Aluminum fluoride adding method for aluminum electrolysis production
By using the data relationship between aluminum fluoride addition amount - bath temperature - molecular ratio and the change in sodium oxide content in aluminum electrolysis production to adjust the aluminum fluoride addition amount, the problem of inaccurate aluminum fluoride addition amount was solved and the electrolyte molecular ratio was achieved. Accurate adjustment and electrolytic cell stability improvement.
Patent Information
- Application Number
- CN202410739937.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-01
AI Technical Summary
The planned addition amount of aluminum fluoride in existing aluminum electrolysis production is not accurately grasped, resulting in large deviations in the electrolyte molecular ratio adjustment results, affecting the stability and current efficiency of the electrolytic cell.
Use the data relationship of aluminum fluoride addition amount - bath temperature - molecular ratio to determine the addition amount. Calculate and adjust the required aluminum fluoride addition amount through a formula, and adjust it according to changes in sodium oxide content. Temporarily halve or stop adding to maintain the electrolytic cell. stability.
The electrolyte molecular ratio is accurately adjusted to the target range, the stability and current efficiency of the electrolytic cell are improved, and the temperature fluctuation of the electrolytic cell and the difficulty in carbon residue separation are reduced.
Smart Images

Figure FT_1 
Figure FT_2 
Figure QLYQS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of production methods in the aluminum electrolysis industry, and specifically to a method for adding aluminum fluoride in aluminum electrolysis production. Background Art
[0002] As aluminum electrolysis develops today, energy conservation and high efficiency are inevitable. Therefore, how to save energy and produce efficiently has become a research topic in the industry. Aluminum fluoride is a commonly used additive in aluminum electrolysis production. In the cryolite-alumina molten salt electrolysis production process, aluminum fluoride is added to supplement the chemical reaction and volatilization loss of fluorine in the electrolyte, maintain and adjust the electrolyte molecular ratio within the target control range, and achieve the purpose of improving electrolyte properties, controlling electrolyte temperature, and improving current efficiency. Reasonably controlling the amount of aluminum fluoride added and maintaining and adjusting the electrolyte molecular ratio to the target range are the key points of electrolytic aluminum production process control.
[0003] If aluminum fluoride is not added sufficiently, a high molecular ratio will cause a loss of current efficiency and poor electrolyte-carbon-slag separation; if aluminum fluoride is added excessively, the molecular ratio will be too low, which will have many adverse effects on the normal production of electrolysis.
[0004] 1. The molecular ratio is too low, the electrolyte conductivity is low, and the cathode and anode distances of the electrolytic cell are compressed, causing voltage fluctuations and current efficiency loss in the electrolytic cell; 2. The molecular ratio is too low, the electrolyte crystallization temperature is seriously reduced, the superheat between the electrolyte temperature and the electrolyte crystallization temperature is widened, the electrolytic cell enters the low-temperature overheating process, the electrolytic cell furnace side melts, the electrolyte rise is difficult to control, the electrolytic cell stability deteriorates, and the current efficiency decreases; 3. If the molecular ratio is too low, the solubility of alumina in the electrolyte will deteriorate, which will also cause the electrolyte conductivity to deteriorate. At the same time, a large amount of bottom furnace precipitation will be produced, affecting the stability of electrolytic cell operation.
[0005] At present, most aluminum electrolytic enterprises still use computer-controlled fixed-dose addition for aluminum fluoride addition. The daily planned aluminum fluoride addition amount is added to the electrolytic cell through an aluminum fluoride feed container at an average addition time interval. Electrolytic process technicians adjust the planned aluminum fluoride addition amount based on the molecular ratio changes reflected in regular electrolyte analysis reports. In reality, there is a large deviation in the molecular ratio adjustment result due to inaccurate control of the planned aluminum fluoride addition amount. Summary of the invention
[0006] The purpose of the present invention is to provide a method for adding aluminum fluoride in aluminum electrolysis production, which is used to solve the problem that the molecular ratio adjustment result has a large deviation due to inaccurate grasp of the planned addition amount of aluminum fluoride.
[0007] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a method for adding aluminum fluoride in aluminum electrolysis production, wherein when adding aluminum fluoride, the data relationship of aluminum fluoride addition amount-bath temperature-molecular ratio in Table 1 of the specification is used to determine the addition amount.
[0008] Furthermore, the data relationship in Table 1 is obtained by the following steps to obtain the amount of aluminum fluoride added: (1) Calculate using formula (a): ; (a) Wherein, Q is the amount of aluminum fluoride added required for adjustment, P is the mass of cryolite in the electrolyte, K1 is the molecular ratio before adjustment, and K2 is the molecular ratio after adjustment; (2) On the basis of step (1), the amount of aluminum fluoride added was adjusted according to the change of the sodium oxide content in the aluminum oxide. The adjustment basis was: 1 kg of sodium oxide required 0.903 kg of aluminum fluoride to react with it for neutralization. Finally, Table 1 was obtained.
[0009] Furthermore, when adding aluminum fluoride: when there is a problem with the stability of the electrolytic cell, it is necessary to temporarily halve or stop adding aluminum fluoride.
[0010] Compared with the prior art, the present invention has the following beneficial effects: The present invention has the following beneficial effects: This patent provides a method for adding aluminum fluoride to aluminum electrolytic production. It is based on the basic theory and production practice of aluminum electrolysis. According to the changes in the relevant technical conditions of the electrolytic cell and the changes in the electrolyte molecular ratio, it determines the reasonable planned addition amount of aluminum fluoride to the electrolytic cell, and can accurately adjust the electrolyte molecular ratio to within the target range. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 It is the molecular ratio-fitting line diagram of the present invention; Figure 2 It is the electrolyte temperature-fitting line diagram of the present invention. DETAILED DESCRIPTION
[0012] The present invention provides a technical solution: See also Figure 1-2 , a method for adding aluminum fluoride in aluminum electrolysis production, when adding aluminum fluoride, the addition amount is determined by using the data relationship of aluminum fluoride addition amount-bath temperature-molecular ratio in the following Table 1.
[0013] Table 1 The data relationship in Table 1 uses the following steps to obtain the amount of aluminum fluoride added: (1) Calculate using formula (a): ; (a) Wherein, Q is the amount of aluminum fluoride added required for adjustment, P is the mass of cryolite in the electrolyte, K1 is the molecular ratio before adjustment, and K2 is the molecular ratio after adjustment.
[0014] (2) On the basis of step (1), the amount of aluminum fluoride added is adjusted according to the change in the sodium oxide content in the aluminum oxide. The adjustment basis is: calculated by the following formula, 1 kg of sodium oxide requires 0.903 kg of aluminum fluoride to react with it to neutralize it, and finally Table 1 is obtained.
[0015] Track the changes in the sodium oxide content in alumina in real time, and calculate the increase or decrease in aluminum fluoride under the condition of adjusting this factor.
[0016] When adding aluminum fluoride: the molecular ratio will affect the conductivity of the electrolyte, which in turn affects the distance between the cathode and anode of the electrolytic cell, and affects the stability of the electrolytic cell; when there is a problem with the stability of the electrolytic cell, it is necessary to temporarily halve or stop adding aluminum fluoride.
[0017] Production practice has proved that when adding aluminum fluoride in increments, if the molecular ratio change does not respond, the amount of aluminum fluoride added should be adjusted to the basic amount in time, and the tank conditions should be analyzed before further adjustment of the amount of addition. Generally, it is caused by the reduction of aluminum production in the tank. At this time, the aluminum production should be adjusted first, and then aluminum fluoride should be added in increments.
[0018] The molecular ratio and electrolyte temperature fitting line diagram was obtained through production practice, as shown in the attached manual. Figure 1 As shown; The molecular ratio and electrolyte temperature fitting line diagram was obtained through production practice, as shown in the attached manual. Figure 2 As shown; Taking the practical data in the above figure as an example, the performance of electrolyte temperature and molecular ratio under different conditions of aluminum fluoride addition is derived, and the amount of aluminum fluoride addition can be determined according to the performance of different bath temperatures.
[0019] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for adding aluminum fluoride in aluminum electrolysis production, characterized in that: When adding aluminum fluoride, the amount of addition is determined using the data relationship of aluminum fluoride addition amount - bath temperature - molecular ratio in Table 1 of the instruction manual.
2. The method for adding aluminum fluoride to aluminum electrolysis production according to claim 1, characterized in that: The data relationship in Table 1 is obtained by the following steps to obtain the amount of aluminum fluoride added: (1) Calculate using formula (a): ; (a) Wherein, Q is the amount of aluminum fluoride added required for adjustment, P is the mass of cryolite in the electrolyte, K1 is the molecular ratio before adjustment, and K2 is the molecular ratio after adjustment; (2) On the basis of step (1), the amount of aluminum fluoride added was adjusted according to the change of the sodium oxide content in the aluminum oxide. The adjustment basis was: 1 kg of sodium oxide required 0.903 kg of aluminum fluoride to react with it for neutralization. Finally, Table 1 was obtained.
3. The method for adding aluminum fluoride in aluminum electrolysis production according to claim 1, characterized in that: When adding aluminum fluoride: When there is a problem with the stability of the electrolytic cell, it is necessary to temporarily halve or stop adding aluminum fluoride.