Low-density flame-retardant smoke-suppression epoxy composite material and preparation method thereof
Through the synergistic effect of lignin-modified epoxy resin and silicone-modified polyetheramine, combined with carbon black filler, a cross-linked network structure is constructed, which solves the insulation and lightweight properties caused by adding halogen-free flame retardants to epoxy resin. It significantly improves the flame retardant and smoke suppression performance and is suitable for high-power electronic packaging materials.
Patent Information
- Application Number
- CN202410819658.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-01
AI Technical Summary
The addition of halogen-free flame retardants to epoxy resin leads to a decrease in insulation and lightweight properties, and the high density and conductivity of traditional inorganic filler flame retardants limit its application.
Using lignin-modified epoxy resin and silicone-modified polyetheramine, through the substitution reaction of lignin phenolic hydroxyl active groups and epoxy resin and the chemical reaction of hydrogen-containing polysiloxane silicon hydrogen groups, combined with carbon black Fillers and dispersants build a cross-linked network structure with good compatibility to improve flame retardant and smoke suppression properties.
It maximizes the flame retardant performance and smoke suppression performance of epoxy composite materials, meets the fire retardant and flame retardant requirements of high-power electronic packaging materials, while maintaining insulation and lightweight properties.
Smart Images

Figure CN118725820A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electronic packaging, and in particular relates to a low-density flame-retardant and smoke-suppressing epoxy composite material and a preparation method thereof. Background Art
[0002] Epoxy composite materials are widely used due to their excellent mechanical properties, good bonding properties and other advantages. Due to the influence of its own molecular chain structure, epoxy resin is a flammable material with a limiting oxygen index of less than 20. It will produce a lot of smoke after burning, and the self-extinguishing effect after burning is poor, which is an extremely fatal weakness for packaging materials. As the electronics industry gradually develops towards high power, heat generation and accumulation have become the norm, so the safety requirements for fire retardancy are getting higher and higher. At present, most electronic packaging applications have put forward flame retardant requirements for epoxy packaging materials.
[0003] In recent years, there have been many reports on the research of epoxy resin flame retardants. In the past three decades, halogen compounds have been used to improve the flame retardancy of epoxy encapsulation materials due to their high efficiency. However, most halogen flame retardants are harmful to human health and are prone to environmental problems. At the same time, halogen flame retardants have obvious corrosion phenomena on electronic components under long-term use, which greatly affects the service life of electronic components, and therefore are restricted in use. At present, halogen-free flame retardants have become an important way to study the flame retardancy of epoxy resin encapsulation materials. Traditional inorganic filler flame retardants include aluminum hydroxide, magnesium hydroxide, graphite oxide, alumina, silicon dioxide, etc., which can be used as a halogen-free flame retardant to improve the flame retardancy of epoxy resin. However, due to their high density and conductivity, coupled with the poor compatibility of these materials with epoxy resin, the insulation and lightweight properties of epoxy resin are reduced, limiting further application. Lignin is a renewable, widely available, and low-cost bio-based polymer raw material. Research on the application of modified lignin in polymer polymer materials has excellent application value for controlling environmental pollution and making full use of renewable resources. However, some disadvantages of lignin-based flame retardants, especially their poor dispersion uniformity due to particle aggregation, limit their widespread application in epoxy resins. Summary of the invention
[0004] In view of the problem in the prior art that the addition of halogen-free flame retardant to epoxy resin leads to a decrease in the insulation and lightweight performance of epoxy resin, the present invention provides a low-density flame-retardant and smoke-suppressing epoxy composite material.
[0005] The low-density flame-retardant and smoke-suppressing epoxy composite material comprises a resin component A and a curing agent component B, wherein the component A comprises the following components in parts by weight:
[0006]
[0007]
[0008] The B component includes the following components in parts by weight:
[0009] 10-40 parts of silicone modified polyetheramine;
[0010] 1 to 10 parts of defoaming agent.
[0011] Furthermore, the mass ratio of the component A to the component B is (10:1) to (1:1).
[0012] Furthermore, the lignin-modified epoxy resin is prepared by a substitution reaction of lignin phenolic hydroxyl active groups with an epoxy resin, the lignin is selected from one or more of cellulose, hemicellulose, S-lignin, G-lignin and H-lignin, and the epoxy resin is selected from one or more of bisphenol A epoxy resin, halogenated bisphenol A epoxy resin, bisphenol S epoxy resin, bisphenol F epoxy resin, glycerol epoxy resin, ethylene glycol epoxy resin, phenolic epoxy resin and amino epoxy resin.
[0013] Furthermore, the organosilicon-modified polyetheramine is prepared by a chemical reaction of a hydrogen-containing polysiloxane silicon hydrogen group and a polyetheramine, the hydrogen-containing polysiloxane polymer corresponding to the hydrogen-containing polysiloxane silicon hydrogen group is selected from one or more of a linear hydrogen-containing polysiloxane, a cyclic hydrogen-containing polysiloxane, a cross-linked hydrogen-containing polysiloxane, and a modified hydrogen-containing polysiloxane, and the polyetheramine is selected from one or more of a monofunctional polyetheramine, a difunctional polyetheramine, and a trifunctional polyetheramine.
[0014] Further, the diluent is an alicyclic reactive diluent;
[0015] The reinforcing filler is carbon black, and its particle size is 20um-40um;
[0016] The dispersant is carbon black, and its particle size is 1nm-100nm;
[0017] The defoamer is selected from one or more of an organic silicon defoamer, a polyoxyethylene defoamer and an inorganic defoamer.
[0018] The invention also provides a method for preparing the low-density flame-retardant and smoke-suppressing epoxy composite material.
[0019] The preparation method of the low-density flame-retardant and smoke-suppressing epoxy composite material comprises the following steps:
[0020] The component A and the component B are mixed and stirred to obtain an epoxy composite material.
[0021] Further, the A component is prepared by the following method:
[0022] 10 to 20 parts by weight of a diluent are added to 20 to 100 parts by weight of the lignin-modified epoxy resin, and then 1 to 10 parts by weight of the dispersant and 10 to 50 parts by weight of the reinforcing filler are added, and then the mixture is put into a planetary mixer for high-speed dispersion for 30 to 50 minutes at a rotation speed of 2000 rpm to 4000 rpm.
[0023] Furthermore, the lignin-modified epoxy resin is prepared by the following method:
[0024] (1) Add 20-80 parts by weight of lignin and the first solvent into a four-necked round-bottom flask, heat to 100-200° C., mechanically stir for 1-5 hours to mix evenly, and filter;
[0025] (2) adding 10-100 parts by weight of epoxy resin to the mixture, mixing evenly, and then dropping 0.1-1 parts by weight of the first catalyst, reacting for 4-8 hours, then cooling to 25° C., performing reduced pressure distillation, and removing the solvent;
[0026] (3) Finally, centrifugation is performed to obtain a brown-black viscous liquid, which is the lignin-modified epoxy resin.
[0027] The first solvent is selected from one or more of toluene, xylene, n-butanol, cyclohexane, and heptane; the first catalyst is an organic base catalyst, selected from one or more combinations of sodium methoxide, sodium ethoxide, sodium isopropoxide, and sodium phthalate; and the amount of the first catalyst added is 0.05%-1% of the total mass of all raw materials in the preparation process of the lignin-modified epoxy resin.
[0028] Furthermore, the B component is prepared by the following method: 10 to 40 parts by weight of the organosilicon-modified polyetheramine and 1 to 10 parts by weight of a defoamer are added into a stirring kettle and stirred for 10 to 30 minutes at a rotation speed of 50 rpm to 120 rpm.
[0029] Furthermore, the organosilicon-modified polyetheramine is prepared by the following method:
[0030] (1) Add 10-100 parts by weight of polyetheramine and a second solvent into a three-necked flask, heat to 100-200° C., and mechanically stir for 1-5 hours to mix evenly;
[0031] (2) slowly dropwise adding 10-100 parts by weight of hydrogen-containing polysiloxane, mixing evenly, dropwise adding 0.1-1 parts by weight of the second catalyst, reacting for 4-8 hours, then cooling to 25° C., performing reduced pressure distillation to remove the solvent;
[0032] (3) Finally, centrifugation is performed to obtain a yellow viscous liquid, which is the siloxane-modified curing agent.
[0033] The second solvent is selected from one or more of toluene, xylene, n-butanol, cyclohexane, and heptane; the second catalyst is an organic base catalyst selected from one or more of sodium methoxide, sodium ethoxide, sodium isopropoxide, and sodium phthalate; and the amount of the second catalyst added is 0.05%-1% of the total mass of all raw materials in the preparation process of the organosilicon-modified polyetheramine.
[0034] Beneficial effects:
[0035] (1) The epoxy composite material prepared by the present invention is designed and synthesized by lignin-modified epoxy resin, and the active groups of lignin are introduced, and the excellent charring performance of the lignin-modified epoxy resin is utilized to improve the flame retardant and smoke suppression performance of the epoxy composite material.
[0036] (2) The epoxy composite material prepared by the present invention introduces a flexible siloxane chain through the design and synthesis of organosilicon-modified polyetheramine, and utilizes the SiO2 generated on the surface during its combustion to improve the flame retardant and smoke suppression properties of the epoxy composite material.
[0037] (3) The epoxy composite material prepared by the present invention constructs a cross-linked network structure with good compatibility through the good synergistic effect of lignin and silicone, and simultaneously achieves the maximum improvement of the flame retardant and smoke suppression properties of the epoxy composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 The present invention is a flow chart of the preparation method of low-density flame-retardant and smoke-suppressing epoxy composite materials. DETAILED DESCRIPTION
[0039] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific implementation modes of the present invention are described in detail below with reference to the accompanying drawings, but they should not be construed as limiting the applicable scope of the present invention.
[0040] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the background technology and provide an epoxy composite material with improved flame retardancy and smoke suppression and a preparation method thereof.
[0041] The low-density flame-retardant and smoke-suppressing epoxy composite material comprises a resin component A and a curing agent component B, wherein the component A comprises the following components in the following parts by weight:
[0042]
[0043] The B component includes the following components in parts by weight:
[0044] 10-40 parts of silicone modified polyetheramine;
[0045] 1 to 10 parts of defoaming agent.
[0046] Optionally, the mass ratio of the component A to the component B is (10:1) to (1:1).
[0047] Optionally, the lignin-modified epoxy resin is prepared by a substitution reaction of lignin phenolic hydroxyl active groups with an epoxy resin, the lignin is selected from one or more of cellulose, hemicellulose, S-lignin, G-lignin and H-lignin, and the epoxy resin is selected from one or more of bisphenol A epoxy resin, halogenated bisphenol A epoxy resin, bisphenol S epoxy resin, bisphenol F epoxy resin, glycerol epoxy resin, ethylene glycol epoxy resin, phenolic epoxy resin and amino epoxy resin.
[0048] Optionally, the organosilicon-modified polyetheramine is prepared by a chemical reaction of a hydrogen-containing polysiloxane silicon hydrogen group and a polyetheramine, the hydrogen-containing polysiloxane polymer corresponding to the hydrogen-containing polysiloxane silicon hydrogen group is selected from one or more of a linear hydrogen-containing polysiloxane, a cyclic hydrogen-containing polysiloxane, a cross-linked hydrogen-containing polysiloxane, and a modified hydrogen-containing polysiloxane, and the polyetheramine is selected from one or more of a monofunctional polyetheramine, a difunctional polyetheramine, and a trifunctional polyetheramine.
[0049] Optionally, the diluent is an alicyclic reactive diluent;
[0050] The reinforcing filler is carbon black, and its particle size is 20um-40um;
[0051] The dispersant is carbon black, and its particle size is 1nm-100nm;
[0052] The defoamer is selected from one or more of an organic silicon defoamer, a polyoxyethylene defoamer and an inorganic defoamer.
[0053] See also Figure 1 The preparation method of the low-density flame-retardant and smoke-suppressing epoxy composite material comprises the following steps:
[0054] The component A and the component B are mixed and stirred to obtain an epoxy composite material.
[0055] Optionally, the A component is prepared by the following method:
[0056] 10 to 20 parts by weight of a diluent are added to 20 to 100 parts by weight of the lignin-modified epoxy resin, and then 1 to 10 parts by weight of the dispersant and 10 to 50 parts by weight of the reinforcing filler are added, and then the mixture is put into a planetary mixer for high-speed dispersion for 30 to 50 minutes at a rotation speed of 2000 rpm to 4000 rpm.
[0057] Optionally, the lignin-modified epoxy resin is prepared by the following method:
[0058] (1) Add 20-80 parts by weight of lignin and the first solvent into a four-necked round-bottom flask, heat to 100-200° C., mechanically stir for 1-5 hours to mix evenly, and filter;
[0059] (2) adding 10-100 parts by weight of epoxy resin to the mixture, mixing evenly, and then dropping 0.1-1 parts by weight of the first catalyst, reacting for 4-8 hours, then cooling to 25° C., performing reduced pressure distillation, and removing the solvent;
[0060] (3) Finally, centrifugation is performed to obtain a brown-black viscous liquid, which is the lignin-modified epoxy resin.
[0061] The first solvent is selected from one or more of toluene, xylene, n-butanol, cyclohexane, and heptane; the first catalyst is an organic base catalyst, selected from one or more combinations of sodium methoxide, sodium ethoxide, sodium isopropoxide, and sodium phthalate; and the amount of the first catalyst added is 0.05%-1% of the total mass of all raw materials in the preparation process of the lignin-modified epoxy resin.
[0062] Optionally, the B component is prepared by the following method: 10 to 40 parts by weight of the organosilicon-modified polyetheramine and 1 to 10 parts by weight of a defoamer are added to a stirring kettle and stirred for 10 to 30 minutes at a rotation speed of 50 rpm to 120 rpm.
[0063] Optionally, the organosilicon-modified polyetheramine is prepared by the following method:
[0064] (1) Add 10-100 parts by weight of polyetheramine and a second solvent into a three-necked flask, heat to 100-200° C., and mechanically stir for 1-5 hours to mix evenly;
[0065] (2) slowly dropwise adding 10-100 parts by weight of hydrogen-containing polysiloxane, mixing evenly, dropwise adding 0.1-1 parts by weight of the second catalyst, reacting for 4-8 hours, then cooling to 25° C., performing reduced pressure distillation to remove the solvent;
[0066] (3) Finally, centrifugation is performed to obtain a yellow viscous liquid, which is the siloxane-modified curing agent.
[0067] The second solvent is selected from one or more of toluene, xylene, n-butanol, cyclohexane, and heptane; the second catalyst is an organic base catalyst selected from one or more of sodium methoxide, sodium ethoxide, sodium isopropoxide, and sodium phthalate; and the amount of the second catalyst added is 0.05%-1% of the total mass of all raw materials in the preparation process of the organosilicon-modified polyetheramine.
[0068] In one embodiment, a method for preparing a low-density flame-retardant and smoke-suppressing epoxy composite material comprises the following steps:
[0069] 1) preparing component A: adding 10 to 20 parts by weight of alicyclic reactive diluent to 20 to 100 parts by weight of lignin modified epoxy resin, and then adding 1 to 10 parts by weight of dispersant and 10 to 50 parts by weight of reinforcing filler, and then putting into a planetary mixer for high-speed dispersion for 30 to 50 minutes at a speed of 2000 rpm to 4000 rpm;
[0070] 2) Preparation of component B: 10 to 40 parts by weight of organosilicon-modified polyetheramine and 1 to 10 parts by weight of defoamer are added to a stirring kettle and stirred for 10 to 30 minutes at a speed of 50 rpm to 120 rpm;
[0071] 3) Component A and component B are mixed and stirred in a weight ratio of (10:1) to (1:1) to obtain an epoxy composite material.
[0072] The preparation method of the lignin modified epoxy resin synthesis steps mainly includes (1) adding 20-80g of lignin and a first solvent into a four-necked round-bottom flask, heating to 100-200°C, mechanically stirring for 1-5h to mix evenly, and then filtering to remove undissolved residues. (2) adding 10-100g of epoxy resin to the mixture, mixing evenly, and then dripping 0.1-1g of the first catalyst, reacting for 4-8h, then cooling to 25°C, performing reduced pressure distillation, and removing the solvent. Finally, centrifuging to obtain a brown-black viscous liquid, which is the lignin modified epoxy resin.
[0073] The method for synthesizing organosilicon-modified polyetheramine mainly comprises the following steps: (1) adding 10-100g of polyetheramine and a second solvent into a three-necked flask, heating to 100-200°C, and mechanically stirring for 1-5h to mix evenly. (2) slowly dropping 10-100g of hydrogen-containing polysiloxane, dropping 0.1-1g of a second catalyst after mixing evenly, reacting for 4-8h, then cooling to 25°C, performing reduced pressure distillation, and removing the solvent. Finally, centrifuging to obtain a yellow viscous liquid, which is the siloxane-modified curing agent.
[0074] Embodiment 1:
[0075] A low-density flame-retardant and smoke-suppressing epoxy composite material, prepared from 50g of component A and 5g of component B;
[0076] The component A comprises the following ingredients in parts by weight:
[0077] 80 parts of lignin modified epoxy resin;
[0078] 10 parts of diluent;
[0079] 3 parts of dispersant;
[0080] 20 parts of reinforcing filler;
[0081] The B component includes the following ingredients in parts by weight:
[0082] 30 parts of silicone modified polyetheramine;
[0083] 8 parts of defoaming agent;
[0084] The preparation method of the epoxy composite material comprises the following steps:
[0085] 1. Synthesize lignin modified epoxy resin, the steps mainly include (1) adding 60g of S-lignin and toluene into a four-necked round-bottom flask, heating to 130°C, mechanically stirring for 3h to mix evenly, and then filtering to remove undissolved residues. (2) adding 30g of bisphenol A epoxy resin to the mixture, mixing evenly, and then dropping 0.5g of sodium isopropoxide catalyst, reacting for 6h, then cooling to 25°C, performing reduced pressure distillation, and removing the solvent. Finally, centrifuging to obtain a brown-black viscous liquid, which is the lignin modified epoxy resin.
[0086] 2. Synthesize organosilicon-modified polyetheramine, the steps mainly include (1) adding 60g trifunctional polyetheramine and toluene into a three-necked flask, heating to 130°C, and mechanically stirring for 3h to mix evenly. (2) slowly adding 12g cross-linked hydrogen-containing polysiloxane, adding 0.5g sodium isopropoxide catalyst after mixing evenly, reacting for 6h, then cooling to 25°C, performing vacuum distillation, and removing the solvent. Finally, centrifuging to obtain a yellow viscous liquid, which is the siloxane-modified curing agent.
[0087] 3. Prepare component A: add 10 parts of alicyclic reactive diluent to 80 parts of lignin-modified epoxy resin, then add 3 parts of dispersant and 20 parts of reinforcing filler, and then put it into a planetary mixer for high-speed dispersion for 30 minutes at a speed of 2500 rpm;
[0088] 4. Preparation of component B: Add 30 parts of organosilicon-modified polyetheramine and 8 parts of defoamer into a stirring kettle and stir for 30 minutes at a speed of 80 rpm;
[0089] 5. Accurately weigh 50 g of the above component A and 5 g of the above component B, mix and stir for 6 minutes to obtain an epoxy composite material.
[0090] 6. The performance of the obtained epoxy structural adhesive was tested, and the results are shown in Table 1.
[0091] Embodiment 2:
[0092] A low-density flame-retardant and smoke-suppressing epoxy composite material, prepared from 30g of component A and 6g of component B;
[0093] The component A comprises the following ingredients in parts by weight:
[0094] 50 parts of lignin modified epoxy resin;
[0095] 15 parts of diluent;
[0096] 5 parts of dispersant;
[0097] 30 parts of reinforcing filler;
[0098] The B component includes the following ingredients in parts by weight:
[0099] 20 parts of silicone modified polyetheramine;
[0100] 6 parts of defoaming agent;
[0101] The preparation method of the epoxy composite material comprises the following steps:
[0102] 1. Synthesize lignin modified epoxy resin, the steps mainly include (1) adding 80g of G-lignin and xylene into a four-necked round-bottom flask, heating to 140°C, mechanically stirring for 4h to mix evenly, and then filtering to remove undissolved residues. (2) adding 40g of bisphenol S epoxy resin to the mixture, mixing evenly, and then dropping 0.2g of sodium methoxide catalyst, reacting for 7h, then cooling to 25°C, performing reduced pressure distillation, and removing the solvent. Finally, centrifuging to obtain a brown-black viscous liquid, which is the lignin modified epoxy resin.
[0103] 2. Synthesize organosilicon-modified polyetheramine, the steps mainly include (1) adding 75g of bifunctional polyetheramine and xylene into a three-necked flask, heating to 140°C, and mechanically stirring for 4h to mix evenly. (2) slowly adding 15g of cyclic hydrogen-containing polysiloxane, adding 0.2g of sodium methoxide catalyst after mixing evenly, reacting for 7h, then cooling to 25°C, performing vacuum distillation, and removing the solvent. Finally, centrifuging to obtain a yellow viscous liquid, which is the siloxane-modified curing agent.
[0104] 3. Prepare component A: add 15 parts of alicyclic reactive diluent to 50 parts of lignin-modified epoxy resin, then add 5 parts of dispersant and 30 parts of reinforcing filler, and then put it into a planetary mixer for high-speed dispersion for 35 minutes at a speed of 2000 rpm;
[0105] 4. Preparation of component B: Add 20 parts of organosilicon-modified polyetheramine and 6 parts of defoamer into a stirring kettle and stir for 30 minutes at a speed of 60 rpm;
[0106] 5. Accurately weigh 30g of the above component A and 6g of the above component B, mix and stir for 6 minutes to obtain an epoxy composite material. 6. Test the properties of the obtained epoxy structural adhesive, and the results are shown in Table 1.
[0107] Embodiment 3:
[0108] A low-density flame-retardant and smoke-suppressing epoxy composite material, prepared from 20g of component A and 10g of component B;
[0109] The component A comprises the following ingredients in parts by weight:
[0110] 60 parts of lignin modified epoxy resin;
[0111] 12 parts of diluent;
[0112] 6 parts of dispersant;
[0113] 35 parts of reinforcing filler;
[0114] The B component includes the following ingredients in parts by weight:
[0115] 40 parts of silicone modified polyetheramine;
[0116] 3 parts of defoaming agent;
[0117] The preparation method of the epoxy composite material comprises the following steps:
[0118] 1. Synthesize lignin modified epoxy resin, the steps mainly include (1) adding 70g H-lignin and n-butanol into a four-necked round-bottom flask, heating to 150°C, mechanically stirring for 5h to mix evenly, and then filtering to remove undissolved residues. (2) adding 35g bisphenol S epoxy resin to the mixture, mixing evenly, and then dropping 0.3g sodium ethoxide catalyst, reacting for 8h, then cooling to 25°C, performing reduced pressure distillation, and removing the solvent. Finally, centrifuging to obtain a brown-black viscous liquid, which is the lignin modified epoxy resin.
[0119] 2. Synthesize organosilicon-modified polyetheramine, the steps mainly include (1) adding 100g of monofunctional polyetheramine and n-butanol into a three-necked flask, heating to 50°C, and mechanically stirring for 5h to mix evenly. (2) slowly adding 20g of linear hydrogen-containing polysiloxane, adding 0.3g of sodium ethoxide catalyst after mixing evenly, reacting for 8h, then cooling to 25°C, performing vacuum distillation, and removing the solvent. Finally, centrifuging to obtain a yellow viscous liquid, which is the siloxane-modified curing agent.
[0120] 3. Prepare component A: add 12 parts of alicyclic reactive diluent to 60 parts of lignin-modified epoxy resin, then add 6 parts of dispersant and 30 parts of reinforcing filler, and then put it into a planetary mixer for high-speed dispersion for 45 minutes at a speed of 3000 rpm;
[0121] 4. Preparation of component B: Add 40 parts of organosilicon-modified polyetheramine and 3 parts of defoamer into a stirring kettle and stir for 30 minutes at a speed of 80 rpm;
[0122] 5. Accurately weigh 20 g of the above component A and 10 g of the above component B, mix and stir for 6 minutes to obtain an epoxy composite material.
[0123] 6. The performance of the obtained epoxy structural adhesive was tested, and the results are shown in Table 1.
[0124] Blank sample:
[0125] A common epoxy composite material is prepared from 30g of component A and 10g of component B;
[0126] The component A comprises the following ingredients in parts by weight:
[0127] 60 parts of bisphenol F epoxy resin;
[0128] 10 parts of diluent;
[0129] 2 parts of dispersant;
[0130] 50 parts of reinforcing filler;
[0131] The B component includes the following ingredients in parts by weight:
[0132] 40 parts of monofunctional polyetheramine;
[0133] 3 parts of defoaming agent;
[0134] The preparation method of the epoxy composite material comprises the following steps:
[0135] 1) Preparation of component A: Add 10 parts of alicyclic reactive diluent to 60 parts of bisphenol F epoxy resin, then add 2 parts of dispersant and 50 parts of reinforcing filler, and then put into a planetary mixer for high-speed dispersion for 50 minutes at a speed of 3500 rpm;
[0136] 2) Preparation of component B: 40 parts of monofunctional polyetheramine and 3 parts of defoamer were added into a stirring kettle and stirred for 25 minutes at a speed of 70 rpm;
[0137] 3) Accurately weigh 30 g of the above component A and 10 g of the above component B, mix and stir for 8 minutes to obtain an epoxy composite material.
[0138] 4) The performance of the obtained epoxy structural adhesive was tested, and the results are shown in Table 1.
[0139] Related performance test analysis:
[0140] Test conditions:
[0141] The glass transition temperature of the epoxy composite was obtained using a dynamic thermomechanical analyzer. The test mode was a double cantilever mode, and the temperature was increased from 30°C to 270°C at a heating rate of 5°C / min in a nitrogen atmosphere.
[0142] The viscosity was tested using a rheometer.
[0143] The gel time of the epoxy composite was obtained using a differential scanning calorimeter. In a nitrogen atmosphere, the temperature was raised to 300°C at 10°C / min, then lowered to 25°C at 10°C / min, and then raised to 300°C at 10°C / min.
[0144] The limiting oxygen index (LOI) value was measured using an HC-2C oxygen index meter (Beijing Yaode Instrument Technology Co., Ltd., China) according to ASTM D2863-97.
[0145] The burning behavior of the samples was measured by cone calorimetry (Fire Testing Technologies, UK) according to the ISO 5660 test standard.
[0146] The smoke density of the composites was measured using a smoke chamber (Shanghai Chengwei Instrument Technology Co., Ltd., China) according to ASTM D 2843-99.
[0147] The performance of the bottom filling material prepared in this embodiment was tested and compared, and the results are shown in Table 1.
[0148] Table 1 Performance influence test results of epoxy composite materials prepared in various embodiments
[0149]
[0150] It can be seen from the experimental data in Table 1 that the Tg of the epoxy composite material prepared by the present invention reaches above 127°C, and the gel time is less than 10min, which meets its application requirements. At the same time, its limiting oxygen index (LOI) value is significantly lower than that of the blank sample; the average heat release rate (AHRR), peak HRR (pHRR), mass change parameter (MLR), maximum smoke density (D s,max ) and other characteristic parameters are significantly lower than those of the blank sample, proving that the introduction of lignin and siloxane chains effectively improves the flame retardant and smoke suppression properties of epoxy composites.
[0151] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A low-density flame-retardant and smoke-suppressing epoxy composite material, characterized in that: It comprises a resin component A and a curing agent component B, wherein the component A comprises the following components in parts by weight: The B component includes the following components in parts by weight: 10-40 parts of silicone modified polyetheramine; 1 to 10 parts of defoaming agent.
2. The low-density flame-retardant and smoke-suppressing epoxy composite material according to claim 1, characterized in that: The mass ratio of the component A to the component B is (10:1) to (1:1).
3. The low-density flame-retardant and smoke-suppressing epoxy composite material according to claim 1, characterized in that: The lignin-modified epoxy resin is prepared by a substitution reaction between a lignin phenolic hydroxyl active group and an epoxy resin, wherein the lignin is selected from one or more of cellulose, hemicellulose, S-lignin, G-lignin and H-lignin, and the epoxy resin is selected from one or more of bisphenol A epoxy resin, halogenated bisphenol A epoxy resin, bisphenol S epoxy resin, bisphenol F epoxy resin, glycerol epoxy resin, ethylene glycol epoxy resin, phenolic epoxy resin and amino epoxy resin.
4. The low-density flame-retardant and smoke-suppressing epoxy composite material according to claim 1, characterized in that: The organosilicon-modified polyetheramine is prepared by chemical reaction of hydrogen-containing polysiloxane silicon hydrogen groups and polyetheramine, the hydrogen-containing polysiloxane polymer corresponding to the hydrogen-containing polysiloxane silicon hydrogen groups is selected from one or more of linear hydrogen-containing polysiloxane, cyclic hydrogen-containing polysiloxane, cross-linked hydrogen-containing polysiloxane, and modified hydrogen-containing polysiloxane, and the polyetheramine is selected from one or more of monofunctional polyetheramine, difunctional polyetheramine, and trifunctional polyetheramine.
5. The low-density flame-retardant and smoke-suppressing epoxy composite material according to claim 1, characterized in that: The diluent is an alicyclic reactive diluent; The reinforcing filler is carbon black, and its particle size is 20um-40um; The dispersant is carbon black, and its particle size is 1nm-100nm; The defoamer is selected from one or more of an organic silicon defoamer, a polyoxyethylene defoamer, and an inorganic defoamer.
6. A method for preparing a low-density flame-retardant and smoke-suppressing epoxy composite material according to any one of claims 1 to 5, characterized in that: The following steps are involved: The component A and the component B are mixed and stirred to obtain an epoxy composite material.
7. The method for preparing the low-density flame-retardant and smoke-suppressing epoxy composite material according to claim 6, characterized in that: The A component is prepared by the following method: 10 to 20 parts by weight of a diluent are added to 20 to 100 parts by weight of the lignin-modified epoxy resin, and then 1 to 10 parts by weight of the dispersant and 10 to 50 parts by weight of the reinforcing filler are added, and then the mixture is put into a planetary mixer for high-speed dispersion for 30 to 50 minutes at a rotation speed of 2000 rpm to 4000 rpm.
8. The method for preparing the low-density flame-retardant and smoke-suppressing epoxy composite material according to claim 7, characterized in that: The lignin modified epoxy resin is prepared by the following method: (1) Add 20-80 parts by weight of lignin and the first solvent into a four-necked round-bottom flask, heat to 100-200° C., mechanically stir for 1-5 hours to mix evenly, and filter; (2) adding 10-100 parts by weight of epoxy resin to the mixture, mixing evenly, and then dropping 0.1-1 parts by weight of the first catalyst, reacting for 4-8 hours, then cooling to 25° C., performing reduced pressure distillation, and removing the solvent; (3) Finally, centrifugation is performed to obtain a brown-black viscous liquid, which is the lignin-modified epoxy resin. The first solvent is selected from one or more of toluene, xylene, n-butanol, cyclohexane, and heptane; the first catalyst is an organic base catalyst, selected from one or more combinations of sodium methoxide, sodium ethoxide, sodium isopropoxide, and sodium phthalate; and the amount of the first catalyst added is 0.05%-1% of the total mass of all raw materials in the preparation process of the lignin-modified epoxy resin.
9. The method for preparing the low-density flame-retardant and smoke-suppressing epoxy composite material according to claim 6, characterized in that: The B component is prepared by the following method: 10 to 40 parts by weight of the organosilicon-modified polyetheramine and 1 to 10 parts by weight of a defoamer are added into a stirring kettle and stirred for 10 to 30 minutes at a rotation speed of 50 rpm to 120 rpm.
10. The method for preparing the low-density flame-retardant and smoke-suppressing epoxy composite material according to claim 9, characterized in that: The organosilicon-modified polyetheramine is prepared by the following method: (1) Add 10-100 parts by weight of polyetheramine and a second solvent into a three-necked flask, heat to 100-200° C., and mechanically stir for 1-5 hours to mix evenly; (2) slowly dropwise adding 10-100 parts by weight of hydrogen-containing polysiloxane, mixing evenly, dropwise adding 0.1-1 parts by weight of the second catalyst, reacting for 4-8 hours, then cooling to 25° C., performing reduced pressure distillation to remove the solvent; (3) Finally, centrifugation is performed to obtain a yellow viscous liquid, which is the siloxane-modified curing agent. The second solvent is selected from one or more of toluene, xylene, n-butanol, cyclohexane, and heptane; the second catalyst is an organic base catalyst selected from one or more of sodium methoxide, sodium ethoxide, sodium isopropoxide, and sodium phthalate; and the added amount of the catalyst is 0.05%-1% of the total mass of all raw materials in the preparation process of the organosilicon-modified polyetheramine.
Citation Information
Patent Citations
Lignin-epoxy resin composite material and preparation method thereof
CN102585531A
Modified epoxy thin-layer adhesive used for bridge road pavement and preparation technology thereof
CN106995672A
Organosilicon modified epoxy resin water-based curing agent and preparation method thereof
CN108250411A
Flame-retardant epoxy resin floor coating and preparation method thereof
CN114350232A
High-temperature-resistant epoxy pouring sealant as well as preparation method and application thereof
CN118048121A