Process for improving color fastness of polyester fabric
Through the combination of plasma treatment and acid dyes, the problems of insufficient dye binding force and high-temperature sublimation in the dyeing of polyester fabrics are solved, and the color fastness and soaping resistance of polyester fabrics are improved, especially the storage color transfer effect of dark-colored fabrics. .
Patent Information
- Application Number
- CN202410946981.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing polyester fabric dyeing technology, the binding force between the dye and the fabric is weak, and it is easy to sublimate the dye under high temperature conditions, resulting in relatively poor color fastness, especially the soaping fastness and storage migration of dark-colored fabrics. Poor color performance.
Plasma treatment technology is used to use NH3 gas to etch polyester fibers, increase their specific surface area, and generate polar groups -NH2 on the fibers, which combine with acid dyes to enhance the binding force between dyes and fabrics and avoid dye sublimation caused by high temperatures. The process includes fabric joining, desizing, plasma treatment, dyeing, washing and drying, shaping and finishing, and final inspection.
It significantly improves the color depth and color fastness of polyester fabrics, especially the soaping fastness and storage color transfer performance of dark-colored fabrics, avoids dye sublimation problems caused by high-temperature setting, and has energy-saving effects.
Smart Images

Figure CN118727474A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fabric dyeing and finishing, in particular to a process for improving the color fastness of polyester fabrics. Background Art
[0002] As the largest chemical fiber, polyester fiber has been widely used in all aspects of life. At present, disperse dyes are usually used for polyester dyeing. The dyes are combined with fabrics by Van der Vaar force and adsorbed on the surface of the fabric. This method leads to a weaker binding force between polyester and dyes. In addition, disperse dyes are prone to sublimation under high temperature conditions, which makes the color fastness of polyester relatively poor, especially the soap fastness and storage color transfer of dark polyester colors.
[0003] After polyester fabrics are dyed, they are usually shaped and finished to ensure the stability of their shrinkage or to give them certain functionality. The shaped finishing temperature is generally relatively high. Since disperse dyes are easy to sublimate under high temperature conditions, the shaped finishing process will cause part of the disperse dyes to sublimate to the surface of the fabric, thereby reducing the color depth, soap fastness and storage color transfer of the fabric, especially for dark-colored fabrics.
[0004] In view of this, the present invention is developed by deeply considering the many deficiencies and inconveniences caused by the imperfections in the existing polyester fabric dyeing and finishing processes, and actively researching, improving and trial-making to develop the present invention. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a process for improving the color fastness of polyester fabrics, which can improve the color depth and color fastness of polyester fabrics.
[0006] In order to achieve the above object, the solution of the present invention is:
[0007] A process for improving the color fastness of polyester fabrics, comprising the following steps:
[0008] Step S1, receiving fabrics, selecting polyester fabrics of 50D or above;
[0009] Step S2, desizing, removing surface impurities and slurry of the fabric selected in step S1;
[0010] Step S3, plasma treatment, using plasma equipment to micro-treat the surface of the fabric after desizing in step S2, using reactive gas NH3, and using NH3 plasma to treat the desizing fabric, thereby increasing the specific surface area of the polyester and generating polar groups -NH2 on the fabric;
[0011] Step S4, dyeing, using an acid dye to dye the plasma-treated fabric, the sulfonic acid group in the acid dye reacts with the polar group -NH2 to increase the interaction between the fabric and the dye;
[0012] Step S5, washing and drying, washing the dyed cloth to remove the residual pigment additives on the surface, and drying;
[0013] Step S6, shaping and finishing;
[0014] Step S7: Inspection.
[0015] Further, in step S3, the plasma equipment is selected as a normal pressure plasma jet equipment, the equipment power is 100W-120W, the frequency is 12MHz-15MHz, the flow rate is 1.0L / min-1.2L / min, the spacing is 2cm-2.5cm, and the time is 30s-40s.
[0016] Further, in step S4, the chemical formula of the polar group -NH2 and the sulfonic acid group is:
[0017] R-SO3 (-) +R'-NH2 (+) CCCRSO3 (-)(+) NH2R'.
[0018] Furthermore, in step S4, the formula of the dye is: 100 g / l of acid dye, 0.5%-1% of leveling agent, 1 g / l-1.5 g / l of dispersant, and 2 g / l-3 g / l of bath softener.
[0019] Further, in step S6, the shaping formula is: water repellent / absorption agent 40g / l-60g / l, bridging agent 0.5g / l, shaping temperature 160°C-170°C, speed 40m / min, overfeed 3%.
[0020] After adopting the above structure, the process of improving the color fastness of polyester fabric of the present invention is mainly through plasma treatment of polyester fabric, and the reactive gas NH3 is selected as the gas for plasma treatment. The polyester fiber is treated with NH3 plasma, which can etch the polyester fiber, increase the specific surface area of polyester, increase the contact area of dye, and improve the color depth of fabric; and NH3 plasma will react with polyester and generate polar group -NH2 on polyester fiber, and this group can react with sulfonic acid group in acid dye, which can increase the interaction force between polyester fiber and dye and improve the adsorption capacity of dye. During dyeing, since acid dye can react with polar group -NH2, the binding force between dye and polyester can be improved, so the color fastness of polyester can be improved, and at the same time, the problems such as dye sublimation caused by high temperature setting in the future, reduced color depth, decreased fastness (especially soap washing fastness) can be avoided. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is the dyeing curve diagram of the present invention. DETAILED DESCRIPTION
[0022] In order to further explain the technical solution of the present invention, the present invention is described in detail below through specific embodiments.
[0023] The present invention discloses a process for improving the color fastness of polyester fabrics, which comprises the following steps:
[0024] Step S1, receiving the fabric, selecting polyester fabric with a density of 50D or above. If the fabric is too thin, it is easy to cause the strength of the fabric to be too low after plasma treatment and dyeing.
[0025] Step S2: desizing to remove surface impurities and slurry of the fabric selected in step S1.
[0026] Step S3, plasma treatment, using plasma equipment to micro-treat the surface of the fabric after desizing in step S2. The plasma equipment is selected as a normal pressure plasma jet equipment, the equipment power is 100W-120W, the frequency is 12MHz-15MHz, the gas is selected as a reactive gas NH3, the flow rate is 1.0L / min-1.2L / min, the spacing is 2cm-2.5cm, and the time is 30s-40s.
[0027] The main reason for selecting the reactive gas NH3 in the present invention is that treating polyester fiber with NH3 plasma can etch the polyester fiber, increase the specific surface area of polyester, increase the contact area of dye, and improve the color depth of the fabric; and NH3 plasma will react with polyester and generate a polar group -NH2 on the polyester fiber. This group can react with the sulfonic acid group in the acid dye, increase the interaction between the polyester fiber and the dye, and improve the adsorption capacity of the dye.
[0028] The chemical formula of the polar group -NH2 and the sulfonic acid group is:
[0029] R-SO3 (-) +R'-NH2 (+) →RSO3 (-)(+) NH2R'
[0030] Step S4, dyeing. Conventional polyester dyeing uses disperse dyes for dyeing. However, disperse dyes and polyester are attached to polyester fibers through the action of van der Waals forces, resulting in poor color fastness. Affected by high temperatures, the dyes are easily sublimated, and the disperse dyes cannot react with the -NH2 after the above-mentioned plasma treatment. Therefore, the present invention combines plasma treatment technology to break through the convention and uses acid dyes for dyeing. Since acid dyes can react with the polar group -NH2, the binding force between the dye and polyester can be improved, thereby improving the color fastness of the polyester. At the same time, the subsequent sublimation of the dye caused by high-temperature setting can be avoided, which reduces the color depth and the fastness (especially the fastness to soap washing). The dyeing formula is: acid dye 100g / l, leveling agent 0.5%-1%, dispersant 1g / l-1.5g / l, softener in the bath 2g / l-3g / l. The dyeing curve is as follows Figure 1 As shown, the maximum temperature is 115℃-125℃, constant temperature for 30 minutes, which can be adjusted according to the light and dark colors of the fabric, with high temperature for dark colors and low temperature for light colors. This maximum dyeing temperature is lower than the conventional polyester dyeing temperature of 130℃, so it also has an energy-saving effect.
[0031] Step S5, washing and drying, washing the dyed cloth to remove the residual pigment additives on the surface, and drying.
[0032] Step S6, shaping and finishing, giving the fabric functionality and ensuring the stability of the fabric shrinkage and the flatness of the fabric surface. The shaping formula is: water repellent / absorbent 40g / l-60g / l, bridging agent 0.5g / l, shaping conditions are: (160℃-170℃)*40m / min*3%*width (set according to actual needs).
[0033] Step S7: Finished product inspection: inspecting the fabric surface quality of the fabric.
[0034] Taking 50D polyester pongee, 300T, black polyester as an example, the fabric is dyed with conventional disperse dyes and dyed according to the process of the present invention, and a six-fiber test (the main fabric is black and the other fibers are white) is performed to test whether the main fabric and other fabrics are stained. The main physical properties of the finished product are shown in Table 1 under the same shaping and finishing conditions:
[0035] Table 1 is the test comparison results of using conventional disperse dyes and using the process of the present invention
[0036]
[0037]
[0038]
[0039] After testing, after dyeing polyester pongee using the process of steps S1 to S7 of the present invention, compared with the polyester pongee dyed with conventional disperse dyes, the color fastness to soaping, perspiration fastness (acid), perspiration fastness (alkali), water fastness and storage color transfer effect of the present invention are all better than the conventional dyeing effects.
[0040] The above embodiments do not limit the form and style of the present invention. Any appropriate changes or modifications made by ordinary technicians in the relevant technical field should be deemed to be within the patent scope of the present invention.
Claims
1. A process for improving the color fastness of polyester fabrics, characterized in that: The following steps are involved: Step S1, receiving fabrics, selecting polyester fabrics of 50D or above; Step S2, desizing, removing surface impurities and slurry of the fabric selected in step S1; Step S3, plasma treatment, using plasma equipment to micro-treat the surface of the fabric after desizing in step S2, using reactive gas NH3, and using NH3 plasma to treat the desizing fabric, thereby increasing the specific surface area of the polyester and generating polar groups -NH2 on the fabric; Step S4, dyeing, using an acid dye to dye the plasma-treated fabric, the sulfonic acid group in the acid dye reacts with the polar group -NH2 to increase the interaction between the fabric and the dye; Step S5, washing and drying, washing the dyed cloth to remove the residual pigment additives on the surface, and drying; Step S6, shaping and finishing; Step S7: Inspection.
2. A process for improving the color fastness of polyester fabrics as claimed in claim 1, characterized in that: In the step S3, the plasma equipment is a normal pressure plasma jet equipment with an equipment power of 100W-120W, a frequency of 12MHz-15MHz, a flow rate of 1.0L / min-1.2L / min, a spacing of 2cm-2.5cm, and a time of 30s-40s.
3. A process for improving the color fastness of polyester fabrics as claimed in claim 1, characterized in that: In step S4, the chemical formula of the polar group -NH2 and the sulfonic acid group is: <h2 style=";text-align:left;direction:ltr">R-SO3<h2 style=";text-align:left;direction:ltr"> (-) <h2 style=";text-align:left;direction:ltr"> +R'-NH2<h2 style=";text-align:left;direction:ltr"> (+) <h2 style=";text-align:left;direction:ltr"> →RSO3<h2 style=";text-align:left;direction:ltr"> (-)(+) <h2 style=";text-align:left;direction:ltr"> NH2R'。 4. A process for improving the color fastness of polyester fabrics as claimed in claim 1, characterized in that: In step S4, the formula of the dye is: 100 g / l of acid dye, 0.5%-1% of leveling agent, 1 g / l-1.5 g / l of dispersant, and 2 g / l-3 g / l of bath softener.