Technology for controlling silicon and removing iron through oxygen-sulfur synergistic leaching in wet smelting
By separating the leaching process of roasted ore and oxidized ore in hydrosmelting, controlling the temperature and pH value, and reducing the soluble silicon content of roasted ore, the problem of difficult filtration of high-temperature and high-acid leaching slurry of roasted ore is solved, and the zinc leaching rate is improved. and iron removal efficiency, achieving higher leaching rates and lower steam consumption.
Patent Information
- Application Number
- CN202410952727.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-01
AI Technical Summary
The high temperature and high acid leaching slurry of roasted ore in hydrometallurgy is difficult to filter, resulting in low zinc leaching rate, inability to produce lead and silver slag, low iron removal process efficiency and high cost, mainly due to the high soluble silicon content and zinc sulfide in roasted ore The silicate generated by roasting SiO2 in the concentrate forms silica gel under acidic conditions, which affects filtration.
The oxygen-sulfur synergistic leaching silicon-controlled iron removal process in hydrometallurgy is adopted. By separating the leaching processes of roasted ore and oxidized ore, the temperature and pH value of different processes are controlled, and flocculants and electrolytic waste liquid are used to adjust the leaching conditions to reduce the loss of roasted ore. Soluble silicon content, separates the leaching residue of roasted ore and oxidized ore, reduces steam consumption and improves the leaching rate of zinc.
It effectively solves the problem of silica gel formation, improves the zinc leaching rate and iron removal efficiency, reduces the difficulty of filtering the high-acid leaching residue of roasted ore, reduces steam consumption, and makes the high-acid leaching residue of roasted ore contain salable Pb and Ag. , improving the efficiency and economy of the iron removal process.
Smart Images

Figure CN118726748A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrometallurgy, and in particular relates to a process for oxygen-sulfur coordinated leaching and silicon-controlled iron removal in hydrometallurgy. Background Art
[0002] In recent years, with the gradual depletion of high-grade zinc oxide ores in mines, raw materials can no longer meet production needs, and the mismatch between technology and raw materials has become increasingly prominent year by year.
[0003] Due to the mismatch between process and raw materials, the metal content of roasted sand dust and zinc oxide ore changed from 3:7 in the initial design to the current 7:3; at the same time, the iron content of roasted sand dust increased from 5.42% in 2019 to 8.48% in 2021. In order to meet the needs of the oxidation hydrolysis iron removal process, the ratio of zinc oxide ore and roasted sand dust raw materials increased year by year, from 2.8 in 2019 and 3.1 in 2020 to 3.98 in 2021. Due to the increase in the ratio, the equipment processing capacity was limited, resulting in the smelter's scale benefits unable to be exerted, the market competitiveness was extremely weak, and the smelting was in a loss-making situation. Over the years, smelters have adopted the oxidation hydrolysis iron removal process, which requires oxidizing ferrous iron to ferric iron and then controlling the endpoint pH value of the slurry to hydrolyze the ferric iron and wrap the leaching slag, and quickly separate it from the solution; its operation process must meet the ratio of zinc oxide ore to roasted sand dust of 2.8-3.2 to meet the rapid iron removal needs in production; in 2022, Jinding Zinc Industry Smelter plans to have a production capacity of 82,000 tons, of which 102,300 tons of self-produced and purchased roasted sand; it plans to consume 234,000 tons of zinc oxide ore, and its ratio is only 2.29, which cannot meet all the hydrolysis iron removal needs; it is urgent to adopt new iron removal methods.
[0004] At the same time, the silicon content in zinc oxide ore has remained high. The silicon dioxide content in roasted ore has increased from 2-4% in previous years to 6.5-7.8% in 2022. The silicon content in the solution has increased, and the difficulty of operating the leaching process has increased. To ensure that silica gel is not formed in the solution, the pH value is controlled at a high level during the entire leaching process. It is difficult to ensure neutral leaching of roasted ore and raw ore. A large amount of zinc metal and impurity elements in the roasted ore are leached from the high-temperature and high-acid leaching section of the roasted ore, and a large amount of zinc metal in the raw ore is leached by the second-stage acid leaching, which not only increases the difficulty of filtration, but also increases the pressure of alkaline zinc precipitation. How to improve the leaching rate of intermediate leaching, the primary issue is to prevent the formation of silica gel and the reduction of silicon in the solution.
[0005] like Figure 1As shown in the figure, the current wet process flow chart of the smelter of the smelter, the process roasting ore only goes through two stages of leaching (neutral leaching-high temperature high acid leaching), the high leaching slag contains 10% zinc, the zinc recovery rate of the whole plant is low, and a rough statistical analysis of this item alone shows that the loss of Zn metal reaches 1500t / a~2000t / a. The second problem of this process is that the roasting high temperature high acid leaching slurry cannot be filtered, and the high temperature high acid leaching slurry is finally mixed with the oxide ore slurry and filtered together, and no valuable lead and silver slag can be obtained; at the same time, the high temperature high acid leaching slurry contains up to 10g / L of iron, there is no independent iron removal process, and it relies on the neutralization of zinc oxide ore to remove iron. This iron removal method is inefficient and has an adverse effect on subsequent processes. At present, the iron removal oxidant uses hydrogen peroxide, potassium permanganate, and manganese powder. The cost of zinc oxidant per ton is 130 yuan, and the manganese ion concentration in the system is as high as 20g / l.
[0006] In summary, the main problems of this process are: 1) low zinc leaching rate; 2) lead and silver slag cannot be produced; 3) low iron removal efficiency and high cost. After in-depth analysis of these problems, the ultimate source is that the high-temperature and high-acid leaching slurry of roasting cannot be filtered. The difficulty in filtering the high-temperature and high-acid leaching slurry of roasting is mainly due to the high soluble silicon content of roasting. The zinc sulfide concentrate provided by the mine contains a certain amount of SiO2, which cannot react under acidic conditions and is called "insoluble silicon". However, when the zinc sulfide concentrate is roasted into zinc roasted ore through a boiling furnace, SiO2 will be roasted to varying degrees into silicates such as ZnSiO3 and PbSiO3. This type of silicate is very easy to leach (generally, it can react when the pH value is lower than 3.0) to generate silicic acid, which forms silica gel under acidic conditions, thus affecting filtration. The silicate in roasted ore is called "soluble silicon", and its content is closely related to the silicon content of zinc sulfide concentrate and the roasting temperature of the fluidized bed furnace. Generally speaking, the higher the silicon content of zinc sulfide concentrate and the roasting temperature of the fluidized bed furnace, the higher the soluble silicon in the roasted ore, and the more difficult it is to filter the subsequent acid leaching slurry of the roasted ore.
[0007] Controlling the soluble silicon content of roasted ore can fundamentally solve the problem of difficulty in filtering roasted acid leaching slurry. However, in actual production, due to reasons such as raw materials, equipment, and operation, it is difficult to reduce the soluble silicon content of roasted ore to 0 100%. Therefore, the problem of silica gel needs to be solved in the leaching process.
[0008] In order to solve this problem, there are several ways in the prior art: 1. One is the practice of China Nonferrous Zinc Industry, which controls the soluble silicon content of roasted ore to less than 2.5%, and uses iron alum to adsorb silica gel to form filterable alum slag during the leaching process; but there are also disadvantages: 1) The amount of high leaching slag is large, and the lead and silver enrichment ratios are low, and subsequent ore dressing is required to reflect the value; 2) The steam consumption is large. It is understood that the process consumes 1.3 tons of steam per ton of zinc in summer and 1.7 tons in winter (excluding steam produced by the boiling furnace, and including heating steam in winter); 2. Another approach is the approach of Baiyin Nonferrous Northwest Lead and Zinc Smelter, which controls the pH of the intermediate leaching tank No. 1: 1.5-2.0 (close to 1.5) and the pH of the intermediate leaching tank No. 3: 4.5; but precise control of pH can only alleviate the impact of silicon on the system to a certain extent. The principle is the same as the first approach, and the silica gel will dissolve again as the iron slag is leached.
[0009] The above methods can only alleviate the impact of silicon on the system to a certain extent. To solve the problem substantially, we must find ways to reduce the soluble silicon content in the roasted sand, thereby further improving the iron removal efficiency.
[0010] Therefore, this paper proposes a process of oxygen-sulfur synergistic leaching to control silicon and remove iron in hydrometallurgy. Summary of the invention
[0011] In order to solve the above technical problems, the present invention provides a process for oxygen-sulfur coordinated leaching and silicon-controlled iron removal in hydrometallurgy, which reduces the soluble silicon content in roasted sand, thereby further improving the iron removal efficiency and zinc leaching rate.
[0012] In order to achieve the above technical effects, the present invention is implemented by the following technical scheme: a process for oxygen-sulfur coordinated leaching and silicon-controlled iron removal in hydrometallurgy, specifically comprising the following steps: S1, roasted ore leaching: take the middle supernatant as the bottom flow, first add roasted ore, then add roasted ore low acid supernatant, oxidized ore low acid supernatant, hydrolyzed liquid, electrolytic waste liquid respectively, the process pH value is 3.0-4.0, the end pH value is 4.5 (considering that roasted ore has no copper and Ss is high, the pH is appropriately high, which is conducive to hydrolysis and iron removal), the reaction time is 2h, the reaction temperature is 70℃; 800g roasted ore is added in each cycle, the reaction is completed, flocculant is added for flocculation and sedimentation, the supernatant is poured out, and the bottom flow is used for weak acid leaching-low acid leaching; Furthermore, the post-hydrolysis liquid in S1 includes post-iron precipitation liquid and post-iron precipitation slag pickling liquid.
[0013] S2, the bottom flow in S1 is subjected to weak acid leaching and low acid leaching in turn: the reaction temperature of weak acid leaching (mainly to solve the problem of silicon affecting filtration) is 80°C, the reaction time is 2h, the pH value is adjusted with electrolytic waste liquid, and electrolytic waste liquid is directly added for low acid leaching after the reaction is completed. After leaching, the low leaching pulp is flocculated and settled, the bottom flow is filtered, the roasted ore low acid supernatant and filtrate are returned to the roasted ore for leaching, and the filter residue is subjected to hot acid leaching; Furthermore, during the low-acid leaching in S2, the waste heat of weak acid leaching can be used for heating without further heating, the temperature is 70° C., and the reaction time is 0.5 hours.
[0014] S3, hot acid leaching is performed on the filter residue in S2 to obtain hot acid residue and hot acid supernatant, and then the hot acid residue is subjected to high acid leaching to obtain high acid supernatant and high leaching residue, and the hot acid supernatant is used as the pre-iron removal liquid; in this step, the roasting hot acid leaching and high acid leaching are mainly to destroy ZnO•Fe 2 O 3 , improve the zinc leaching rate, and obtain the iron removal pre-liquid; Furthermore, the high-acid leaching pre-liquid in S2 is electrolytic waste liquid, and the high-acid supernatant is used as the hot acid leaching pre-liquid, and the reaction temperatures of hot acid leaching and high-acid leaching are both 80°C, the reaction time is both 3h, the slurry is flocculated and settled, and the bottom flow is filtered. When the high-acid leaching residue is quickly filtered and dried, 200ml of hot water is added to the funnel for infiltration and washing; wherein, the high-acid leaching residue can be used for external sale.
[0015] S4, hydrolyzing and removing iron from the hot acid supernatant in S3: hydrolyzing and removing iron by using oxide ore as a neutralizing agent, and precipitating iron by jarosite method to obtain iron precipitated slag and iron precipitated liquid, and adding sulfuric acid to the iron precipitated slag to obtain storable iron slag and pickling liquid; or using zinc precipitated slag as a hydrolysis neutralizing agent, and using the para-goethite method to precipitate iron; Furthermore, when the oxide ore is used as the neutralizing agent in S4, in order to ensure the iron precipitation rate and filtration performance during the hydrolysis iron precipitation process, the end point pH value is close to 4.5, and a large amount of ZnCO 3 It cannot participate in the reaction and needs further pickling to increase the metal leaching rate. The liquid-to-solid ratio is 2.6:1, the temperature is 80℃, the time is 2h, and the pH value is adjusted with sulfuric acid solution. The end point pH value is 2.5.
[0016] Furthermore, when zinc precipitation slag is used as a neutralizing agent in S4, air can be used as an oxidant under the condition of pH 4.0-5.0 (this method can increase the iron precipitation rate, reduce steam consumption, and reduce the amount of oxidant used).
[0017] S5, leaching of oxide ore: first add electrolytic waste liquid weak acid leaching, then add electrolytic waste liquid low acid leaching, obtain oxide ore low acid supernatant and low leaching residue, then wash the oxide ore low leaching residue with water, the washing liquid-solid ratio is 2:1, stir for 1h, temperature 70 o C. Finally, high silicon slag and water-washed liquid are obtained. The high silicon slag is stored and zinc is precipitated from the water-washed liquid.
[0018] The beneficial effects of the present invention are: This process can solve the problem of silicon affecting filtration. The roasted ore and oxidized ore are leached separately. Each process controls different temperatures according to the actual needs of leaching, reducing steam consumption and achieving a higher leaching rate. In addition, the roasted ore contains soluble silicon (ZnO•SiO2, PbO•SiO2), which will affect the filtration performance of the leached slag after leaching. Separate leaching can avoid mutual interference, reduce filtration pressure, reduce slag water content, and reduce slag washing pressure. The roasted ore high-leaching slag obtained by separate leaching contains a certain grade of Pb and Ag, which can be sold or further processed. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for describing the embodiments are briefly introduced below. Those skilled in the art can also obtain other drawings based on these drawings without creative work.
[0020] Figure 1 Flow chart of wet process in prior art; Figure 2 The process flow chart of leaching silicon controlled iron removal of the present invention; In the accompanying drawings, the components represented by the reference numerals are listed as follows: DETAILED DESCRIPTION
[0021] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention. Example 1
[0022] like Figure 2 As shown, in this embodiment, the inventors reduced the soluble silicon content in the roasted sand, thereby further improving the iron removal efficiency and zinc leaching rate; Therefore, a process for oxygen-sulfur coordinated leaching and silicon-controlled iron removal in hydrometallurgy is provided, which specifically comprises the following steps: S1, roasted ore leaching: take the middle supernatant as the bottom flow, first add roasted ore, then add roasted ore low acid supernatant, oxidized ore low acid supernatant, hydrolyzed liquid, electrolytic waste liquid respectively, the process pH value is 3.0-4.0, the end pH value is 4.5 (considering that roasted ore has no copper and Ss is high, the pH is appropriately high, which is conducive to hydrolysis and iron removal), the reaction time is 2h, the reaction temperature is 70℃; 800g roasted ore is added in each cycle, the reaction is completed, flocculant is added for flocculation and sedimentation, the supernatant is poured out, and the bottom flow is used for weak acid leaching-low acid leaching; The post-hydrolysis liquid in S1 includes post-iron precipitation liquid and post-iron precipitation slag pickling liquid.
[0023] S2, the bottom flow in S1 is subjected to weak acid leaching and low acid leaching in turn: the reaction temperature of weak acid leaching (mainly to solve the problem of silicon affecting filtration) is 80°C, the reaction time is 2h, the pH value is adjusted with electrolytic waste liquid, and electrolytic waste liquid is directly added for low acid leaching after the reaction is completed. After leaching, the low leaching pulp is flocculated and settled, the bottom flow is filtered, the roasted ore low acid supernatant and filtrate are returned to the roasted ore for leaching, and the filter residue is subjected to hot acid leaching; Among them, during the low-acid leaching of S2, the residual heat of weak acid leaching can be used for heating without further heating. The temperature is 70°C and the reaction time is 0.5 hours.
[0024] S3, hot acid leaching is performed on the filter residue in S2 to obtain hot acid residue and hot acid supernatant, and then the hot acid residue is subjected to high acid leaching to obtain high acid supernatant and high leaching residue, and the hot acid supernatant is used as the pre-iron removal liquid; in this step, the roasting hot acid leaching and high acid leaching are mainly to destroy ZnO•Fe 2 O 3 , improve the zinc leaching rate, and obtain the iron removal pre-liquid; Among them, the high-acid leaching pre-liquid in S2 is electrolytic waste liquid, and the high-acid supernatant is used as the hot acid leaching pre-liquid. The reaction temperatures of hot acid leaching and high-acid leaching are both 80°C, and the reaction time is 3h. The slurry is flocculated and settled, and the bottom flow is filtered. When the high-leaching residue is quickly filtered and dried, 200ml of hot water is added to the funnel for infiltration and washing; among them, the high-leaching residue can be used for external sale.
[0025] S4, hydrolyzing and removing iron from the hot acid supernatant in S3: hydrolyzing and removing iron by using oxide ore as a neutralizing agent, and precipitating iron by jarosite method to obtain iron precipitated slag and iron precipitated liquid, and adding sulfuric acid to the iron precipitated slag to obtain storable iron slag and pickling liquid; or using zinc precipitated slag as a hydrolysis neutralizing agent, and using the para-goethite method to precipitate iron; Among them, when oxide ore is used as a neutralizer in S4, in order to ensure the iron precipitation rate and filtration performance during the hydrolysis iron precipitation process, the end point pH value is close to 4.5, and a large amount of ZnCO 3 It cannot participate in the reaction and needs further pickling to increase the metal leaching rate. The liquid-to-solid ratio is 2.6:1, the temperature is 80℃, the time is 2h, and the pH value is adjusted with sulfuric acid solution. The end point pH value is 2.5.
[0026] Among them, when zinc precipitation slag is used as a neutralizer in S4, air can be used as an oxidant under the condition of pH 4.0-5.0 (this method can increase the iron precipitation rate, reduce steam consumption, and reduce the amount of oxidant used).
[0027] S5, leaching of oxide ore: first add electrolytic waste liquid weak acid leaching, then add electrolytic waste liquid low acid leaching, obtain oxide ore low acid supernatant and low leaching residue, then wash the oxide ore low leaching residue with water, the washing liquid-solid ratio is 2:1, stir for 1h, temperature 70 oC. Finally, high silicon slag and water-washed liquid are obtained. The high silicon slag is stored and zinc is precipitated from the water-washed liquid. Example 2
[0028] To verify the feasibility of the above process, the inventors also conducted the following experiments: 1. Experimental equipment and instruments 1.1 Experimental instruments 1) Leaching tank, effective volume 23L, 2 pieces; 2) Small panel frame, 2m2, 1 unit; 3) Vacuum pump, 2 pcs; 4) Filter bottle, volume 2L, 2 pieces; 5) 3L beakers, 10 pieces; 6) IKA automatic heating stirrer, 4 units; 7) Flotation machines, 2 units, handheld pH meters, 2 units.
[0029] 1.2 Experimental materials The chemical compositions of roasted ore, oxidized ore and electrolyte required for the experiment are shown in Tables 1 and 2 below.
[0030]
[0031]
[0032] Electrolytic wastewater contains H 2 SO 4 :168.02g / L,Zn 2+ :40.74 g / L.
[0033] 2. Experimental technical route like Figure 2 As shown, the main components of roasted ore are ZnO and ZnO•Fe 2 O 3 , and the composition of the oxide ore is ZnO (after the experiment, it was found that it is ZnCO 3 ), ZnO can be leached under weak acidic conditions, while ZnO•Fe 2 O 3 High temperature and high acid are required, so roasting and oxidized ore leaching are carried out separately, and different temperatures are set according to different leaching conditions to reduce system steam consumption. In addition, roasted ore contains soluble silicon (ZnO•SiO 2 、PbO•SiO 2 ), which will affect the filtration performance of the leached residue after leaching. Separate leaching can avoid mutual interference, reduce filtration pressure, reduce slag water content, and reduce slag washing pressure. The roasted ore high leaching residue obtained by separate leaching contains a certain grade of Pb and Ag, which can be sold or further processed.
[0034] 2.1. Roasting and leaching Take the middle supernatant as the bottom flow, first add roasted ore, then add roasted ore low acid supernatant, oxidized ore low acid supernatant, hydrolyzed liquid, electrolytic waste liquid, process pH value 3.0-4.0, end point pH value 4.5 (considering that roasted ore has no copper and Ss is high, the pH is appropriately high, which is conducive to hydrolysis and iron removal), reaction time 2h, reaction temperature 70 o C. 800g of roasted ore was added in each cycle. After the reaction was completed, flocculants were added to flocculate and settle. The supernatant was poured out and the bottom flow was used for weak acid leaching. Table 3 shows the composition of the supernatant.
[0035]
[0036] 2.2. Roasted ore weak acid leaching - low leaching Weak acid leaching is mainly used to solve the problem of silicon affecting filtration. The temperature is 80 o C, time 2h, use electrolytic waste liquid to adjust pH value, after the reaction is completed, add electrolytic waste liquid directly for low acid leaching, low acid leaching uses the residual heat of weak acid leaching without heating (temperature about 70 o C), reaction time 0.5 hours. The low-leaching slurry is flocculated and settled, the underflow is filtered, the supernatant and filtrate are returned to the roasted ore for leaching, and the filter residue is subjected to hot acid leaching. Table 4 shows the composition of the low-acid supernatant.
[0037]
[0038] 2.3. Hot acid leaching and high acid leaching of roasted ore Roasted ore hot acid leaching and high acid leaching are mainly used to destroy ZnO•Fe 2 O 3 , improve the leaching rate of zinc, and obtain the iron removal pre-liquid at the same time. The high acid leaching pre-liquid is the electrolytic waste liquid, and the high acid leaching post-liquid is the hot acid leaching pre-liquid. The reaction temperature is 80 o C, the reaction time is 3h, the slurry is flocculated and settled, and the bottom flow is filtered. When the high-leaching residue is quickly filtered and dried, 200ml of hot water is added to the funnel for filtration. Table 5 shows the composition of the hot acid supernatant and high-acid supernatant, Table 6 shows the composition of the roasted high-leaching residue, and Table 7 shows the leaching rate of each metal in the roasted ore.
[0039]
[0040]
[0041]
[0042] 2.4. Hydrolysis of iron - acid washing of hydrolysis slag Oxide ore is used as a neutralizer for hydrolysis of iron. Previously, it was believed that the composition of the oxide ore was ZnO, but it is actually ZnCO 3 , ZnCO 3Compared with ZnO, it is more difficult to react with acid, so the first three cycles were not successful, the iron removal rate was low, and the filtration was difficult. Only the fourth cycle was successful. Table 8 shows the composition of the hydrolysis liquid, Table 9 shows the composition of the hydrolysis slag, and Table 10 shows the leaching rate of each metal of the hydrolysis neutralizer.
[0043]
[0044]
[0045]
[0046] In order to ensure the iron precipitation rate and filtration performance during the hydrolysis iron precipitation process, the end point pH value is close to 4.5, and a large amount of ZnCO 3 Unable to participate in the reaction, further pickling is required to increase the metal leaching rate. Liquid-to-solid ratio 2.6:1, temperature 80 o C, time 2h, use sulfuric acid solution to adjust pH value, the end point pH value is 2.5. Table 11 shows the composition of hydrolysis slag washing liquid, Table 12 shows the composition of hydrolysis slag after pickling, Table 13 shows the leaching rate of each metal in hydrolysis slag pickling, and Table 14 shows the total leaching rate of each metal in hydrolysis neutralizer.
[0047]
[0048]
[0049]
[0050]
[0051] Common iron removal methods in the hydrometallurgical zinc smelting process include jarosite method, goethite method, para-goethite method (spray iron removal method), and hematite method. Considering that Jinding Zinc's raw materials do not have copper, indium, germanium and other by-products to be recovered, jarosite or para-goethite method can be used. The crystals generated by the jarosite method are MFe 3 (OH) 6 (SO 4 ) 2 (M is NH 4+ 、Na + , H 3 O + The crystals generated by the secondary goethite method are Fe 2 O 3 •H 2 O•nSO 3(n≤1), from the generated products, it can be seen that the jarosite method takes away more acid than the parathionite method, and the system needs to add more acid to maintain the acid balance of the system. In addition, the pH of the jarosite method is 1.0-3.0, which is in a slightly acidic condition. In order to increase the iron precipitation rate and ensure the filtration performance, the reaction temperature and reaction time are very high; while the parathionite method has a pH of 4.0-5.0, which is in a slightly neutral condition, the iron precipitation rate is faster, ferrous iron is easier to oxidize, and the slurry is easier to filter, and the reaction temperature and reaction time requirements are relatively low.
[0052] In this experiment, an oxide ore was selected as the neutralizer. At that time, it was mainly believed that the oxide ore was ZnO, but later it was found that it was ZnCO 3 , ZnCO 3 It needs to react under slightly acidic conditions, and the final iron slag as an iron precipitation neutralizer can only be yellow potassium iron alum slag. It is recommended to use zinc precipitation slag as a hydrolysis neutralizer and use the secondary goethite method to precipitate iron, increase the iron precipitation rate, reduce steam consumption, and reduce the amount of oxidant. Air can be used as an oxidant under pH 4.0-5.0.
[0053] 2.5. Oxide ore leaching The main component of oxide ore is ZnCO 3 , it can be leached under low acid conditions. In order to compare the filtration performance, cycles 1 and 3 are first leached with weak acid, then with low acid, and cycles 2 and 4 are directly leached with low acid. When filtering with a filter funnel, the speed of filtering the liquid on the surface of the slurry is not much different between the two, but the time spent on filtering the slurry dry in cycles 2 and 4 is 2.5 times that of cycles 1 and 3. Table 15 shows the leaching conditions and leachate composition of the oxide ore, Table 16 shows the composition of the leaching slag of the oxide ore, and Table 17 shows the leaching rate of each metal in the oxide ore.
[0054] The leaching residue of the oxide ore contains high water-soluble zinc. The leaching residue of the oxide ore is washed with water, the washing liquid-solid ratio is 2:1, stirred for 1 hour, and the temperature is 70 o C, Table 18 is the composition of the leached residue after washing with oxide ore, Table 19 is the composition of the leached residue after washing with oxide ore, Table 20 is the leaching rate of each metal after washing with oxide ore leached residue, and Table 21 is the total leaching rate of each metal in oxide ore. In order to further improve the zinc leaching rate, the final acid can be appropriately increased or the reaction time can be delayed.
[0055] According to the acid balance calculation, the sulfuric acid content of oxide ore is 0.19t / t ore. According to the Ca content of oxide ore, the sulfuric acid content is 0.212t / t ore. The sulfuric acid content per ton of zinc is 2.11t and 2.38t (100% pure sulfuric acid) respectively.
[0056]
[0057]
[0058]
[0059]
[0060]
[0061]
[0062]
[0063] 3. Experimental conclusion: Roasting must be subjected to enhanced leaching to destroy ZnO•Fe 2 O 3 , final acid 100-120g / l, high leaching residue zinc content can be reduced to 6%, zinc leaching rate reaches 98%. The main component of oxide ore is ZnCO 3 , which is not suitable as an iron precipitation neutralizing agent. Zinc precipitation slag can be used as an iron precipitation neutralizing agent. During leaching, the final acid is 5g / l. After the leached slag is washed with water, the zinc leaching rate can reach 89%. In order to further improve the zinc leaching rate, the final acid can be appropriately increased or the reaction time can be delayed. This process can solve the problem of silicon affecting filtration. Roasted ore and oxidized ore are leached separately. Different temperatures are controlled in each process according to the actual needs of leaching to reduce steam consumption and achieve a higher leaching rate.
[0064] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0065] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A process for removing iron from silicon by oxygen-sulfur synergistic leaching in hydrometallurgy, comprising the following steps: S1, roasted ore leaching: take the middle supernatant as the bottom flow, first add roasted ore, then add roasted ore low acid supernatant, oxidized ore low acid supernatant, hydrolyzed liquid, electrolytic waste liquid respectively, process pH value 3.0-4.0, end point pH value 4.5, reaction time 2h, reaction temperature 70℃; each cycle puts in 800g roasted ore, after the reaction is finished, add flocculant for flocculation and sedimentation, pour out the supernatant, and the bottom flow is used for weak acid leaching-low acid leaching; S2, the bottom flow in S1 is subjected to weak acid leaching and low acid leaching in sequence: the reaction temperature of weak acid leaching is 80°C, the reaction time is 2h, the pH value is adjusted with electrolytic waste liquid, and electrolytic waste liquid is directly added for low acid leaching after the reaction is completed. After leaching, the low leaching pulp is flocculated and settled, the bottom flow is filtered, the roasted ore low acid supernatant and the filtrate are returned to the roasted ore for leaching, and the filter residue is subjected to hot acid leaching; S3, hot acid leaching the filter residue in S2 to obtain hot acid residue and hot acid supernatant, then high acid leaching the leached hot acid residue to obtain high acid supernatant and high leaching residue, and the hot acid supernatant is used as the pre-iron removal liquid; S4, hydrolyzing and removing iron from the hot acid supernatant in S3: hydrolyzing and removing iron by using oxide ore as a neutralizing agent, and precipitating iron by jarosite method to obtain iron precipitated slag and iron precipitated liquid, and adding sulfuric acid to the iron precipitated slag to obtain storable iron slag and pickling liquid; or using zinc precipitated slag as a hydrolysis neutralizing agent, and using the para-goethite method to precipitate iron; S5, leaching of oxide ore: first add electrolytic waste liquid weak acid leaching, then add electrolytic waste liquid low acid leaching, obtain oxide ore low acid supernatant and low leaching residue, then wash the oxide ore low leaching residue with water, the washing liquid-solid ratio is 2:1, stir for 1h, temperature 70 o C. Finally, high silicon slag and water-washed liquid are obtained. The high silicon slag is stored and zinc is precipitated from the water-washed liquid.
2. The process of oxygen-sulfur synergistic leaching and silicon-controlled iron removal in hydrometallurgy according to claim 1, characterized in that: The post-hydrolysis liquid in S1 includes post-iron precipitation liquid and post-iron precipitation slag pickling liquid.
3. The process of oxygen-sulfur synergistic leaching and silicon-controlled iron removal in hydrometallurgy according to claim 1, characterized in that: During the low-acid leaching of S2, the residual heat of weak acid leaching can be used for heating without further heating. The temperature is 70° C. and the reaction time is 0.5 hours.
4. The process for removing iron from silicon by oxygen-sulfur synergistic leaching in hydrometallurgy according to claim 1, characterized in that: The high-acid leaching pre-liquid in S2 is electrolytic waste liquid, and the high-acid supernatant is used as the hot acid leaching pre-liquid. The reaction temperatures of hot acid leaching and high-acid leaching are both 80°C, and the reaction time is 3 hours. The slurry is flocculated and settled, and the bottom flow is filtered. When the high-acid leaching residue is quickly filtered and dried, 200 ml of hot water is added to the funnel for infiltration and washing; among them, the high-acid leaching residue can be used for external sale.
5. The process of oxygen-sulfur synergistic leaching and silicon-controlled iron removal in hydrometallurgy according to claim 1, characterized in that: When oxide ore is used as a neutralizing agent in the S4, in order to ensure the iron precipitation rate and filtration performance during the hydrolysis iron precipitation process, the end point pH value is close to 4.5, and a large amount of ZnCO3 cannot participate in the reaction. Further pickling is required to increase the metal leaching rate. The liquid-to-solid ratio is 2.6:1, the temperature is 80°C, the time is 2h, and the pH value is adjusted using sulfuric acid solution. The end point pH value is 2.
5.
6. The process of oxygen-sulfur synergistic leaching and silicon-controlled iron removal in hydrometallurgy according to claim 1, characterized in that: When zinc precipitate slag is used as a neutralizer in S4, air can be used as an oxidant under the condition of pH 4.0-5.0.