Method for separating valuable metal elements from copper-containing metals

By breaking down the gaseous membrane in an acidic or alkaline electrolyte to generate a plasma reaction, the copper separation process is simplified, the problems of high toxic consumption and energy consumption in the existing technology are solved, and efficient copper separation and purity improvement are achieved.

CN118727062APending Publication Date: 2024-10-01赖志煌
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310327991.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The use of toxic organic extractants in existing copper separation and recovery technology is high in energy consumption, and it is difficult to effectively separate high-content impurity elements, which limits the purity and efficiency of copper recovery.

Method used

By providing a predetermined voltage in an acidic or alkaline electrolyte to break down the gaseous membrane and generate a plasma reaction, thereby precipitating solid copper or copper oxide and its impurity elements in the electrolyte, using centrifugation, sedimentation separation or membrane filtration. Solid-liquid separation simplifies the copper separation process.

Benefits of technology

It reduces the cost of chemical drugs and energy consumption, improves the purity and efficiency of copper recovery, and achieves efficient copper separation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727062A_ABST
    Figure CN118727062A_ABST
Patent Text Reader

Abstract

The invention discloses a method for separating valuable metal elements from copper-containing metal. The method comprises the following steps: (a) immersing an anode and the copper-containing metal serving as a cathode into an electrolyte with an acidic or alkaline pH value; and (b) providing a predetermined voltage to the anode and the cathode to form a gaseous film around the cathode during the electrolytic reaction between the cathode and the electrolyte, the predetermined voltage being sufficient to break down the gaseous film around the cathode so as to generate plasma in the electrolyte to precipitate solid copper metal or copper oxide, and the impurity element is dissolved in the electrolyte and is in an ionic state. When the pH value of the electrolyte is acidic, the step (b) is to separate out the solid copper metal; when the pH value of the electrolyte is alkaline, the step (b) is to precipitate the solid copper oxide. The gaseous film around the cathode is punctured through the preset voltage in the step (b) so as to generate plasma in the electrolyte, so that solid copper metal or copper oxide and impurity elements which are dissolved in the electrolyte and are in an ionic state can be separated out in the electrolyte, the use cost of chemicals can be reduced, and the energy consumption can also be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for separating valuable metal elements, in particular to a method for separating valuable metal elements from copper-containing metals. Background Art

[0002] Copper metal has excellent ductility, high thermal conductivity, and electrical conductivity, and is widely used in various fields and has become one of the most important metals in industry. Compared with other metal materials commonly used in industry, such as iron and aluminum, copper metal has a very low reserves-to-production ratio (that is, a low reserve life); and due to problems such as mineral depletion, difficulty in mining, and high costs, more industries are willing to choose recycled copper as an industrial material.

[0003] In the existing copper separation and recovery industry, the front-end process and the back-end process are combined. The existing copper separation and recovery front-end process generally uses hydrometallurgy or pyrometallurgy technology to perform the first step of purification, and the resulting copper purity is relatively low (<99wt%). After completing the existing copper separation and recovery front-end process, the electrorefining technology of the back-end process is combined to complete the second step of refining (copper purity is nearly 99.99wt%).

[0004] As for the technology of implementing hydrometallurgy, it includes the steps of acid dissolution and extraction, which requires the use of toxic organic extractants, generates a large amount of chemical consumption, and has a long reaction time.

[0005] In terms of pyrometallurgical technology, high-temperature melting is used to separate elements based on their different physical properties. This process consumes a lot of energy (~16,000 J / g), and certain elements may exist in the form of alloys due to their similar physical properties, making it impossible to achieve the best separation effect.

[0006] In addition, in the electrolytic refining technology used in refining, it uses the difference in basic potential of elements to separate elements by controlling the potential difference. Although it has good benefits and purification effects, it is only suitable for use in refining steps with low impurity content due to the limitations of the basic principle.

[0007] From the above description, it can be seen that reducing the use of toxic organic extractants to reduce the cost of chemical drugs while also reducing the energy consumption required for recovering valuable metal copper is a topic that needs to be broken through by relevant practitioners in the relevant technical field. Summary of the invention

[0008] The object of the present invention is to provide a method for separating valuable metal elements from copper-containing metals, which can reduce the cost of chemical drugs and also reduce the energy consumption required for recovering valuable metal copper.

[0009] The method for separating valuable metal elements from copper-containing metals of the present invention comprises the following steps: step (a) and step (b).

[0010] The step (a) is to immerse the anode and the copper-containing metal as the cathode in an electrolyte, wherein the pH value of the electrolyte is either acidic or alkaline.

[0011] The step (b) is to provide a predetermined voltage to the anode and the cathode to form a gaseous film around the cathode during the electrolytic reaction between the cathode and the electrolyte, and the predetermined voltage is sufficient to break through the gaseous film around the cathode to generate plasma in the electrolyte to precipitate solid copper metal or solid copper oxide, and impurity elements dissolved in the electrolyte and in ionic state. When the pH value of the electrolyte is acidic, the step (b) is to precipitate the solid copper metal; when the pH value of the electrolyte is alkaline, the step (b) is to precipitate the solid copper oxide.

[0012] The method for separating valuable metal elements from copper-containing metals of the present invention further comprises a step (c) after the step (b), wherein the step (c) is to subject the electrolyte after the step (b) to solid-liquid separation, thereby separating the solid copper metal or the solid copper oxide from the electrolyte.

[0013] In the method for separating valuable metal elements from copper-containing metals of the present invention, the solid-liquid separation in step (c) is selected from centrifugation, sedimentation separation, vacuum concentration, or membrane filtration.

[0014] The method of separating valuable metal elements from copper-containing metal of the present invention is selected from brass containing impurity elements or pure copper containing impurity elements.

[0015] The present invention relates to a method for separating valuable metal elements from copper-containing metals, wherein the impurity elements include zinc, iron, lead, and nickel.

[0016] In the method for separating valuable metal elements from copper-containing metals of the present invention, in the step (a), the pH value of the electrolyte is greater than 11 or less than 5.

[0017] In the method for separating valuable metal elements from copper-containing metals of the present invention, when the pH value of the electrolyte is greater than 11, the predetermined voltage of step (b) is between 70V and 250V.

[0018] In the method for separating valuable metal elements from copper-containing metals of the present invention, the electrolyte is selected from sodium hydroxide solution, potassium hydroxide solution, lithium hydroxide solution, cesium hydroxide solution, or rubidium hydroxide solution.

[0019] In the method for separating valuable metal elements from copper-containing metal of the present invention, when the pH value of the electrolyte is less than 5, the predetermined voltage of step (b) is between 160V and 400V.

[0020] In the method for separating valuable metal elements from copper-containing metals of the present invention, the electrolyte is selected from citric acid solution, acetic acid solution, sulfuric acid solution, or carbonic acid solution.

[0021] In the method for separating valuable metal elements from copper-containing metals of the present invention, the electrolyte in step (a) and step (b) has a working temperature between 50°C and 90°C.

[0022] In the method for separating valuable metal elements from copper-containing metal of the present invention, the electrolyte in step (a) and step (b) is contained in a reaction tank, and the reaction tank includes a double-layer wall, and the double-layer wall defines a peripheral space for circulating cooling water. The peripheral space is connected to a water circulation temperature control device so that the cooling water can circulate back and forth between the water circulation temperature control device and the peripheral space, and the water circulation temperature control device can control the temperature of the cooling water.

[0023] The beneficial effect of the present invention is that the solid copper metal or solid copper oxide and the impurity elements dissolved in the electrolyte in ionic state can be precipitated in the electrolyte by only breaking down the gaseous film around the cathode (i.e., copper-containing metal) by the predetermined voltage of the step (b) to generate the plasma in the electrolyte (i.e., solution plasma reaction), thereby reducing the cost of chemical drugs and energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Other features and effects of the present invention will be clearly presented in the embodiments with reference to the accompanying drawings, in which:

[0025] Figure 1 FIG. 1 is a schematic diagram illustrating a separation system used in implementing the method of separating valuable metal elements from copper-containing metals of the present invention. DETAILED DESCRIPTION

[0026] Before the present invention is described in detail, it should be noted that similar elements are denoted by the same reference numerals in the following description.

[0027] One embodiment of the method for separating valuable metal elements from copper-containing metals of the present invention is mainly through a method as follows Figure 1The separation system 2 shown in the figure is implemented. The separation system 2 includes a reaction tank 21 containing an electrolyte 20, an anode 23 and a cathode 24 disposed in the electrolyte 20, a power supply 22 electrically connected to the anode 23 and the cathode 24, and a water circulation temperature control device 3 connected to the reaction tank 21.

[0028] The reaction tank 21 has a double wall 211, and the double wall 211 defines a peripheral space 200 for circulating cooling water. The peripheral space 200 is connected to the water circulation temperature control device 3 so that the cooling water can circulate back and forth between the water circulation temperature control device 3 and the peripheral space 200, and the water circulation temperature control device 3 can control the temperature of the cooling water. In this embodiment of the present invention, the water circulation temperature control device 3 uses a chiller.

[0029] In detail, the water circulation temperature control device 3 has a water outlet 31 and a water inlet 32, and the water outlet 31 and the water inlet 32 ​​are respectively connected to the peripheral space 200 by a water pipe. After the temperature (low temperature) of the cooling water is controlled in the water circulation temperature control device 3, the low-temperature cooling water is output to the peripheral space 200 through the water outlet 31 to absorb the heat (high temperature) generated by the electrolyte 20 in the reaction tank 21 during the execution of the method of the embodiment, and then the cooling water in the peripheral space 200 after absorbing heat is recovered by the water inlet 32, and the low-temperature cooling water is further output from the water outlet 31 to the peripheral space 200 to maintain the temperature of the cooling water in the peripheral space 200. In this way, the temperature of the entire electrolytic solution 20 can be controlled by controlling the temperature of the cooling water in the peripheral space 200.

[0030] The method for separating valuable metal elements from copper-containing metal according to this embodiment of the present invention comprises the following steps: a step (a), a step (b), and a step (c).

[0031] The step (a) is to immerse the anode 23 and a copper-containing metal as the cathode 24 in the electrolyte 20, and the pH value of the electrolyte 20 is one of acidic and alkaline. The copper-containing metal suitable for this embodiment of the present invention is selected from brass containing impurity elements or pure copper containing impurity elements; wherein the impurity elements include zinc (Zn), iron (Fe), lead (Pb), and nickel (Ni).

[0032] The step (b) is to provide a predetermined voltage from the power supply 22 to the anode 23 and the cathode 24 to form a gas film 240 around the cathode 24 during an electrolytic reaction between the cathode 24 and the electrolyte 20, and the predetermined voltage is sufficient to break through the gas film 240 around the cathode 24, thereby generating a plasma in the electrolyte 20 to precipitate a solid copper metal or a solid copper oxide, and impurity elements dissolved in the electrolyte 20 and in ionic state.

[0033] When the pH value of the electrolyte 20 is acidic, the step (b) is to precipitate the solid copper metal; when the pH value of the electrolyte 20 is alkaline, the step (b) is to precipitate the solid copper oxide.

[0034] Preferably, in step (a), the pH value of the electrolyte 20 is greater than 11 or less than 5. It should be further explained here that in order to make the gaseous film 240 around the cathode 24 sufficiently broken down by the predetermined voltage, it is also necessary to prevent the cathode 24 from melting during the electrolysis reaction and failing to be in an ionized state due to receiving an excessively high predetermined voltage value. Therefore, preferably, the electrolyte 20 in step (a) and step (b) is maintained at a working temperature between 50°C and 90°C by the water circulation temperature control device 3 (water chiller). More preferably, when the pH value of the electrolyte 20 is greater than 11, the predetermined voltage of step (b) is between 70V and 250V, and the electrolyte 20 applicable to the present invention is selected from sodium hydroxide (NaOH) solution, potassium hydroxide (KOH) solution, lithium hydroxide (LiOH) solution, cesium hydroxide (CsOH) solution, or rubidium hydroxide (RbOH); when the pH value of the electrolyte 20 is less than 5, the predetermined voltage of step (b) is between 160V and 400V, and the electrolyte 20 applicable to the present invention is selected from citric acid (C 6 H 8 O 7 ) solution, acetic acid (CH 3 COOH) solution, sulfuric acid (H 2 SO 4 ) solution, or carbonic acid (H 2 CO 3 ) solution.

[0035] The step (c) is to perform a solid-liquid separation on the electrolyte 20 after the step (b) is implemented, so as to separate the solid copper metal or the solid copper oxide from the electrolyte 20. Preferably, the solid-liquid separation in the step (c) is selected from centrifugation, sedimentation separation, vacuum concentration, or membrane filtration. The membrane filtration method suitable for this embodiment of the present invention can be selected from microfiltration membrane (MF membrane), ultrafiltration membrane (UF membrane) or nanofiltration membrane (NF membrane). In step (c) of this embodiment of the present invention, centrifugation is used.

[0036] The method for separating valuable metal elements from copper-containing metals of the present invention provides the following four specific examples based on the above embodiments, and the separation method and experimental results are described in detail as follows.

[0037] <Concrete example 1 (E1)>

[0038] In step (a) of a specific example 1 (E1) of the method for separating valuable metal elements from copper-containing metal of the present invention, a brass containing impurity elements is used as the cathode 24, a titanium mesh is used as the anode 23, and a 1M citric acid solution with a pH value of 3 is used as the electrolyte 20. When implementing step (b) of the specific example 1 (E1), the operating temperature of the electrolyte 20 is controlled to be 60° C. by the circulation temperature control device 3 (water chiller), and a predetermined voltage of 350V is provided to the anode 23 and the cathode 24 by the power supply 22, so that a gas film is formed around the brass during the electrolytic reaction between the brass and the citric acid solution, and the predetermined voltage of 350V breaks through the gas film to generate a plasma in the citric acid solution (i.e., a solution plasma reaction), thereby precipitating solid copper metal and impurity elements dissolved in the citric acid solution in an ionic state in the citric acid solution. Finally, a centrifuge (not shown) is used to perform solid-liquid separation on the citric acid solution containing the precipitated solid copper metal and the dissolved ionic impurities, thereby separating the solid copper metal and the ionic impurities from the citric acid solution.

[0039] The solid copper metal and ionic impurities obtained after solid-liquid separation in the specific example 1 (E1) of the present invention were analyzed by inductively coupled plasma mass spectrometry (ICP-MS), showing that the recovery purity of the solid copper metal reached 99.995wt% (summarized as shown in the following Table 1), and the ionic impurity elements were zinc (Zn), iron (Fe), and lead (Pb).

[0040] <Concrete example 2 (E2)>

[0041] A specific example 2 (E2) of the method of separating valuable metal elements from copper-containing metal of the present invention is substantially the same as the specific example 1 (E1), except that in step (a) of the specific example 2 (E2), pure copper containing impurity elements is used as the cathode 24.

[0042] The solid copper metal and ionic impurities obtained after solid-liquid separation in the specific example 2 (E2) of the present invention were analyzed by ICP-MS method, showing that the recovery purity of the solid copper metal reached 99.993wt% (summarized as shown in the following Table 1), and the ionic impurity elements were zinc (Zn), iron (Fe), and nickel (Ni).

[0043] <Concrete example 3 (E3)>

[0044] A specific example 3 (E3) of the method for separating valuable metal elements from copper-containing metals of the present invention is substantially the same as the specific example 1 (E1), except that in step (a) of the specific example 3, a 1M NaOH solution with a pH value of 14 is used as the electrolyte 20, and the predetermined voltage when implementing step (b) is 200 V. Specifically, in the specific example 3 (E3) of the present invention, when implementing step (b), a gas film is formed around the brass during the electrolytic reaction between the brass and the NaOH solution, and the predetermined voltage of 200 V breaks through the gas film to generate a solution plasma reaction in the NaOH solution, thereby precipitating solid copper oxide (CuO) and impurity elements dissolved in the NaOH solution in an ionic state in the NaOH solution.

[0045] The solid copper oxide and ionic impurities obtained after the solid-liquid separation of the specific example 3 (E3) of the present invention were analyzed by ICP-MS method, and the recovery purity of the solid copper oxide was 99.992wt% (summarized as shown in the following Table 1).

[0046] <Concrete example 4 (E4)>

[0047] A specific example 4 (E4) of the method for separating valuable metal elements from copper-containing metal of the present invention is substantially the same as the specific example 3 (E3), except that in step (a) of the specific example 4 (E4), pure copper containing impurity elements is used as the cathode 24.

[0048] The solid copper oxide and ionic impurities obtained after solid-liquid separation in the specific example 4 (E4) of the present invention were analyzed by ICP-MS method, and the recovery purity of the solid copper oxide reached 99.998wt% (summarized as shown in the following Table 1).

[0049] Table 1.

[0050]

[0051] @ The valuable metal element of E3 and E4 refers to copper in CuO.

[0052] The applicant further compares the present embodiment of the present invention with the existing copper separation and recovery methods recorded in the background art (i.e., the combination of hydrometallurgy and electrolytic refining, and the combination of pyrometallurgy and electrolytic refining) in terms of the three indicators of process steps, chemical cost and energy consumption. The aforementioned comparison is obtained by the applicant based on the published technical literature such as Surface and Coatings Technology 169-170 (2003) 91-95, Resources, Conservation & Recycling 146 (2019) 35-44, Resources, Conservation & Recycling 167 (2021) 105382, and Copper Recycling in Chapter 7 of Handbook of Recycling (i.e., taken from the webpage http: / / dx.doi.org / 10.1016 / B978-0-12-396459-5.00007-6), which is hereby stated in advance.

[0053] In terms of the process steps, although the embodiment of the present invention records the step (a), step (b) and step (c), in fact, the solution plasma reaction generated when implementing the step (b) can achieve the purpose of precipitating solid copper or solid copper oxide, and the process is quite simplified. In contrast, the existing copper separation and recovery method requires hydrometallurgy to go through the three steps of leaching, primary purification and secondary purification in sequence, while pyrometallurgy requires smelting, converting and fire refining in sequence, and then combined with an electrolytic refining step. Therefore, the process steps of the existing copper separation and recovery method are cumbersome.

[0054] In terms of the cost of chemical reagents, the embodiment of the present invention only needs to use one of the two solutions, acidic (e.g., 19.2g of citric acid) and alkaline (e.g., 8g of NaOH), which is low in cost. In contrast, the existing copper separation and recovery method requires 25g of ammonia (NH 3 ) and 36 g of ammonium chloride (NH 4 Cl), and 10.5 g of hydroxyapatite (CaCl) is required for one purification. 5 (PO 4 ) 3), and its secondary purification requires the use of 6.8g of magnesium chloride (MgCl 2 ), and the final electrolytic refining also requires the use of 20ml of sulfuric acid (H 2 SO 4 ), 20g of copper sulfate (CuSO 4 ) and additives. Therefore, the cost of the drug used in the existing copper separation and recovery method is higher than that in this embodiment of the present case.

[0055] Further studying the energy consumption, the energy consumption required for the existing copper separation and recovery method in hydrometallurgy combined with electrolytic refining is about 4300 J / g. Although the energy consumption of the solution plasma reaction of this embodiment of the present invention is slightly higher than that of hydrometallurgy combined with electrolytic refining (about 4500 J / g). However, in terms of the energy consumption required for pyrometallurgy combined with electrolytic refining, the smelting energy consumption is about 9000 J / g, the conversion energy consumption is about 1500 J / g, the pyrometallurgy energy consumption is about 1200 J / g, and the subsequent electrolytic refining energy consumption is about 4300 J / g, the total energy consumption is as high as 16000 J / g. Therefore, the energy consumption of pyrometallurgy combined with electrolytic refining is much higher than that of this embodiment of the present case.

[0056] Finally, no matter hydrometallurgy or pyrometallurgy combined with electrolytic refining, the purity of copper that can be separated and recovered is 99.99wt%. However, the embodiment of the present invention only needs to use a simplified solution plasma reaction, and the purity of the precipitated copper or copper oxide is greater than 99.99wt%.

[0057] In summary, the method of separating valuable metal elements from copper-containing metals of the present invention can obtain solid copper metal or solid copper oxide with a purity greater than 99.99wt% under the premise of simplifying the process steps (only the solution plasma reaction of step (b) is required), low chemical cost and much lower energy consumption than pyrometallurgy combined with electrolytic refining, so the purpose of the present invention can be achieved.

[0058] The above is only an embodiment of the present invention and should not be used to limit the scope of the present invention. All simple equivalent changes and modifications made according to the claims and description of the present invention are still within the scope of the present invention.

Claims

1. A method for separating valuable metal elements from copper-containing metals, characterized in that: The following steps are involved: Step (a) is to immerse the anode and the copper-containing metal as the cathode in an electrolyte, wherein the pH value of the electrolyte is either acidic or alkaline; and Step (b) is to provide a predetermined voltage to the anode and the cathode to form a gas film around the cathode during the electrolytic reaction between the cathode and the electrolyte, and the predetermined voltage is sufficient to break through the gas film around the cathode to generate plasma in the electrolyte to precipitate solid copper metal or solid copper oxide, and impurity elements dissolved in the electrolyte and in ionic state; Wherein, when the pH value of the electrolyte is acidic, the step (b) is to precipitate the solid copper metal; and Wherein, when the pH value of the electrolyte is alkaline, the step (b) is to precipitate the solid copper oxide.

2. The method for separating valuable metal elements from copper-containing metal according to claim 1, characterized in that: The method further comprises a step (c) after the step (b), wherein the step (c) is to perform solid-liquid separation on the electrolyte after the step (b) is performed, so as to separate the solid copper metal or the solid copper oxide from the electrolyte.

3. The method for separating valuable metal elements from copper-containing metal according to claim 2, characterized in that: The solid-liquid separation in step (c) is selected from centrifugation, sedimentation separation, vacuum concentration, or membrane filtration.

4. The method for separating valuable metal elements from copper-containing metal according to claim 1, characterized in that: The copper-containing metal is selected from brass containing impurity elements or pure copper containing impurity elements.

5. The method for separating valuable metal elements from copper-containing metal according to claim 4, characterized in that: The impurity elements include zinc, iron, lead, and nickel.

6. The method for separating valuable metal elements from copper-containing metal according to claim 1, characterized in that: In the step (a), the pH value of the electrolyte is greater than 11 or less than 5.

7. The method for separating valuable metal elements from copper-containing metal according to claim 6, characterized in that: When the pH value of the electrolyte is greater than 11, the predetermined voltage of step (b) is between 70V and 250V.

8. The method for separating valuable metal elements from copper-containing metal according to claim 7, characterized in that: The electrolyte is selected from sodium hydroxide solution, potassium hydroxide solution, lithium hydroxide solution, cesium hydroxide solution, or rubidium hydroxide solution.

9. The method for separating valuable metal elements from copper-containing metal according to claim 6, characterized in that: When the pH value of the electrolyte is less than 5, the predetermined voltage of step (b) is between 160V and 400V.

10. The method for separating valuable metal elements from copper-containing metal according to claim 9, characterized in that: The electrolyte is selected from citric acid solution, acetic acid solution, sulfuric acid solution, or carbonic acid solution.

11. The method for separating valuable metal elements from copper-containing metal according to claim 1, characterized in that: The electrolyte in step (a) and step (b) has a working temperature between 50°C and 90°C.

12. The method for separating valuable metal elements from copper-containing metal according to claim 11, characterized in that: The electrolyte in step (a) and step (b) is contained in a reaction tank, which includes a double-layer wall, and the double-layer wall defines a peripheral space for circulation of cooling water. The peripheral space is connected to a water circulation temperature control device so that the cooling water can circulate back and forth between the water circulation temperature control device and the peripheral space, and the water circulation temperature control device can control the temperature of the cooling water.