Self-lubricating composite material with coating structure and preparation method thereof

By adopting a coating structure in self-lubricating composite materials, wrapping WS2 or MoS2 powder on Ti3SiC2 or Ti3AlC2 powder solves the problems of lubricating phase decomposition and insufficient mechanical properties in the existing technology, achieving high strength, toughness and good lubricity. Suitable for sealing and transmission parts.

CN118726795AActive Publication Date: 2024-10-01NORTHEASTERN UNIV CHINA
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410911292.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-01
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

Existing self-lubricating materials are prone to in-situ reactions during sintering, leading to the decomposition of the lubricating phase. They cannot meet the high mechanical properties and wear resistance requirements of mechanical components, and have poor lubrication effects.

Method used

Using a self-lubricating composite material with a coating structure, the WS2 or MoS2 powder is evenly wrapped on the Ti3SiC2 or Ti3AlC2 powder through a low-energy ball milling process, and mixed with Ni, Co or Fe-based alloy powder to form a lubricating phase coating structure to avoid the lubricating phase. Uniform distribution in the matrix improves mechanical properties and lubricity.

Benefits of technology

It achieves high strength and toughness, excellent corrosion resistance and good friction-reducing and wear-resisting properties, ensuring the long-term safe and stable operation of mechanical equipment and reducing the friction coefficient and wear rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726795A_ABST
    Figure CN118726795A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of metal-based self-lubricating composite materials, and particularly relates to a self-lubricating composite material with a coating structure and a preparation method of the self-lubricating composite material. The composite material is prepared from 70-90% of Ni, Co or Fe-based alloy powder; 5 to 15 percent of Ti3SiC2 or Ti3AlC2 powder; and 5 to 15 percent of WS2 or MoS2 powder. Through component design and ball milling process regulation and control, the surface of the protruding hard phase is coated with the limited low-strength self-lubricating phase, on the premise of exerting the maximum lubricity, the defect that the obdurability of the composite material is reduced due to the fact that excessive self-lubricating phases are added in a traditional method is overcome, the material has the advantages of high strength, high toughness, high self-lubricating performance and the like, and the service life of the composite material is prolonged. The method is suitable for production of movement and transmission parts such as seals and bearings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal-based self-lubricating composite materials, and in particular relates to a self-lubricating composite material with a coating structure and a preparation method thereof. Background Art

[0002] With the rapid development of aviation, aerospace, marine and nuclear power industries, the operating conditions of some key transmission or motion components are becoming increasingly demanding. Under certain working conditions, lubricating oil and grease will no longer meet the use requirements, and for closed components, it is impossible to improve the lubricity by adding external lubricants. In view of this situation, new self-lubricating materials are the key to solving such problems.

[0003] Usually, researchers add self-lubricating phases such as graphite, Ag, WS2, MoS2 and BN into the metal matrix to reduce friction. However, due to the low hardness and shear strength of the lubricating phase, the wettability between the lubricating phase and the matrix is ​​poor, and some lubricating phases are easily decomposed during sintering. When these lubricating phases are evenly distributed in the matrix, the mechanical properties and wear resistance of the material will decrease, which brings challenges to the composite materials as mechanical parts. Therefore, it is urgent to develop self-lubricating composite materials with both excellent mechanical properties and good friction and wear resistance. Nickel-based alloys, cobalt-based alloys and stainless steel have the advantages of high corrosion resistance, high strength and plasticity, and are often used as self-lubricating material matrices in moving parts. However, these alloys are prone to in-situ reactions when sintered with the lubricating phase, resulting in the decomposition of the lubricating phase (WS2, MoS2, Ti3SiC2, etc.) or the generation of harmful phases, which cannot meet the requirements of friction and wear resistance, limiting their application in the direction of self-lubrication.

[0004] Therefore, according to the industrial development requirements for mechanical properties and self-lubricating properties of materials, it is urgent to develop a new self-lubricating composite material with high strength, toughness and high self-lubricating properties. Summary of the invention

[0005] In view of the problems in the prior art, the present invention provides a self-lubricating composite material with a coating structure and a preparation method thereof. The composite material is suitable for the production of motion and transmission parts such as seals and bearings, and solves the problems of easy decomposition and failure of the lubricating phase of the self-lubricating material in the prior art, mismatch in strength and toughness, and poor lubrication effect.

[0006] The technical solution of the present invention is: A self-lubricating composite material with a coating structure, the composite material comprises the following components in terms of weight percentage: Ni, Co or Fe-based alloy powder 70-90%; Ti3SiC2 or Ti3AlC2 powder 5-15%; WS2 or MoS2 powder 5-15%.

[0007] Furthermore, in the above-mentioned self-lubricating composite material with a coating structure, the Ni, Co or Fe-based alloy includes Ni, NiCr, NiCrAl, Co, CoCr and stainless steel, and the original powder particle size is 30 to 100 μm; the Ti3SiC2 or Ti3AlC2 powder particle size is 30 to 80 μm; the WS2 or MoS2 powder particle size is less than 5 μm.

[0008] The preparation method of the self-lubricating composite material with a coating structure described above has the following specific steps: (1) Powder mixing: firstly, Ti3SiC2 or Ti3AlC2 powder is mixed with WS2 or MoS2 powder by planetary ball milling at a speed of 100-150 rpm for 2-4 hours, thereby obtaining a coating structure of Ti3SiC2 or Ti3AlC2 powder coated with WS2 or MoS2 powder; then, the coated powder is mixed with Ni, Co or Fe-based alloy powder by planetary ball milling at a speed of 100-150 rpm for 2-4 hours, thereby obtaining a uniformly mixed composite powder; (2) Pre-pressing: the composite powder obtained in step (1) is loaded into a graphite mold and then pre-pressed using a cold press; (3) Spark plasma sintering: The graphite abrasive tool loaded with the composite powder in step (2) is placed in a spark plasma sintering equipment furnace chamber for sintering. After sintering, the composite material is obtained by cooling the furnace.

[0009] Furthermore, in the method for preparing the self-lubricating composite material with a coating structure, the ball mill and the mixing material used in the planetary ball mill in step (1) are both made of stainless steel, and the ball-to-material ratio is 10:1.

[0010] Furthermore, in the method for preparing the self-lubricating composite material with a coating structure, when pre-pressing with a cold press in step (2), the pre-pressing is performed at a rate of 10 MPa / min to 20 MPa, and the pre-pressing is maintained for 10 minutes before unloading.

[0011] Furthermore, in the method for preparing the self-lubricating composite material with a coating structure, the process parameters of the spark plasma sintering are as follows: The vacuum degree is less than 1×10 -2 Pa; sintering temperature is 1000~1250 ℃; heating rate is 40~80 ℃ / min; sintering pressure is 30~50 MPa; holding time is 10~30 min.

[0012] Furthermore, the performance indexes of the self-lubricating composite material prepared by the method of the above-mentioned self-lubricating composite material with a coating structure are as follows: Density ≥ 99%; hardness ≥ 350HV; compression strength ≥ 1400MPa; compression rate ≥ 28%; friction with Si3N4 material at room temperature with parameters of 10N and 24mm / s, the average friction coefficient in atmospheric environment is less than 0.28, the friction coefficient in seawater corrosion environment is less than 0.10, and the wear rate is less than 1.0×10 -5 mm 3 / (Nm).

[0013] The design idea of ​​the present invention is: The present invention is designed to firstly use a low-energy ball milling process to uniformly coat the lubricating phase WS2 (or MoS2) powder with a smaller grain size on the Ti3SiC2 (or Ti3AlC2) powder, and then mix the coated powder with the matrix alloy powder by low-energy ball milling. Although the lubricating phase will decompose during sintering, an in-situ reaction will also occur at the same time, so that a hard phase is formed inside the coating structure and a MAX phase Ti2SC with excellent lubricity is formed outside. The coating structure concentrates and agglomerates the lubricating phase, which not only avoids the uniform distribution of the lubricating phase with poor mechanical properties in the matrix, but also improves the mechanical properties of the self-lubricating composite material. It can also protrude from the surface of the matrix, so that the coating structure with higher strength and better lubricity is preferentially subjected to the friction load, providing lubrication and support, thereby achieving the effect of reducing friction and resisting wear.

[0014] The advantages and beneficial effects of the present invention are: (1) The present invention uses Ni, Co or Fe-based alloy as the matrix, which has the advantages of high toughness, excellent corrosion resistance, etc. After adding WS2 (or MoS2) powder and Ti3SiC2 (or Ti3AlC2) powder, an in-situ reaction will occur to generate new hard phase and lubricating phase. While ensuring excellent mechanical properties, it can also avoid the problem of self-lubricating failure caused by the decomposition of the lubricating phase. This is of great significance for ensuring the long-term safe and stable operation of mechanical equipment.

[0015] (2) The present invention adopts a secondary ball milling process to obtain a coating structure in which a lubricating phase encapsulates a hard phase in a Ni, Co or Fe-based alloy. This coating structure protrudes from the surface of the substrate. When subjected to friction and load, the coating structure can preferentially provide lubrication and support, thereby greatly reducing the friction coefficient and wear rate of the material.

[0016] (3) The process parameters in the material preparation process of the present invention are easy to control and highly feasible, the experimental method is simple and novel, the metal powder used in the present invention is moderately priced and easy to obtain, and the material properties can be controlled by simple process adjustments. It has a wide range of uses in engineering machinery, nuclear power industry, aerospace and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 Schematic diagram of the ball milling process to obtain the coated structure; Figure 2 The material structure morphology after sintering by secondary coating ball milling is shown in Example 1, with NiCr alloy powder as the matrix and WS2 and Ti3SiC2 powder as the added phase; Figure 3 The material structure morphology after sintering by direct ball milling is shown in Comparative Example 1, in which NiCr alloy powder is used as the matrix and WS2 and Ti3SiC2 powders are used as the additive phases; Figure 4 It is an enlarged view of the coating structure in Example 1 and the corresponding EDS spectrum. DETAILED DESCRIPTION

[0018] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention but cannot be used to limit the scope of the present invention. Example 1

[0019] In this embodiment, a method for preparing a self-lubricating composite material with a coating structure is to use a NiCr high temperature alloy as a matrix with a particle size of 30-50 μm, and to use WS2 powder and Ti3SiC2 particles as additives to prepare the composite material, wherein the WS2 powder particle size is less than 5 μm, and the Ti3SiC2 particle size is 30-60 μm, and the composite material ratio is 80 wt% NiCr alloy, 10 wt% WS2 powder, and 10 wt% Ti3SiC2 powder. The specific preparation process and parameters are as follows: (1) Powder mixing: Ti3SiC2 powder and WS2 powder are first mixed by planetary ball milling at a speed of 150 rpm for 2 hours to obtain a particle structure of WS2 powder coated with Ti3SiC2 powder; then the coated powder is mixed with NiCr alloy powder by planetary ball milling at a speed of 150 rpm for 2 hours to obtain a uniformly mixed composite powder, such as Figure 1 Shown is a schematic diagram of the ball milling process for obtaining the coating structure, and an enlarged view of the coating structure and the corresponding EDS spectrum are shown in the figure.

[0020] (2) Pre-pressing: The composite powder obtained in step (1) is placed in a graphite mold, and the composite powder is pre-pressed to 20 MPa at a rate of 10 MPa / min using a cold press, maintained for 10 min, and then unloaded.

[0021] (3) Spark plasma sintering: Put the graphite abrasive containing composite powder into the furnace chamber and undergo spark plasma sintering: The vacuum degree is less than 1×10 -2 Pa; sintering temperature is 1100 ℃; heating rate is 40 ℃ / min; sintering pressure is 40MPa; holding time is 15 min.

[0022] The morphology of the material after sintering is as follows Figure 2 As shown in the figure, the density of the sintered composite material is 99.4%; the hardness is 425HV; the yield strength is 856MPa; the compressive strength is 1608MPa; the compression rate is 32.1%; the average friction coefficient is 0.24 when rubbed with Si3N4 ball (diameter 9.5mm) at room temperature with the parameters of 10N and 24mm / s; the wear rate is 7.5×10 -6 mm 3 / (Nm). Comparative Example 1

[0023] The difference between this comparative example and Example 1 is that the ball milling process of the composite material is direct ball milling.

[0024] The ball milling process is as follows: NiCr alloy powder, WS2 powder and Ti3SiC2 particles are simultaneously put into a ball mill for ball milling, the ball milling speed is 300 rpm, and the ball milling time is 4 h.

[0025] The morphology of the material after sintering is as follows Figure 3 As shown in the figure, the density of the sintered composite material is 99.5%, the hardness is 411HV, the yield strength is 880MPa, the compressive strength is 1433MPa, the compression rate is 24.4%, the average friction coefficient at room temperature is 0.38, and the wear rate is 9.8×10 -6 mm 3 / (Nm). Comparative Example 2

[0026] The difference between this comparative example and Example 1 is that the composition ratio of the composite material is 90 wt% of NiCr alloy, 5 wt% of WS2 powder, and 5 wt% of Ti3SiC2 powder.

[0027] The density of the sintered composite material is 99.7%, the hardness is 318HV, the yield strength is 670MPa, the compressive strength is 1682MPa, the compression rate is 38.9%, the average friction coefficient at room temperature is 0.35, and the wear rate is 4.6×10 -5 mm 3 / (Nm). Comparative Example 3

[0028] The difference between this comparative example and Example 1 is that the composition ratio of the composite material is 70 wt % of NiCr alloy, 15 wt % of WS2 powder, and 15 wt % of Ti3SiC2 powder.

[0029] The density of the sintered composite material is 99.3%, the hardness is 522HV, the yield strength is 1011MPa, the compression strength is 1525MPa, the compression rate is 18.5%, the average friction coefficient at room temperature is 0.21, and the wear rate is 5.9×10 -6 mm 3 / (Nm). Comparative Example 4

[0030] The difference between this comparative example and Example 1 is that the composition ratio of the composite material is 80 wt % of NiCr alloy, 10 wt % of MoS2 powder, and 10 wt % of Ti3SiC2 powder.

[0031] The density of the sintered composite material is 99.4%; the hardness is 404HV; the yield strength is 815MPa; the compressive strength is 1586MPa; the compression rate is 30.5%; the average friction coefficient at room temperature is 0.26, and the wear rate is 8.4×10 -6 mm 3 / (Nm). Comparative Example 5

[0032] The difference between this comparative example and Example 1 is that the composition ratio of the composite material is 80 wt % of NiCr alloy, 10 wt % of WS2 powder, and 10 wt % of Ti3AlC2 powder.

[0033] The density of the sintered composite material is 99.5%; the hardness is 398HV; the yield strength is 768MPa; the compression strength is 1541MPa; the compression rate is 31.2%; the average friction coefficient at room temperature is 0.29, and the wear rate is 9.2×10 -6 mm 3 / (Nm). Comparative Example 6

[0034] The difference between this comparative example and Example 1 is that the composition ratio of the composite material is 100 wt % of NiCr alloy.

[0035] The density of the sintered composite material is 99.1%; the hardness is 208HV; the yield strength is 421MPa; the average friction coefficient at room temperature is 0.55, and the wear rate is 9.8×10 -5 mm 3 / (Nm). Example 2

[0036] In this embodiment, the preparation method of the self-lubricating composite material with a coating structure is the same as that of Example 1, and a NiCr-based self-lubricating composite material with a coating structure is obtained. However, the friction environment of the material is different from that of Example 1, and its specific friction and wear parameters are as follows: (1) The samples were subjected to friction and wear tests in 3.5% NaCl solution.

[0037] (2) To prevent liquid splashing, the experiment was carried out with friction against a Si3N4 ball (diameter 9.5 mm) at parameters of 10 N and 12 mm / s.

[0038] Its friction and wear properties in 3.5% NaCl solution are as follows: the average friction coefficient is 0.08, the wear rate is 3.2×10 -6 mm 3 / (Nm). Comparative Example 7

[0039] The difference between this comparative example and Example 2 is that the ball milling process of the composite material is direct ball milling.

[0040] Its friction and wear properties in 3.5% NaCl solution are as follows: the average friction coefficient is 0.23, the wear rate is 8.4×10 -6 mm 3 / (Nm). Comparative Example 8

[0041] The difference between this comparative example and Example 2 is that the mass fraction of the NaCl solution is 5%.

[0042] Its friction and wear properties in 5% NaCl solution are as follows: the average friction coefficient is 0.07, the wear rate is 2.9×10 -6 mm 3 / (Nm). Example 3

[0043] In this embodiment, the preparation method of the self-lubricating composite material with a coating structure is to use pure Ni as the matrix, the particle size is 50-90 μm, and MoS2 powder and Ti3AlC2 particles are used as additives to prepare the composite material, the particle size of MoS2 powder is less than 5 μm, the particle size of Ti3AlC2 particles is 40-80 μm, and the ratio of the composite material is 80 wt% pure Ni powder, 10 wt% MoS2 powder, and 10 wt% Ti3AlC2 powder. The specific preparation process and parameters are as follows: (1) Powder mixing: Ti3AlC2 powder and MoS2 powder were first mixed by planetary ball milling at a speed of 150 rpm for 2 hours to obtain a particle structure of MoS2 powder coated with Ti3AlC2 powder. The coated powder was then mixed with Ni powder by planetary ball milling at a speed of 150 rpm for 2 hours to obtain a uniformly mixed composite powder.

[0044] (2) Pre-pressing: The composite powder obtained in step (1) is placed in a graphite mold, and the composite powder is pre-pressed to 20 MPa at a rate of 10 MPa / min using a cold press, maintained for 10 min, and then unloaded.

[0045] (3) Spark plasma sintering: Put the graphite abrasive containing composite powder into the furnace chamber and undergo spark plasma sintering: The vacuum degree is less than 1×10 -2 Pa; sintering temperature is 1100 ℃; heating rate is 40 ℃ / min; sintering pressure is 40MPa; holding time is 15 min.

[0046] The density of the sintered composite material is 99.6%; the hardness is 393HV; the yield strength is 818MPa; the compressive strength is 1589MPa; the compression rate is 31.4%; the average friction coefficient is 0.26 when rubbed with Si3N4 ball (diameter 9.5mm) at room temperature with the parameters of 10N and 24mm / s; the wear rate is 7.9×10 -6 mm 3 / (Nm). Comparative Example 9

[0047] The difference between this comparative example and Example 3 is that the ball milling process of the composite material is direct ball milling.

[0048] The ball milling process is as follows: pure Ni powder, MoS2 powder and Ti3AlC2 particles are put into a ball mill at the same time for ball milling, the ball milling speed is 300 rpm, and the ball milling time is 4 hours.

[0049] The density of the sintered composite material is 99.6%, the hardness is 411HV, the yield strength is 861MPa, the compressive strength is 1538MPa, the compression rate is 23.8%, the average friction coefficient at room temperature is 0.35, and the wear rate is 1.1×10 -5 mm 3 / (Nm). Example 4

[0050] In this embodiment, a method for preparing a self-lubricating composite material with a coating structure is to use NiCrAl alloy as a matrix with a particle size of 50-80 μm, and to use MoS2 powder and Ti3SiC2 particles as additives to prepare the composite material, wherein the particle size of MoS2 powder is less than 5 μm, and the particle size of Ti3SiC2 particles is 30-60 μm. The composite material ratio is 80 wt% of NiCrAl alloy powder, 10 wt% of MoS2 powder, and 10 wt% of Ti3SiC2 powder. The specific preparation process and parameters are as follows: (1) Powder mixing: Ti3SiC2 powder and MoS2 powder were first mixed by planetary ball milling at a speed of 150 rpm for 2 hours to obtain a particle structure of MoS2 powder coated with Ti3SiC2 powder. The coated powder was then mixed with NiCrAl alloy powder by planetary ball milling at a speed of 150 rpm for 2 hours to obtain a uniformly mixed composite powder.

[0051] (2) Pre-pressing: The composite powder obtained in step (1) is placed in a graphite mold, and the composite powder is pre-pressed to 20 MPa at a rate of 10 MPa / min using a cold press, maintained for 10 min, and then unloaded.

[0052] (3) Spark plasma sintering: Put the graphite abrasive containing composite powder into the furnace chamber and undergo spark plasma sintering: The vacuum degree is less than 1×10 -2 Pa; sintering temperature is 1150 ℃; heating rate is 60 ℃ / min; sintering pressure is 40MPa; holding time is 15 min.

[0053] The density of the sintered composite material is 99.6%; the hardness is 431HV; the yield strength is 896MPa; the compressive strength is 1710MPa; the compression rate is 26.5%; the average friction coefficient is 0.27 when rubbed with Si3N4 ball (diameter 9.5mm) at room temperature with the parameters of 10N and 24mm / s; the wear rate is 6.8×10 -6 mm 3 / (Nm). Comparative Example 10

[0054] The difference between this comparative example and Example 4 is that the ball milling process of the composite material is direct ball milling.

[0055] The ball milling process is as follows: NiCrAl alloy powder, MoS2 powder and Ti3SiC2 particles are simultaneously put into a ball mill for ball milling, the ball milling speed is 300 rpm, and the ball milling time is 4 hours.

[0056] The density of the sintered composite material is 99.6%, the hardness is 438HV, the yield strength is 887MPa, the compression strength is 1735MPa, the compression rate is 19.8%, the average friction coefficient at room temperature is 0.37, and the wear rate is 1.6×10 -5 mm 3 / (Nm). Comparative Example 11

[0057] The difference between this comparative example and Example 4 is that the composition ratio of the composite material is 90 wt% of NiCrAl alloy powder, 5 wt% of MoS2 powder, and 5 wt% of Ti3SiC2 powder.

[0058] The density of the sintered composite material is 99.7%, the hardness is 339HV, the yield strength is 689MPa, the compression strength is 1765MPa, the compression rate is 36.7%, the average friction coefficient at room temperature is 0.37, and the wear rate is 4.4×10 -5 mm 3 / (Nm) Example 5

[0059] In this embodiment, the preparation method of the self-lubricating composite material with a coating structure is the same as that of Example 4, and a NiCrAl-based self-lubricating composite material with a coating structure is obtained. However, the friction environment of the material is different from that of Example 4, and its specific friction and wear parameters are as follows: (1) The samples were subjected to friction and wear tests in 3.5% NaCl solution.

[0060] (2) To prevent liquid splashing, the experiment was carried out with friction against a Si3N4 ball (diameter 9.5 mm) at parameters of 10 N and 12 mm / s.

[0061] Its friction and wear properties in 3.5% NaCl solution are as follows: the average friction coefficient is 0.10, the wear rate is 3.8×10 -6 mm 3 / (Nm). Comparative Example 12

[0062] The difference between this comparative example and Example 5 is that the ball milling process of the composite material is direct ball milling.

[0063] Its friction and wear properties in 3.5% NaCl solution are as follows: the average friction coefficient is 0.26, the wear rate is 7.9×10 -6 mm 3 / (Nm). Comparative Example 13

[0064] The difference between this comparative example and Example 5 is that the mass fraction of the NaCl solution is 5%.

[0065] Its friction and wear properties in 5% NaCl solution are as follows: the average friction coefficient is 0.09, the wear rate is 3.1×10 -6 mm 3 / (Nm). Example 6

[0066] In this embodiment, a method for preparing a self-lubricating composite material with a coating structure is used. Co is used as a matrix, and the particle size is 30-50 μm. WS2 powder and Ti3AlC2 particles are used as additives to prepare the composite material. The WS2 powder particle size is less than 5 μm, and the Ti3AlC2 particle size is 40-80 μm. The composite material ratio is 80 wt% pure Co powder, 10 wt% WS2 powder, and 10 wt% Ti3AlC2 powder. The specific preparation process and parameters are as follows: (1) Powder mixing: Ti3SiC2 powder and WS2 powder were first mixed by planetary ball milling at a speed of 150 rpm for 2 hours to obtain a particle structure of WS2 powder coated with Ti3AlC2 powder. The coated powder was then mixed with pure Co powder by planetary ball milling at a speed of 150 rpm for 2 hours to obtain a uniformly mixed composite powder.

[0067] (2) Pre-pressing: The composite powder obtained in step (1) is placed in a graphite mold, and the composite powder is pre-pressed to 20 MPa at a rate of 10 MPa / min using a cold press, maintained for 10 min, and then unloaded.

[0068] (3) Spark plasma sintering: Put the graphite abrasive containing composite powder into the furnace chamber and undergo spark plasma sintering: The vacuum degree is less than 1×10 -2 Pa; sintering temperature is 1150 ℃; heating rate is 60 ℃ / min; sintering pressure is 40MPa; holding time is 15 min.

[0069] The density of the sintered composite material is 99.5%; the hardness is 418HV; the yield strength is 968MPa; the compressive strength is 1824MPa; the compression rate is 27.3%; the average friction coefficient is 0.28 when rubbed with Si3N4 ball (diameter 9.5mm) at room temperature with the parameters of 10N and 24mm / s; the wear rate is 8.1×10 -6 mm 3 / (Nm). Example 7

[0070] In this embodiment, a method for preparing a self-lubricating composite material with a coating structure is used. CoCr is used as a matrix, and the particle size is about 50 μm. WS2 powder and Ti3AlC2 particles are used as additives to prepare the composite material. The particle size of WS2 powder is less than 5 μm, and the particle size of Ti3AlC2 particles is 40-80 μm. The ratio of the composite material is 80 wt% of CoCr powder, 10 wt% of WS2 powder, and 10 wt% of Ti3AlC2 powder. The specific preparation process and parameters are as follows: (1) Powder mixing: Ti3SiC2 powder and WS2 powder were first mixed by planetary ball milling at a speed of 150 rpm for 2 hours to obtain a particle structure of WS2 powder coated with Ti3AlC2 powder. The coated powder was then mixed with CoCr powder by planetary ball milling at a speed of 150 rpm for 2 hours to obtain a uniformly mixed composite powder.

[0071] (2) Pre-pressing: The composite powder obtained in step (1) is placed in a graphite mold, and the composite powder is pre-pressed to 20 MPa at a rate of 10 MPa / min using a cold press, maintained for 10 min, and then unloaded.

[0072] (3) Spark plasma sintering: Put the graphite abrasive containing composite powder into the furnace chamber and undergo spark plasma sintering: The vacuum degree is less than 1×10 -2 Pa; sintering temperature is 1150 ℃; heating rate is 60 ℃ / min; sintering pressure is 40MPa; holding time is 15 min.

[0073] The density of the sintered composite material is 99.5%; the hardness is 479HV; the yield strength is 951MPa; the compressive strength is 1921MPa; the compression rate is 28.7%; the average friction coefficient is 0.26 when rubbed with Si3N4 ball (diameter 9.5mm) at room temperature with the parameters of 10N and 24mm / s; the wear rate is 7.4×10 -6 mm 3 / (Nm). Example 8

[0074] In this embodiment, a method for preparing a self-lubricating composite material with a coating structure is used. 316 stainless steel powder is used as a matrix, and the particle size is about 30 μm. MoS2 powder and Ti3AlC2 particles are used as additives to prepare the composite material. The particle size of MoS2 powder is less than 5 μm and the particle size of Ti3AlC2 particles is 40-80 μm. The composite material ratio is 80 wt% of 316 stainless steel powder, 10 wt% of MoS2 powder, and 10 wt% of Ti3AlC2 powder. The specific preparation process and parameters are as follows: (1) Powder mixing: Ti3SiC2 powder and MoS2 powder were first mixed by planetary ball milling at a speed of 150 rpm for 2 hours to obtain a particle structure of MoS2 powder coated with Ti3AlC2 powder. The coated powder was then mixed with 316 stainless steel powder by planetary ball milling at a speed of 150 rpm for 2 hours to obtain a uniformly mixed composite powder.

[0075] (2) Pre-pressing: The composite powder obtained in step (1) is placed in a graphite mold, and the composite powder is pre-pressed to 20 MPa at a rate of 10 MPa / min using a cold press, maintained for 10 min, and then unloaded.

[0076] (3) Spark plasma sintering: Put the graphite abrasive containing composite powder into the furnace chamber and undergo spark plasma sintering: The vacuum degree is less than 1×10 -2 Pa; sintering temperature is 1250 ℃; heating rate is 50 ℃ / min; sintering pressure is 40MPa; holding time is 15 min.

[0077] The density of the sintered composite material is 99.4%; the hardness is 378HV; the yield strength is 689MPa; the compressive strength is 1320MPa; the compression rate is 29.1%; the average friction coefficient is 0.28 when rubbed with Si3N4 ball (diameter 9.5mm) at room temperature with the parameters of 10N and 24mm / s; the wear rate is 8.3×10 -6 mm 3 / (Nm).

[0078] The results of the embodiments and comparative examples show that the present invention is designed to firstly use a low-energy ball milling process to uniformly coat the lubricating phase WS2 (or MoS2) powder with a smaller grain size on the Ti3SiC2 (or Ti3AlC2) powder, and then the coated powder is mixed with Ni, Co or Fe-based alloy powder by low-energy ball milling. During sintering, a coating structure in which the lubricating phase coats the hard phase is formed. The coating structure not only improves the mechanical properties of the nickel-based self-lubricating material, but also plays a supporting and lubricating role when subjected to friction loads, thereby achieving the effect of reducing friction and resisting wear.

[0079] The above is only a preferred embodiment of the present invention. For those skilled in the art, the present invention is not limited to the above detailed composition and preparation method. Any improvement of the present invention, substitution of product raw materials and addition of auxiliary components are within the protection scope and disclosure scope of the present invention.

Claims

1. A self-lubricating composite material with a coating structure, It is characterized in that The composite material is composed of the following components by weight percentage: Ni, Co or Fe-based alloy powder 70-90%; Ti 3 SiC 2 or Ti 3 AlC 2 Powder 5-15%; WS 2 or MoS 2 Powder 5-15%.

2. The self-lubricating composite material with a coating structure according to claim 1, It is characterized in that The Ni, Co or Fe-based alloy includes Ni, NiCr, NiCrAl, Co, CoCr and stainless steel, and the original powder particle size is 30-100 μm; the Ti 3 SiC 2 or Ti 3 AlC 2 The powder particle size is 30 to 80 μm; the WS 2 or MoS 2 The powder particle size is less than 5μm.

3. A method for preparing the self-lubricating composite material with a coating structure according to claim 1, It is characterized in that The specific steps of this method are as follows: (1) Powder mixing: First, mix Ti 3 SiC 2 or Ti 3 AlC 2 Powder and WS 2 or MoS 2 The powders were mixed by planetary ball milling at a speed of 100-150 rpm for 2-4 hours to obtain WS 2 or MoS 2 Powder coated Ti 3 SiC 2 or Ti 3 AlC 2 The coated powder is then mixed with Ni, Co or Fe-based alloy powder by planetary ball milling at a speed of 100 to 150 rpm for 2 to 4 hours to obtain a uniformly mixed composite powder; (2) Pre-pressing: the composite powder obtained in step (1) is loaded into a graphite mold and then pre-pressed using a cold press; (3) Spark plasma sintering: The graphite abrasive tool loaded with the composite powder in step (2) is placed in a spark plasma sintering equipment furnace chamber for sintering. After sintering, the composite material is obtained by cooling the furnace.

4. The method for preparing the self-lubricating composite material with a coating structure according to claim 3, It is characterized in that The ball mill and mixing material used in the planetary ball mill in step (1) are both made of stainless steel, and the ball-to-material ratio is 10:

1.

5. The method for preparing the self-lubricating composite material with a coating structure according to claim 3, It is characterized in that When pre-pressing with a cold press in step (2), pre-press to 20 MPa at a rate of 10 MPa / min, maintain for 10 minutes, and then unload.

6. The method for preparing the self-lubricating composite material with a coating structure according to claim 3, It is characterized in that The process parameters of the spark plasma sintering are as follows: The vacuum degree is less than 1×10 -2 Pa; sintering temperature is 1000~1250 ℃; heating rate is 40~80 ℃ / min; sintering pressure is 30~50 MPa; holding time is 10~30 min.

7. The method for preparing the self-lubricating composite material with a coating structure according to claim 3, It is characterized in that The performance indicators of the self-lubricating composite material prepared by this method are as follows: Density ≥ 99%; Hardness ≥ 350HV; Compression strength ≥ 1400MPa; Compression rate ≥ 28%; At room temperature, the parameters of 10N and 24mm / s are comparable to Si 3 N 4 The average friction coefficient of the material in the atmospheric environment is less than 0.28, the friction coefficient in the seawater corrosion environment is less than 0.10, and the wear rate is less than 1.0×10 -5 mm 3 / (Nm).

Citation Information

Patent Citations

  • TiAl-based high-temperature-resistant self-lubricating composite and preparation method

    CN107916349A

  • Fe-based high-temperature-resistant self-lubricating composite material and preparation method thereof

    CN109022993A

  • TiAl-Ti3AlC2 self-lubricating composite material and preparation method thereof

    CN109136722A

  • Self-lubricating wear-resistant titanium-based composite material part and preparation method thereof

    CN114411009A

  • High-strength low-cost self-supplementing lubricating phase composite material and preparation method thereof

    CN117020196A