:

[0140] Preparation of the first precursor polymer solution

[0141] Add 27.5 g of tetraethoxysilane, 8.6 g of methyltriethoxysilane, 5.2 g of perfluorooctylethyltrimethoxysilane and 150 g of acetone into a round-bottom flask, add 2.5 g of acidic ion resin and 1.5 g of water, heat to 90 ° C for 2 h, filter out the ion resin after cooling, distill off the solvent acetone, add 130 g of propylene glycol methyl ether, and obtain the first precursor solution 4.

[0142] Preparation of the second precursor solution

[0143] The anti-fingerprint solution PPG EC700X was diluted with Novel 7200 from 20% to 0.4% to prepare the second precursor solution 3.

[0144] Composition preparation

[0145] 36.1 g of the first precursor solution 4, 58.5 g of the second precursor solution 3, 155.2 g of Novel7200, 168.1 g of propylene glycol monomethyl ether and 11.5 g of ethylene glycol were added to a round-bottom flask and stirred at room temperature overnight to obtain a coating composition.

[0146] Example 6

[0147] This embodiment provides a coating composition, and its specific composition and preparation method are as follows:

[0148] Preparation of the first precursor polymer solution

[0149] 28.3 g of tetraethoxysilane, 4.2 g of methyltriethoxysilane, 5.6 g of 3-(2,3-epoxypropoxy)propyltrimethoxysilane and 150 g of acetone were added to a round-bottom flask, and 25.3 g of 0.1 M nitric acid was added dropwise. After the addition was completed, the temperature was raised to 90° C. and the reaction was carried out for 2 h. After cooling, the solvent acetone was distilled off, and 135 g of propylene glycol methyl ether was added to obtain a first precursor solution 5.

[0150] Preparation of the second precursor solution

[0151] The second precursor solution 4 was prepared by diluting perfluorodecylethyltriethoxysilane with 3-methoxy-2-trifluoromethyldecafluoropentane to 0.4%.

[0152] Composition preparation

[0153] 38.5 g of the first precursor solution 5, 62.5 g of the second precursor solution 4, 160.1 g of Novel7200, 176.2 g of propylene glycol monomethyl ether and 12.5 g of ethylene glycol were added to a round-bottom flask and stirred at room temperature overnight to obtain a coating composition.

[0154] Example 7

[0155] This embodiment provides a coating composition, and its specific composition and preparation method are as follows:

[0156] Composition preparation

[0157] Take 35.5g of the first precursor solution methylphenyl silicone resin (Shin-Etsu Chemical KR-112, diluted to 10% with propylene glycol methyl ether), 65.2g of the second precursor 2 (prepared by the same method as in Example 1), 156.6g of Novel7200, 168.2g of propylene glycol monomethyl ether and 11.5g of ethylene glycol, add them into a round-bottom flask, stir at room temperature overnight, and obtain a coating composition.

[0158] Example 8

[0159] This embodiment provides a coating composition, and its specific composition and preparation method are as follows:

[0160] Preparation of the first precursor polymer solution

[0161] 27.1 g of tetraethoxysilane, 6.2 g of 1,2-bistriethoxymethylsilylethane, 3.8 g of methyltrimethoxysilane and 150 g of acetone were added to a round-bottom flask, and 26.5 g of 0.1 M nitric acid was added dropwise. After the addition was completed, the temperature was raised to 90° C. and the reaction was carried out for 2 h. After cooling, the solvent acetone was distilled off, and 135 g of propylene glycol methyl ether was added to obtain a first precursor solution 6.

[0162] Composition preparation

[0163] 36.5 g of the first precursor solution 6, 58.1 g of the second precursor solution 2 (prepared by the same method as in Example 1), 165.3 g of Novel 7200, 176.1 g of propylene glycol monomethyl ether and 12.1 g of ethylene glycol were added to a round-bottom flask and stirred at room temperature overnight to obtain a coating composition.

[0164] Example 9

[0165] This embodiment provides a coating composition, and its specific composition and preparation method are as follows:

[0166] Preparation of the first precursor polymer solution

[0167] 27.1 g of tetraethoxysilane, 6.8 g of 1,2-bistriethoxymethylsilylethane, 3.5 g of phenyltrimethoxysilane and 150 g of acetone were added to a round-bottom flask, and 26.3 g of 0.1 M nitric acid was added dropwise. After the addition was completed, the temperature was raised to 90° C. and the reaction was carried out for 2 h. After cooling, the solvent acetone was distilled off, and 125 g of propylene glycol methyl ether was added to obtain a first precursor solution 7.

[0168] Composition preparation

[0169] 35.2 g of the first precursor solution 7, 56.1 g of the second precursor solution 2 (prepared by the same method as in Example 1), 165.5 g of Novel 7200, 178.6 g of propylene glycol monomethyl ether and 10.1 g of ethylene glycol were added to a round-bottom flask and stirred at room temperature overnight to obtain a coating composition.

[0170] Example 10

[0171] This embodiment provides a coating composition, and its specific composition and preparation method are as follows:

[0172] Preparation of the first precursor polymer solution

[0173] 28.7 g of tetraethoxysilane, 5.6 g of 1,2-bistriethoxymethylsilylethane, 3.8 g of perfluorooctylethyltrimethoxysilane and 150 g of acetone were added to a round-bottom flask, and 26.1 g of 0.1 M nitric acid was added dropwise. After the addition was completed, the temperature was raised to 90° C. for reaction for 2 h. After cooling, the solvent acetone was distilled off, and 135 g of propylene glycol methyl ether was added to obtain a first precursor solution 8.

[0174] Composition preparation

[0175] 35.5 g of the first precursor solution 8, 57.2 g of the second precursor solution 2 (prepared by the same method as in Example 1), 165.8 g of Novel 7200, 175.5 g of propylene glycol monomethyl ether and 11.5 g of ethylene glycol were added to a round-bottom flask and stirred at room temperature overnight to obtain a coating composition.

[0176] Comparative Example 1

[0177] Compared with Example 1, two coatings were prepared using the first and second precursor solutions of Example 1, respectively.

[0178] Comparative Example 2

[0179] Compared with Example 1, the first precursor solution is replaced by trifluoropropyltrimethoxysilane with a solid content of 10%.

[0180] Comparative Example 3

[0181] Compared with Example 1, the second precursor solution is replaced by tetraethoxysilane with a solid content of 0.4%.

[0182] Test Case

[0183] The obtained coating composition can be deposited on a substrate by techniques such as spraying, spin coating, roller coating, rod coating, and slit coating. For each deposition technique, the formulation, material composition, solvent system, and additives must be selected in a manner suitable for the specific deposition technique. It is particularly advantageous for the novel material described in the present invention that other solvents besides fluorinated solvents can be used in combination with material deposition. In order to obtain satisfactory optical, mechanical, and chemical properties, the film thickness, coating uniformity, and coating quality of the coating must be optimized. By adjusting the material composition, formulation, and deposition parameters, the film thickness, coating uniformity, and coating quality can be optimized. The material of the present invention allows particularly high adjustability in composition and formulation to suit the wide range of liquid deposition techniques used. In addition, when optimizing the low temperature curing properties of the material, such as working at a curing temperature of 80°C, the solvent mixture must be optimized so that all solvents can evaporate during thermal curing to promote the desired film properties.

[0184] For purposes of the examples, spray coating is described as the coating method of choice.

[0185] Application examples:

[0186] The films were prepared by using a spray tool on pretreated (plasma) glass, anodized aluminum or ceramic substrates.

[0187] In this test example, the substrate is soda-lime glass and the following sample cleaning process is used:

[0188] 1) Alkaline cleaning (RBS or similar alkaline cleaning solution PH 10);

[0189] 2) Deionized water cleaning:

[0190] 3) Plasma cleaning.

[0191] Typical spraying process parameters used to prepare samples from the material synthesis example:

[0192] Scanning speed: 300 mm / s;

[0193] Spacing-: 50mm;

[0194] Gap: 100mm;

[0195] Flow rate: 5-6mL / min:

[0196] Atomizing air pressure: 5kg / cm 2 ;

[0197] The spraying process is followed by heat curing, for example, at 150° C. for 60 minutes (for glass and ceramics) and at 80° C. for 120 minutes (for anodized aluminum and other metals), either in an oven or on a conveyor belt.

[0198] The prepared samples were characterized, and the specific test method was as follows:

[0199] Film thickness and refractive index

[0200] The film thickness and refractive index were measured by using an ellipsometer (Wuhan Yiguang). Silicon wafers (diameter: 150 mm, type / dopant: P / Bor, orientation: <1-0-0>, resistivity: 1-30 ohm cm, thickness: 675 + / - 25 um, TTV: <5 um, particles: <20 @ 0.2 um, front: polished, back: etched, flat: lSEMI standard) were used as substrates for measurement. The film thickness and refractive index were measured by using a spray tool (typical spray process: scanning rate: 300 mm / s; spacing: 50 mm; gap: 100 mm; flow rate: 5-6 ml / min: atomization pressure: 5 kg / cm 2 ), an example of preparing a material film on a pre-treated (plasma) silicon wafer substrate, followed by thermal curing at 150°C for 60 minutes.

[0201] Transmittance

[0202] The transmittance was tested using Shimadzu UV-1800.

[0203] Pencil hardness (PEHA)

[0204] Pencil hardness was measured according to ASTM standard 03363-00 using an Elcometer pencil hardness tester.

[0205] Water contact angle (CA):

[0206] The static contact angle measurement was performed by using an optical surface tension meter with distilled water, a drop size of 4ul, and the average value of three measurement points was recorded as the measurement result value, and the Young-Laplace equation was used as a numerical method to describe the profile of the droplet (tool: Attension Theta optical surface tension meter). The water contact angle test diagram of Example 1 is shown in FIG. Figure 1 In addition to water, water is replaced with oil when testing the oil contact angle.

[0207] Wear

[0208] Wear tests were performed using Bon Star steel wool ++0000, 1 kg load, 1 x 1 cm indenter, 2 inch stroke, 6 WC / min rate. (Tool: Taber Linear Abraser, 5750). Wear test evaluation criteria: initial water contact angle, water contact angle measurement at 1000 cycle intervals (up to 8000 cycles) and visual inspection of surface damage / visual scratch inspection at 1000 cycle intervals (up to 8000 cycles). Water contact angle was measured according to the water contact angle measurement method, and visual inspection was performed under microscope inspection and green and red light quality light inspection. In addition to steel wool, cotton cloth and Minoan eraser were also used to test wear performance.

[0209] And the data is summarized in the following table.

[0210] Table 1 Coating properties

[0211]

[0212]

[0213] Table 2 Coating properties

[0214]

[0215] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A coating composition, characterized in that include: a first precursor composition, a second precursor composition, and a solvent; (a) The first precursor composition has a structural composition of M1(OR1) m R 2n (I), or, the first precursor composition is a polymer formed by at least partial hydrolysis of the compound represented by formula (I), Among them, M1 is a metal or metalloid with a valence of x; R1 is selected from C1-C 10 Organic or hybrid organic; R2 is selected from C1-C 20 Organic or hybrid organic; The value of M is 1 to x, the value of n is x-1 to 0, and m+n=x; (b) The second precursor composition is selected from fluorine-containing silane or fluorine-containing polysiloxane containing a hydrolyzable group.

2. The coating composition according to claim 1, characterized in that The mass ratio of the first precursor composition to the second precursor composition is 100-0.1:1, preferably 60-0.2:1, and more preferably 35-0.5:

1.

3. The coating composition according to claim 1 or 2, characterized in that The mass ratio of the total mass of the first precursor composition and the second precursor composition to the solvent is 10-0.02:100, preferably 5-0.05:

100.

4. The coating composition according to claim 1, characterized in that In the first precursor, the valence of M1 is greater than 4; optionally, M1 is at least one of Si, Ge, Sb, Ti or Zr; preferably Si; and / or, R1 and R2 are independently selected from substituted or unsubstituted C1 to C 24 Alkyl, substituted or unsubstituted C3 to C 30 Cycloalkyl, substituted or unsubstituted C6 to C 30 Aryl or a combination thereof; Preferably, R2 is C1-C 10 A fluorine-containing organic group or a fluorine-containing hybrid organic group, wherein, more preferably, the fluorine-containing organic group or the fluorine-containing hybrid organic group contains 1-20 fluorine atoms, and further preferably 3-17 fluorine atoms; And / or, in the structure represented by formula (I), the value of n is 0-3, preferably 0-2.

5. The coating composition according to claim 1, characterized in that The method for forming a polymer from a compound represented by formula (I) comprises: reacting the compound represented by formula (I) to form a polymer under the action of a solvent and a catalyst; Optionally, the catalyst is an organic acid or an organic base; Optionally, the reaction temperature is 50-150° C., and the reaction time is 0.5-10 h.

6. The coating composition according to claim 1, characterized in that The fluorine-containing silane containing a hydrolyzable group in the second precursor composition has a structure shown in formula (II): R F -Q-Si(OR3) a R 4b (II) in: R F is a fluorine-containing group, optionally, the fluorine-containing group R F It is a fluorine-containing long chain or a fluoropolyether group, usually having a molecular weight of 250-10000 g / mol, preferably 400-5000 g / mol; Q is a divalent linking group; preferably an amide-containing group or an alkylene group; R3 are each independently selected from C1-C 10 An organic group or a hybrid organic group, preferably an alkoxy group, an acyloxy group or an aryloxy group; R4 are each independently selected from C1-C 20 Organic or hybrid organic groups: a is 1, 2 or 3, preferably 2 or 3; b is 0, 1 or 2, preferably 0 or 1; a+b=3.

7. The coating composition according to claim 1, characterized in that The solvent includes at least one of a fluorine-containing solvent, an alcohol solvent, an alcohol ether solvent, and an ester solvent; Optionally, the fluorine-containing solvent comprises at least one of a perfluorinated alkane, a partially fluorinated alkane; The alcohol solvent includes at least one of aliphatic hydrocarbon monoalcohol and aliphatic hydrocarbon diol; The alcohol ether solvent includes at least one of aliphatic alcohol ethers; The ester solvent includes at least one of aliphatic alkane esters; Optionally, the solvent is a mixed solvent of a fluorine-containing solvent, an ether solvent and an alcohol solvent, and the mass composition ratio of the three is 10-0.1:10-0.1:5-0, and a more preferred ratio is 5-0.1:5-0.1:1-0.

8. A method for preparing the coating composition according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: dissolving the first precursor composition and the second precursor composition in solvents respectively, mixing them, and obtaining the coating composition.

9. A coating, characterized in that: Prepared by the coating composition according to any one of claims 1 to 7 or the coating composition prepared by the preparation method according to claim 8; Optionally, the coating has a thickness of 10-500 nm; Optionally, the method for preparing the coating comprises applying the coating composition onto a substrate and curing to obtain the coating; Optionally, the substrate is selected from ceramic, glass, metal, natural or artificial stone, polymer material, paint, powder coating, wood or fiber substrate.

10. Use of the coating according to claim 9 in the fields of solar panels, display panels, electronic product housings or decoration.

Citation Information

Patent Citations

  • Coating easy to clean

    CN113015581A

  • Organopolysiloxane and coating composition containing same

    CN115216020A